A kind of graphene-doped conductive silver paste and preparation method thereof

By adding doped graphene to conductive silver paste and preparing silver/graphene composite materials, the problems of high preparation cost and reduced curing performance caused by high silver content in conductive silver paste are solved, and high conductivity and mechanical strength are improved.

CN118553462BActive Publication Date: 2024-10-01常州碳禾新材料科技有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411009424.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-01
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The high silver content in existing conductive silver pastes leads to high preparation costs, and the reduced binder content leads to reduced curing performance, making it difficult to meet the high conductivity requirements of electronic products.

Method used

Add doped graphene to the conductive silver paste, and prepare silver/graphene composite materials through silver composite technology. Optimize the binder composition and process flow, including ultrasonic mixing, temperature control and precipitation reaction, to form high conductivity and mechanical strength. of silver/graphene composites.

Benefits of technology

It effectively reduces the amount of silver powder added, reduces the preparation cost, increases the conductivity and mechanical strength, and improves the curing performance and mechanical properties of the conductive silver paste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of conductive silver paste, specifically to a conductive silver paste doped with graphene and a preparation method thereof, comprising the following processes: mixing epoxy resin, toughening agent, cellulose and diluent, stirring for 30 to 60 minutes; adding silver powder, graphene and adhesion promoter in batches, grinding for 30 to 60 minutes, and ultrasonically dispersing for 24 hours; adding curing agent, accelerator, anti-settling agent and leveling defoaming agent, mixing, grinding for 30 to 60 minutes, and obtaining conductive silver paste. The present invention reduces the amount of silver powder added by adding graphene to the conductive silver paste, and can effectively reduce the cost of the prepared conductive silver paste. And by sulfonating the graphene and compounding it with silver, a silver / graphene composite material is prepared, which further improves the conductivity and mechanical strength of the silver paste after curing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conductive silver paste, and in particular to a graphene-doped conductive silver paste and a preparation method thereof. Background Art

[0002] Conductive silver paste is a material that is formed by mixing conductive powder with a binder and curing to form a conductor. It is widely used in the fields of electronic circuits, electronic component electrodes, lead terminals, circuit contacts, etc. The conductive powder in the conductive silver paste is metallic silver particles, which gives it the characteristics of high conductivity, stable performance, and good printability. With the advancement of science and technology, in order to meet the high conductivity requirements of electronic products, the silver content in the conductive silver paste is usually 60-90%, which makes the conductive silver paste have a higher preparation cost. At the same time, the reduction of the binder content will also lead to a decrease in curing performance. Therefore, we propose a graphene-doped conductive silver paste and a preparation method thereof. Summary of the invention

[0003] The object of the present invention is to provide a graphene-doped conductive silver paste and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a graphene-doped conductive silver paste, comprising the following mass components: 60 to 68 parts of silver powder, 12 to 20 parts of graphene, 10 to 20 parts of a binder and 9.0 to 16.4 parts of an auxiliary agent.

[0005] Furthermore, the binder includes thermoplastic resin and cellulose.

[0006] Furthermore, the thermoplastic resin is one or more of epoxy resin, acrylic resin, and polyurethane.

[0007] Furthermore, the cellulose is a mixture of one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, carboxymethyl cellulose, cellulose acetate butyrate, ethyl cellulose, and ethyl hydroxyethyl cellulose.

[0008] Furthermore, the binder includes 8 to 12 parts of epoxy resin, 0 to 12 parts of cellulose, 1.6 to 2.4 parts of curing agent and 0.06 to 0.12 parts of accelerator.

[0009] Furthermore, the curing agent is one of an amine curing agent and an acid anhydride curing agent.

[0010] Furthermore, the silver powder includes 20-30 wt % of nano silver particles and 70-80 wt % of micron silver flakes.

[0011] Furthermore, the auxiliary agent includes 5 to 10 parts of diluent, 2.5 to 3.5 parts of toughening agent, 0.4 to 0.6 parts of adhesion promoter, 0.5 to 0.8 parts of anti-settling agent and 0.5 to 1.5 parts of leveling defoaming agent.

