High temperature resistant carbon fiber cloth and preparation method thereof
High-temperature resistant carbon fiber cloth was prepared by modifying the spinning solution and surface treatment, which solved the problem of performance degradation of carbon fiber cloth at high temperature and achieved better high-temperature resistance and mechanical properties.
Patent Information
- Application Number
- CN202411029947.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing carbon fiber cloth is prone to oxidation and pyrolysis in high-temperature environments, which leads to a decline in its performance and poor high-temperature resistance and mechanical properties.
High-temperature resistant carbon fiber cloth was prepared by preparing fiber precursors through modified spinning solution, followed by pre-oxidation and carbonization treatment, and then by treatment with polyetherimide sizing agent and bismaleimide resin modification components.
It significantly improves the high temperature resistance and mechanical properties of carbon fiber cloth, and enhances its chemical stability and impact resistance in high temperature environments.
Smart Images

Figure 1L8RUYCA2FONVTY0SNBSCSZGA7Y1OJGGN9NCFBYF
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon fiber cloth, and in particular to a high temperature resistant carbon fiber cloth and a preparation method thereof. Background Art
[0002] With the rapid development of modern industrial technology, especially in the fields of aerospace, automobile manufacturing, power electronics, etc., the requirements for high temperature resistance of materials are increasing day by day. As a lightweight, high-strength composite material, carbon fiber cloth has great application potential in the field of high temperature resistant materials due to its unique physical and chemical properties. However, traditional carbon fiber cloth is prone to oxidation, pyrolysis and other reactions in high temperature environments, resulting in a decrease in its performance and limiting its scope of application.
[0003] At present, the research on high temperature resistant carbon fiber cloth at home and abroad mainly focuses on the modification, compounding and surface treatment of materials. Among them, the high temperature resistance of carbon fiber cloth can be improved to a certain extent by changing the composition of carbon fiber cloth, adding high temperature resistant additives, using high temperature anti-oxidation coating and other methods. However, the existing methods for improving the high temperature resistance of carbon fiber cloth have not yet reached the ideal optimal state in practical applications, which will cause the high temperature resistance to be not lasting. Therefore, how to prepare carbon fiber cloth with good high temperature resistance and mechanical properties by improving the preparation method of carbon fiber cloth has become a technical problem that needs to be solved urgently by technicians in this field. Summary of the invention
[0004] Technical issues solved
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a high temperature resistant carbon fiber cloth and a preparation method thereof, which can effectively solve the problem of poor high temperature resistance and mechanical properties of the carbon fiber cloth in the prior art.
[0006] Technical Solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A method for preparing a high temperature resistant carbon fiber cloth, the method comprising the following steps:
[0009] S1, modifying polyacrylonitrile with polypropylene glycol to prepare a modified spinning solution, then preparing fiber precursors from the spinning solution by dry-wet spinning method, and preparing carbon fibers after pre-oxidation and carbonization treatment of the fiber precursors;
[0010] Among them, the operation of the dry-wet spinning method is: the fiber precursor liquid is sprayed out from the spinneret and then enters the coagulation bath with a dimethyl sulfoxide content of 40% through the air layer. The coagulated filaments are guided by the guide hook at the bottom of the coagulation bath tank, and then led out of the coagulation bath by the guide roller. The coagulated primary fibers enter the preheating bath for washing and low-multiple stretching. The preheating bath temperature is 60°C, and then enter the boiling water bath for the second stretching. The stretched filaments are collected and dried at a low temperature of 25°C in a vacuum oven.
[0011] S2, weighing a calculated amount of polyetherimide particles and dissolving them in a calculated amount of chloroform, mixing them evenly at room temperature and then performing magnetic stirring to prepare a sizing agent with a polyetherimide content of 1 wt%, then dispersing the sizing agent and deionized water evenly in a weight ratio of 2:3, and the resultant is recorded as a sizing component;
[0012] S3, after sizing the carbon fiber with the above sizing components, weaving the sizing carbon fiber into carbon fiber cloth;
[0013] S4, using diphenylmethane bismaleimide, diallyl bisphenol A and 4,4'-diphenyl ether dipropargyl ether as raw materials to prepare a bismaleimide resin modified component;
[0014] S5. The bismaleimide resin modified component is evenly coated on the surface of the carbon fiber cloth, first placed in a fume hood to dry for 12 hours, and then placed in a vacuum oven at 65° C. to dry for 3-5 hours to obtain a high temperature resistant carbon fiber cloth.