[0012] Furthermore, the graphene is compounded with silver to form a silver / graphene composite material.

[0013] Furthermore, the silver / graphene composite material is prepared by the following process:

[0014] Add polyvinyl pyrrolidone to the graphene dispersion and mix ultrasonically for 30 to 120 minutes; add 50% to 55% of the component weight of silver nitrate, adjust the system pH to 6.0±0.2, and mix ultrasonically for 8 to 12 hours; place at 95 to 100° C., stir and slowly add 55% to 60% of the component weight of hydrazine hydrate, add within 30 minutes, and react for 2 to 4 hours;

[0015] Slowly add the remaining components of silver nitrate and sodium chloride, raise the temperature to 160-195°C, and stir to react for 2-4 hours; slowly add the remaining component of hydrazine hydrate, and continue to react for 4-7 hours;

[0016] The mixture was cooled, centrifuged at a speed of 7500-8000 r / min for 15-20 min, the precipitate was washed with anhydrous ethanol and deionized water, and vacuum dried at a temperature of 30-60° C. for 12-24 h to obtain a silver / graphene composite material.

[0017] Further, the mass ratio of graphene oxide and silver nitrate is 1:(1-4);

[0018] The mass ratio of silver nitrate, polyvinyl pyrrolidone, hydrazine hydrate and sodium chloride is 10: (25-30): (6.0-6.4): (0.12-0.15);

[0019] The concentration of graphene dispersion is 50 mg / 100 mL;

[0020] Silver nitrate was added in the form of an aqueous solution at a concentration of 5 wt%;

[0021] Hydrazine hydrate was added in the form of an aqueous solution with a concentration of 30 wt%.

[0022] Furthermore, the graphene dispersion is prepared by the following process:

[0023] Mix graphene oxide and deionized water, perform ultrasonic dispersion for 30 to 60 minutes, add sodium borohydride, and perform pre-reduction at 80 to 85° C. for 45 to 60 minutes; cool, centrifuge, wash, and dry to obtain reduced graphene oxide;

[0024] The reduced graphene oxide was dispersed in deionized water by ultrasonic for 30 to 60 minutes, hydrochloric acid was added and mixed, sulfanilic acid and sodium nitrite were added in sequence, and the mixture was stirred at 0 to 5°C for 100 to 150 minutes; the mixture was filtered, washed, and dried at 60°C to obtain sulfonated graphene;

[0025] Deionized water was added and ultrasonic dispersion was performed for 30 to 60 minutes to obtain a graphene dispersion.

[0026] Furthermore, the ratio of graphene oxide, sodium borohydride, and deionized water is 100 mg / (110-130) mg / 100 mL.

[0027] Further, the ratio of reduced graphene oxide, deionized water, and hydrochloric acid (0.05 M) was 100 mg / 100 mL / 50 mL;

[0028] The mass ratio of reduced graphene oxide, sulfanilic acid and sodium nitrite is 10:(13.0-41.7):(7-20).

[0029] In the above technical solution, silver powder is the basic material of conductive silver paste. Adding graphene with high electron migration effect to conductive silver paste helps to improve its conductivity. Moreover, the excellent mechanical properties and stability of graphene also help to build the conductive network made of silver paste and improve its mechanical properties. Graphene oxide is a single atomic layer with a higher electron transition speed, which helps silver paste to obtain better conductive properties.

[0030] In the above technical scheme, sodium borohydride can reduce graphene oxide, remove most of the oxygen-containing functional groups in graphene oxide, and restore its conjugated structure to a certain extent, which can significantly improve the conductivity of the prepared reduced graphene oxide, and help to further improve the conductivity of silver paste. Sulfanilic acid has an aromatic amine structure, and a diazotization reaction will occur in a sodium nitrite solution to generate an aryl diazonium salt. The aryl diazonium salt is easily decomposed in a high temperature environment, so the reaction is maintained in a low temperature environment, so that the graphene is functionalized by the aryl diazonium salt, and the sulfonate group is modified on the graphene surface, so that it has a higher hydrophilicity and a better dispersibility in water. We will record the obtained functionalized graphene as sulfonated graphene, mix it with deionized water, and form a graphene dispersion.