[0015] Furthermore, in S1, the preparation method of the modified spinning solution is:
[0016] Weigh 2-3 parts by weight of polypropylene glycol and 75-80 parts by weight of dimethyl sulfoxide into a beaker, stir at a stirring speed of 300 r / min for 10 minutes, then pour into a flask containing 20-22 parts by weight of dry polyacrylonitrile, then place in a constant temperature water bath at 60°C to swell for 8 hours, finally place in a constant temperature water bath at 70°C to stir and disperse at a stirring speed of 200 r / min for 8 hours, and the modified spinning solution is obtained after standing and degassing.
[0017] Furthermore, in S1, the specific operation of the pre-oxidation treatment is: placing the fiber precursor in a pre-oxidation furnace, and keeping it at 200° C., 230° C. and 250° C. for 10 minutes in sequence.
[0018] Furthermore, in S1, the specific operation of the carbonization treatment is: placing the pre-oxidized fiber precursor in a low-temperature carbonization furnace, using nitrogen as a sealing gas and a carrier gas, and carbonizing it at a temperature of 600°C for 1-2 minutes, and then placing it in a high-temperature carbonization furnace, using nitrogen as a sealing gas and a carrier gas, and carbonizing it at a temperature of 1000°C for 1-2 minutes, wherein the oxygen content in the low-temperature carbonization furnace and the high-temperature carbonization furnace is 0-5ppm, and the pressure is 3-15Pa.
[0019] Furthermore, in S2, the uniform mixing operation method is to stir at a stirring speed of 300 r / min for 5 min, and the magnetic stirring operation method is to stir at a stirring speed of 200 r / min for 10 min.
[0020] Furthermore, in S3, the operation steps of the sizing treatment are: pouring the sizing component into the sizing tank, passing the carbon fiber through the sizing tank at a speed of 15 mm / s under the traction of the motor, then winding the carbon fiber on the glass frame through the rubber extrusion roller, and finally placing it in a vacuum drying oven at 110°C for curing for 1-2 hours.
[0021] Furthermore, in S4, the preparation steps of the bismaleimide resin modified component are:
[0022] Step 1, weigh 60g of diphenylmethane bismaleimide and 39g of diallyl bisphenol A into a flask, heat to 140°C under nitrogen protection and stir at a stirring speed of 200r / min for 20min, and the obtained mixture is recorded as a mixed component;
[0023] Step 2, add 10g of 4,4'-diphenyl ether dipropargyl ether to the mixed components, continue stirring at the original stirring speed for 10min, pour into the mold, place in a vacuum oven to remove air and bubbles, and then transfer to a curing oven for heating and curing, first cure at 140°C for 2h, then heat to 210°C for 2h, and finally heat to 250°C for 2h. The obtained product is recorded as bismaleimide resin;
[0024] Step 3: dissolving the bismaleimide resin in tetrahydrofuran to prepare a solution with a mass fraction of 35%, stirring the solution at a stirring speed of 200 r / min for 10 minutes, and obtaining the bismaleimide resin modified component.
[0025] A high temperature resistant carbon fiber cloth is prepared by a method for preparing the high temperature resistant carbon fiber cloth.
[0026] Beneficial Effects
[0027] The present invention provides a high temperature resistant carbon fiber cloth and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects:
[0028] The invention uses polypropylene glycol to modify polyacrylonitrile to prepare a modified spinning solution, and the prepared fiber precursor is subjected to pre-oxidation treatment and carbonization treatment to prepare carbon fiber. The addition of polypropylene glycol can regulate the density of the fiber and reduce the holes inside the fiber, thereby improving the mechanical properties of the carbon fiber. Moreover, the fiber surface after the pre-oxidation treatment and carbonization treatment is more uniform and dense, and the mechanical properties of the carbon fiber are further enhanced. Secondly, the polyacrylonitrile fiber itself has high heat resistance. After the addition of polypropylene glycol and pre-oxidation and carbonization treatment, the high temperature resistance of the carbon fiber can be further improved, so that it can withstand higher temperatures. Finally, the polyacrylonitrile fiber can resist acids, oxidants and general organic solvents, but has poor alkali resistance. Through the modification treatment of polypropylene glycol, the alkali resistance of the carbon fiber cloth can be improved to a certain extent, and its overall chemical stability can be improved.
[0029] The invention prepares a sizing component by mixing polyetherimide and chloroform, and then weaves the sizing component into a carbon fiber cloth after applying the sizing component on the surface of the carbon fiber, which can enhance the wettability of the carbon fiber and the resin matrix, and is helpful to improve the adsorption performance of the subsequent carbon fiber cloth to the bismaleimide resin modified component. The polyetherimide is a polymer with good thermal stability and compatibility with thermoplastic resins. When the polyetherimide is mixed with chloroform to prepare a sizing agent and applied on the surface of the carbon fiber, the heat resistance and wettability of the carbon fiber can be significantly improved, and the carbon fiber and the resin matrix can be closely combined, thereby improving the interface performance of the composite material. Secondly, the sizing treatment can not only enhance the interface performance of the carbon fiber and the resin matrix, but also improve the overall performance of the carbon fiber cloth, such as improving the wear resistance, tensile strength and heat resistance of the carbon fiber cloth.
[0030] The present invention coats the bismaleimide resin modified component on the carbon fiber cloth, which can improve the high temperature resistance of the carbon fiber cloth. The bismaleimide resin itself has the advantages of good high temperature resistance, radiation resistance, moisture and heat resistance and low water absorption. When the bismaleimide resin modified component is coated on the carbon fiber cloth, the high temperature resistance of the carbon fiber cloth can be significantly improved, and good mechanical properties and chemical stability can be maintained under high temperature environment, so as to adapt to various high temperature application occasions; secondly, when the modified BMI resin component is coated on the carbon fiber cloth, the toughness of the carbon fiber cloth can be significantly improved, so that the carbon fiber cloth has better impact resistance and fatigue resistance. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The present invention will be further described below in conjunction with the embodiments.
[0033] A method for preparing a high temperature resistant carbon fiber cloth according to the present embodiment comprises the following steps:
[0034] S1, modifying polyacrylonitrile with polypropylene glycol to prepare a modified spinning solution, then preparing fiber precursors from the spinning solution by dry-wet spinning method, and preparing carbon fibers after pre-oxidation and carbonization treatment of the fiber precursors;
[0035] Among them, the operation of the dry-wet spinning method is: the fiber precursor liquid is sprayed out from the spinneret and then enters the coagulation bath with a dimethyl sulfoxide content of 40% through the air layer. The coagulated filaments are guided by the guide hook at the bottom of the coagulation bath tank, and then led out of the coagulation bath by the guide roller. The coagulated primary fibers enter the preheating bath for washing and low-multiple stretching. The preheating bath temperature is 60°C, and then enter the boiling water bath for the second stretching. The stretched filaments are collected and dried at a low temperature of 25°C in a vacuum oven.
[0036] The preparation method of the modified spinning solution is as follows:
[0037] Weigh 2 parts by weight of polypropylene glycol and 75 parts by weight of dimethyl sulfoxide into a beaker, stir at a stirring speed of 300 r / min for 10 minutes, then pour into a flask containing 20 parts by weight of dry polyacrylonitrile, then place in a constant temperature water bath at 60°C to swell for 8 hours, finally place in a constant temperature water bath at 70°C to stir and disperse at a stirring speed of 200 r / min for 8 hours, and the modified spinning solution is obtained after standing and degassing.
[0038] The specific operation of pre-oxidation treatment is: placing the fiber precursor in a pre-oxidation furnace, and keeping it warm at 200°C, 230°C and 250°C for 10 minutes respectively; the specific operation of carbonization treatment is: placing the pre-oxidation fiber precursor in a low-temperature carbonization furnace, using nitrogen as a sealing gas and a carrier gas, and low-temperature carbonizing at 600°C for 1 minute, and then placing it in a high-temperature carbonization furnace, using nitrogen as a sealing gas and a carrier gas, and high-temperature carbonizing at 1000°C for 1 minute, wherein the oxygen content in the low-temperature carbonization furnace and the high-temperature carbonization furnace is 0ppm, and the pressure is 3Pa.
[0039] S2. Weigh a calculated amount of polyetherimide particles and dissolve them in a calculated amount of chloroform. Stir the mixture at a stirring speed of 300 r / min for 5 min and then at a stirring speed of 200 r / min for 10 min at room temperature to prepare a sizing agent with a polyetherimide content of 1 wt%. Then, the sizing agent and deionized water are evenly dispersed in a weight ratio of 2:3. The result is recorded as a sizing component.