[0031] In the above technical scheme, polyvinyl pyrrolidone is added to the graphene dispersion, and graphene is adsorbed on the molecular chain of polyvinyl pyrrolidone through the dipole effect between the sulfonic acid group and the lactam group. The water molecule can promote the extension of the polyvinyl pyrrolidone molecular chain to form a chain structure (necklace-like). Then, part of silver nitrate is added, and the sulfonate groups on the surface of sulfonated graphene are coordinated with silver ions through electrostatic action, so that the silver ions are precipitated and produce a π electron conjugation effect with the benzene ring in the sulfonate group. Sufficient mixing time is conducive to the formation of silver sulfonate, forming silver ion-modified sulfonated graphene, and destroying the structure between polyvinyl pyrrolidone and graphene. Adding the reducing agent hydrazine hydrate, the silver ions in the silver nitrate are reduced to generate silver atoms, and the electron cloud of the silver and the benzene ring (sulfonate group) on the surface of the graphene produces a π-π electron conjugation effect, which helps to improve the conductivity of the graphene; the sulfonate group is released and recombines with the polyvinyl pyrrolidone molecule. Silver atoms interact with N and O atoms in polyvinyl pyrrolidone, adsorbing silver and stabilizing the microstructure of silver-sulfonated graphene. Silver ions, reducing agent and sodium chloride are added again, and the silver atoms generated above are used as cores for silver growth. The chloride ions are combined with silver ions to generate silver chloride colloid, and the concentration of free silver ions is controlled by precipitation-dissolution equilibrium, and silver growth is carried out with the silver atoms generated above as cores. Under the influence of the selective adsorption of polyvinyl pyrrolidone on the silver crystal surface, the subsequently generated silver is deposited on the {111} surface, and the linear growth of nanosilver is achieved, thereby forming a graphene composite material with silver nanocolumns grown on the surface, which is recorded as a silver / graphene composite material, which can effectively separate adjacent graphene sheets and prevent them from agglomerating in the conductive silver paste; improve the interface performance between the graphene surface and the silver powder, and between the silver powder and the silver powder, reduce the interface resistance between the silver, improve the conductivity efficiency, and improve its mechanical properties.

[0032] In the above technical solution, the silver / graphene composite material is mixed with nano silver particles and micro silver flakes.

[0033] The micron silver sheets are stacked layer by layer, and the structure is not tight enough. A conductive short circuit has been formed after the conductive silver paste is cured. The addition of nanosilver particles and silver / graphene composite materials helps the silver particles, silver columns and silver sheets to connect with each other, forming a dense conductive network, reducing the volume resistance of the conductive silver paste cured product, and improving its mechanical properties and conductive properties.

[0034] A method for preparing a graphene-doped conductive silver paste comprises the following processes:

[0035] Mix epoxy resin, toughening agent, cellulose and diluent, and stir for 30 to 60 minutes;

[0036] Add silver powder, graphene and adhesion promoter in batches, grind for 30-60 min, and ultrasonically disperse for 24 h;

[0037] Add curing agent, accelerator, anti-settling agent and leveling defoamer, mix and grind for 30 to 60 minutes to obtain conductive silver paste.

[0038] Furthermore, the grinding speed is 500 r / min.

[0039] In the above technical scheme, the conductive silver paste uses epoxy resin as the binder curing system. The addition of cellulose in the binder helps to improve the thixotropy of the conductive silver paste, promote the transfer of the conductive silver paste during printing and the film formation after printing, limit the flow of the conductive silver paste, inhibit its curing shrinkage, and improve the comprehensive performance of the conductive silver paste cured product.