[0040] S3. After sizing the carbon fiber with the above sizing components, the sized carbon fiber is woven into carbon fiber cloth; wherein, the sizing operation steps are: pouring the sizing components into a sizing tank, passing the carbon fiber through the sizing tank at a speed of 15 mm / s under the traction of a motor, then winding the carbon fiber on a glass frame through a rubber squeezing roller, and finally curing in a vacuum drying oven at 110°C for 1 hour.
[0041] S4, using diphenylmethane bismaleimide, diallyl bisphenol A and 4,4'-diphenyl ether dipropargyl ether as raw materials to prepare a bismaleimide resin modified component;
[0042] Wherein, the preparation steps of the bismaleimide resin modified component are:
[0043] Step 1, weigh 60g of diphenylmethane bismaleimide and 39g of diallyl bisphenol A into a flask, heat to 140°C under nitrogen protection and stir at a stirring speed of 200r / min for 20min, and the obtained mixture is recorded as a mixed component;
[0044] Step 2, add 10g of 4,4'-diphenyl ether dipropargyl ether to the mixed components, continue stirring at the original stirring speed for 10min, pour into the mold, place in a vacuum oven to remove air and bubbles, and then transfer to a curing oven for heating and curing, first cure at 140°C for 2h, then heat to 210°C for 2h, and finally heat to 250°C for 2h. The obtained product is recorded as bismaleimide resin;
[0045] Step 3: dissolving the bismaleimide resin in tetrahydrofuran to prepare a solution with a mass fraction of 35%, stirring the solution at a stirring speed of 200 r / min for 10 minutes, and obtaining the bismaleimide resin modified component.
[0046] S5. The bismaleimide resin modified component is evenly coated on the surface of the carbon fiber cloth, first placed in a fume hood to dry for 12 hours, and then placed in a vacuum oven at 65° C. to dry for 3 hours to obtain a high temperature resistant carbon fiber cloth.
[0047] A method for preparing a high temperature resistant carbon fiber cloth according to the present embodiment comprises the following steps:
[0048] S1, modifying polyacrylonitrile with polypropylene glycol to prepare a modified spinning solution, then preparing fiber precursors from the spinning solution by dry-wet spinning method, and preparing carbon fibers after pre-oxidation and carbonization treatment of the fiber precursors;
[0049] Among them, the operation of the dry-wet spinning method is: the fiber precursor liquid is sprayed out from the spinneret and then enters the coagulation bath with a dimethyl sulfoxide content of 40% through the air layer. The coagulated filaments are guided by the guide hook at the bottom of the coagulation bath tank, and then led out of the coagulation bath by the guide roller. The coagulated primary fibers enter the preheating bath for washing and low-multiple stretching. The preheating bath temperature is 60°C, and then enter the boiling water bath for the second stretching. The stretched filaments are collected and dried at a low temperature of 25°C in a vacuum oven.
[0050] The preparation method of the modified spinning solution is as follows:
[0051] Weigh 3 parts by weight of polypropylene glycol and 80 parts by weight of dimethyl sulfoxide into a beaker, stir at a stirring speed of 300 r / min for 10 minutes, then pour into a flask containing 22 parts by weight of dry polyacrylonitrile, then place in a constant temperature water bath at 60°C to swell for 8 hours, finally place in a constant temperature water bath at 70°C to stir and disperse at a stirring speed of 200 r / min for 8 hours, and the modified spinning solution is obtained after standing and degassing.
[0052] The specific operation of pre-oxidation treatment is: placing the fiber precursor in a pre-oxidation furnace, and keeping it warm at 200°C, 230°C and 250°C for 10 minutes respectively; the specific operation of carbonization treatment is: placing the pre-oxidation fiber precursor in a low-temperature carbonization furnace, using nitrogen as a sealing gas and a carrier gas, and low-temperature carbonizing at 600°C for 2 minutes, and then placing it in a high-temperature carbonization furnace, using nitrogen as a sealing gas and a carrier gas, and high-temperature carbonizing at 1000°C for 2 minutes, wherein the oxygen content in the low-temperature carbonization furnace and the high-temperature carbonization furnace is 5ppm, and the pressure is 15Pa.
[0053] S2. Weigh a calculated amount of polyetherimide particles and dissolve them in a calculated amount of chloroform. Stir the mixture at a stirring speed of 300 r / min for 5 min and then at a stirring speed of 200 r / min for 10 min at room temperature to prepare a sizing agent with a polyetherimide content of 1 wt%. Then, the sizing agent and deionized water are evenly dispersed in a weight ratio of 2:3. The result is recorded as a sizing component.
[0054] S3. After sizing the carbon fiber with the above sizing components, the sized carbon fiber is woven into carbon fiber cloth; wherein, the sizing operation steps are: pouring the sizing components into a sizing tank, passing the carbon fiber through the sizing tank at a speed of 15 mm / s under the traction of a motor, then winding the carbon fiber on a glass frame through a rubber squeezing roller, and finally curing in a vacuum drying oven at 110°C for 2 hours.
[0055] S4, using diphenylmethane bismaleimide, diallyl bisphenol A and 4,4'-diphenyl ether dipropargyl ether as raw materials to prepare a bismaleimide resin modified component;
[0056] Wherein, the preparation steps of the bismaleimide resin modified component are:
[0057] Step 1, weigh 60g of diphenylmethane bismaleimide and 39g of diallyl bisphenol A into a flask, heat to 140°C under nitrogen protection and stir at a stirring speed of 200r / min for 20min, and the obtained mixture is recorded as a mixed component;
[0058] Step 2, add 10g of 4,4'-diphenyl ether dipropargyl ether to the mixed components, continue stirring at the original stirring speed for 10min, pour into the mold, place in a vacuum oven to remove air and bubbles, and then transfer to a curing oven for heating and curing, first cure at 140°C for 2h, then heat to 210°C for 2h, and finally heat to 250°C for 2h. The obtained product is recorded as bismaleimide resin;
[0059] Step 3: dissolving the bismaleimide resin in tetrahydrofuran to prepare a solution with a mass fraction of 35%, stirring the solution at a stirring speed of 200 r / min for 10 minutes, and obtaining the bismaleimide resin modified component.
[0060] S5. The bismaleimide resin modified component is evenly coated on the surface of the carbon fiber cloth, first placed in a fume hood to dry for 12 hours, and then placed in a vacuum oven at 65° C. to dry for 5 hours to obtain a high temperature resistant carbon fiber cloth.
[0061] A method for preparing a high temperature resistant carbon fiber cloth according to the present embodiment comprises the following steps:
[0062] S1, modifying polyacrylonitrile with polypropylene glycol to prepare a modified spinning solution, then preparing fiber precursors from the spinning solution by dry-wet spinning method, and preparing carbon fibers after pre-oxidation and carbonization treatment of the fiber precursors;
[0063] Among them, the operation of the dry-wet spinning method is: the fiber precursor liquid is sprayed out from the spinneret and then enters the coagulation bath with a dimethyl sulfoxide content of 40% through the air layer. The coagulated filaments are guided by the guide hook at the bottom of the coagulation bath tank, and then led out of the coagulation bath by the guide roller. The coagulated primary fibers enter the preheating bath for washing and low-multiple stretching. The preheating bath temperature is 60°C, and then enter the boiling water bath for the second stretching. The stretched filaments are collected and dried at a low temperature of 25°C in a vacuum oven.
[0064] The preparation method of the modified spinning solution is as follows:
[0065] Weigh 3 parts by weight of polypropylene glycol and 78 parts by weight of dimethyl sulfoxide into a beaker, stir at a stirring speed of 300 r / min for 10 minutes, then pour into a flask containing 21 parts by weight of dry polyacrylonitrile, then place in a constant temperature water bath at 60°C to swell for 8 hours, finally place in a constant temperature water bath at 70°C to stir and disperse at a stirring speed of 200 r / min for 8 hours, and the modified spinning solution is obtained after standing and degassing.
[0066] The specific operation of the pre-oxidation treatment is: placing the fiber precursor in a pre-oxidation furnace, and keeping it warm at 200°C, 230°C and 250°C for 10 minutes respectively; the specific operation of the carbonization treatment is: placing the pre-oxidation fiber precursor in a low-temperature carbonization furnace, using nitrogen as a sealing gas and a carrier gas, and low-temperature carbonizing at 600°C for 2 minutes, and then placing it in a high-temperature carbonization furnace, using nitrogen as a sealing gas and a carrier gas, and high-temperature carbonizing at 1000°C for 2 minutes, wherein the oxygen content in the low-temperature carbonization furnace and the high-temperature carbonization furnace is 3ppm, and the pressure is 9Pa.
[0067] S2. Weigh a calculated amount of polyetherimide particles and dissolve them in a calculated amount of chloroform. Stir the mixture at a stirring speed of 300 r / min for 5 min and then at a stirring speed of 200 r / min for 10 min at room temperature to prepare a sizing agent with a polyetherimide content of 1 wt%. Then, the sizing agent and deionized water are evenly dispersed in a weight ratio of 2:3. The result is recorded as a sizing component.
[0068] S3. After sizing the carbon fiber with the above sizing components, the sized carbon fiber is woven into carbon fiber cloth; wherein, the sizing operation steps are: pouring the sizing components into a sizing tank, passing the carbon fiber through the sizing tank at a speed of 15 mm / s under the traction of a motor, then winding the carbon fiber on a glass frame through a rubber squeezing roller, and finally curing in a vacuum drying oven at 110°C for 2 hours.
[0069] S4, using diphenylmethane bismaleimide, diallyl bisphenol A and 4,4'-diphenyl ether dipropargyl ether as raw materials to prepare a bismaleimide resin modified component;
[0070] Wherein, the preparation steps of the bismaleimide resin modified component are:
[0071] Step 1, weigh 60g of diphenylmethane bismaleimide and 39g of diallyl bisphenol A into a flask, heat to 140°C under nitrogen protection and stir at a stirring speed of 200r / min for 20min, and the obtained mixture is recorded as a mixed component;
[0072] Step 2, add 10g of 4,4'-diphenyl ether dipropargyl ether to the mixed components, continue stirring at the original stirring speed for 10min, pour into the mold, place in a vacuum oven to remove air and bubbles, and then transfer to a curing oven for heating and curing, first cure at 140°C for 2h, then heat to 210°C for 2h, and finally heat to 250°C for 2h. The obtained product is recorded as bismaleimide resin;
[0073] Step 3: dissolving the bismaleimide resin in tetrahydrofuran to prepare a solution with a mass fraction of 35%, stirring the solution at a stirring speed of 200 r / min for 10 minutes, and obtaining the bismaleimide resin modified component.
[0074] S5. The bismaleimide resin modified component is evenly coated on the surface of the carbon fiber cloth, first placed in a fume hood to dry for 12 hours, and then placed in a vacuum oven at 65° C. to dry for 4 hours to obtain a high temperature resistant carbon fiber cloth.
[0075] Comparative Example 1
[0076] The high temperature resistant carbon fiber cloth and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that the polypropylene glycol in Example 1 is not added to the modified spinning solution in this comparative example 1.
[0077] Comparative Example 2
[0078] The high temperature resistant carbon fiber cloth and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that the sizing agent in Example 1 is replaced with a PSF sizing agent in this comparative example 2.
[0079] Comparative Example 3
[0080] The high temperature resistant carbon fiber cloth and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 3, the bismaleimide resin modified component in Example 1 is replaced with deionized water.
[0081] Performance Testing
[0082] Single fiber filaments were extracted from the high temperature resistant carbon fiber cloths in Examples 1-3 and Comparative Examples 1-3, and were marked as Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, and Comparative Example 3, respectively. The performance of Examples 1-3 and Comparative Examples 1-3 was then tested, and the specific testing method was as follows:
[0083] 1. The interface shear strength and tensile strength of Examples 1-3 and Comparative Examples 1-3 were tested, and the obtained data were recorded in the following table;
[0084] 2. Examples 1-3 and Comparative Examples 1-3 were placed in an environment of 280° C. and heated for 5 hours. After being taken out, their interface shear strength was tested. The obtained data are recorded in the following table;
[0085]
[0086] It can be seen from the data in the above table that the mechanical properties of the single fiber in the high temperature resistant carbon fiber cloth in Examples 1-3 are better than those in Comparative Example 1, indicating that the fiber prepared by modifying polyacrylonitrile with polypropylene glycol has better mechanical properties. The mechanical properties of Comparative Examples 2-3 after high temperature heating are significantly reduced, and the degree of reduction is greater than that of Examples 1-3, indicating that the sizing agent and bismaleimide resin modified components in the present invention can improve the high temperature resistance of the carbon fiber cloth. In summary, the high temperature resistant carbon fiber cloth prepared by the present invention has better mechanical properties and high temperature resistance, and has excellent market promotion value.
[0087] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0088] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a high temperature resistant carbon fiber cloth, characterized in that: The preparation method comprises the following steps: S1, modifying polyacrylonitrile with polypropylene glycol to prepare a modified spinning solution, then preparing fiber precursors from the spinning solution by dry-wet spinning method, and preparing carbon fibers after pre-oxidation and carbonization treatment of the fiber precursors; S2, weighing a calculated amount of polyetherimide particles and dissolving them in a calculated amount of chloroform, mixing them evenly at room temperature and then performing magnetic stirring to prepare a sizing agent with a polyetherimide content of 1 wt%, then dispersing the sizing agent and deionized water evenly in a weight ratio of 2:3, and the resultant is recorded as a sizing component; S3, after sizing the carbon fiber with the above sizing components, weaving the sizing carbon fiber into carbon fiber cloth; S4, using diphenylmethane bismaleimide, diallyl bisphenol A and 4,4'-diphenyl ether dipropargyl ether as raw materials to prepare a bismaleimide resin modified component; S5, uniformly coating the bismaleimide resin modified component on the surface of the carbon fiber cloth, and obtaining the high temperature resistant carbon fiber cloth after drying; In S1, the modified spinning solution is prepared by: Weigh 2-3 parts by weight of polypropylene glycol and 75-80 parts by weight of dimethyl sulfoxide into a beaker, stir at a stirring speed of 300 r / min for 10 minutes, then pour into a flask containing 20-22 parts by weight of dry polyacrylonitrile, then place in a constant temperature water bath at 60°C for swelling for 8 hours, finally place in a constant temperature water bath at 70°C for stirring and dispersion at a stirring speed of 200 r / min for 8 hours, and after standing and degassing, obtain the modified spinning solution; In S1, the specific operation of the pre-oxidation treatment is: placing the fiber precursor in a pre-oxidation furnace, and keeping it at 200°C, 230°C and 250°C for 10 minutes in sequence; In S1, the specific operation of the carbonization treatment is: placing the pre-oxidized fiber precursor in a low-temperature carbonization furnace, using nitrogen as a sealing gas and a carrier gas, and low-temperature carbonizing for 1-2 minutes at a temperature of 600° C., and then placing it in a high-temperature carbonization furnace, using nitrogen as a sealing gas and a carrier gas, and high-temperature carbonizing for 1-2 minutes at a temperature of 1000° C.; In the specific operation of carbonization treatment, the oxygen content in the low-temperature carbonization furnace and the high-temperature carbonization furnace is 0-5ppm and the pressure is 3-15Pa; In S4, the preparation steps of the bismaleimide resin modified component are: Step 1, weigh 60g of diphenylmethane bismaleimide and 39g of diallyl bisphenol A into a flask, heat to 140°C under nitrogen protection and stir at a stirring speed of 200r / min for 20min, and the obtained mixture is recorded as a mixed component; Step 2, add 10g of 4,4'-diphenyl ether dipropargyl ether to the mixed components, continue stirring at the original stirring speed for 10min, pour into the mold, place in a vacuum oven to remove air and bubbles, and then transfer to a curing oven for heating and curing, first cure at 140°C for 2h, then heat to 210°C for 2h, and finally heat to 250°C for 2h. The obtained product is recorded as bismaleimide resin; Step 3: dissolving the bismaleimide resin in tetrahydrofuran to prepare a solution with a mass fraction of 35%, stirring the solution at a stirring speed of 200 r / min for 10 minutes, and obtaining the bismaleimide resin modified component.
2. The method for preparing a high temperature resistant carbon fiber cloth according to claim 1, characterized in that: In S2, the uniform mixing operation method is to stir at a stirring speed of 300 r / min for 5 min, and the magnetic stirring operation method is to stir at a stirring speed of 200 r / min for 10 min.
3. The method for preparing a high temperature resistant carbon fiber cloth according to claim 1, characterized in that: In S3, the sizing treatment process is as follows: pour the sizing component into the sizing tank, and under the traction of the motor, the carbon fiber passes through the sizing tank at a speed of 15 mm / s, and then the carbon fiber is wound on the glass frame through the rubber extrusion roller, and finally placed in a vacuum drying oven at 110°C for curing for 1-2 hours.
4. The method for preparing a high temperature resistant carbon fiber cloth according to claim 1, characterized in that: In S5, the specific operation of the drying treatment is: first place it in a fume hood to dry for 12 hours, and then place it in a vacuum oven at 65°C to dry for 3-5 hours.
5. A high temperature resistant carbon fiber cloth, characterized in that: The high temperature resistant carbon fiber cloth is prepared by the preparation method of any one of claims 1 to 4.