[0040] The invention discloses an application of graphene-doped conductive silver paste, which is used for preparing conductive circuits. After printing and coating, the conductive silver paste is placed at 60 to 100° C. and cured for 30 to 120 minutes.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] The present invention discloses a graphene-doped conductive silver paste, which can effectively reduce the cost of the conductive silver paste by adding graphene to the conductive silver paste to reduce the amount of silver powder added. The silver / graphene composite material is prepared by sulfonating the graphene and compounding it with silver, which further improves the conductivity and mechanical strength of the cured silver paste. DETAILED DESCRIPTION

[0043] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] In the following specific implementations,

[0045] Graphene oxide: XFQ024, from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.;

[0046] Nanosilver particles: Flow Metal, from Bando Chemical Co., Ltd., Japan;

[0047] Micron silver flakes: PSP-840, from Kunming Norman Electronic Materials Co., Ltd.;

[0048] Epoxy resin: liquid bisphenol A epoxy resin E51 (618), sourced from Jinhong Glue Industry;

[0049] The curing agent is amine curing agent JH-5515 B glue, which comes from Jinhong Glue Industry;

[0050] The diluent is anhydrous ethanol; the adhesion promoter is silane coupling agent KH-560;

[0051] Toughening agent: liquid nitrile rubber LNBR810, from Hengshui Jiansheng Rubber & Plastic Technology Co., Ltd.;

[0052] Anti-settling agent BYK-410 and leveling defoamer BYK-354 are both from BYK in Germany;

[0053] Polyvinylpyrrolidone (PVP): K30, from Tianjin Damao Chemical Reagent Factory;

[0054] Cellulose: Hydroxyethyl cellulose, sourced from Tianjin Zhiyuan Chemical Reagent Co., Ltd.

[0055] Embodiment 1: A method for preparing a graphene-doped conductive silver paste, comprising the following process:

[0056] Step 1:

[0057] 1.1. Mix graphene oxide and deionized water, disperse them by ultrasonication for 30 minutes, add sodium borohydride, and pre-reduce them at 80°C for 45 minutes; cool, centrifuge, wash, and dry to obtain reduced graphene oxide; the ratio of graphene oxide, sodium borohydride, and deionized water is 100 mg / 110 mg / 100 mL;

[0058] The reduced graphene oxide was ultrasonically dispersed in deionized water for 30 minutes, hydrochloric acid was added and mixed, sulfanilic acid and sodium nitrite were added in sequence, and the mixture was stirred and mixed for 100 minutes at 5°C; the mixture was filtered, washed, and dried at 60°C to obtain sulfonated graphene; the ratio of reduced graphene oxide, deionized water, and hydrochloric acid (0.05M) was 100 mg / 100 mL / 50 mL; the mass ratio of reduced graphene oxide, sulfanilic acid, and sodium nitrite was 10:13.0:7;

[0059] Deionized water was added and ultrasonic dispersion was performed for 30 minutes to obtain a graphene dispersion liquid; the concentration of the graphene dispersion liquid was 50 mg / 100 mL;

[0060] 1.2. Add polyvinyl pyrrolidone to the graphene dispersion and mix ultrasonically for 30 minutes; add 50% of the component weight of silver nitrate, adjust the system pH to 6.0, and mix ultrasonically for 8 hours; place at 95°C, stir and slowly add 55% of the component weight of hydrazine hydrate, add within 30 minutes, and react for 4 hours;

[0061] Slowly add the remaining components of silver nitrate and sodium chloride, raise the temperature to 160°C, and stir to react for 4 hours; slowly add the remaining component of hydrazine hydrate, and continue to react for 4 hours;

[0062] Cooling, centrifuging at a speed of 7500r / min for 20min, washing the precipitate with anhydrous ethanol and deionized water, and vacuum drying at 30°C for 24h to obtain a silver / graphene composite material; the mass ratio of sulfonated graphene and silver nitrate is 1:1; the mass ratio of silver nitrate, polyvinyl pyrrolidone, hydrazine hydrate, and sodium chloride is 10:25:6.0:0.12; silver nitrate is added in the form of an aqueous solution with a concentration of 5wt%; hydrazine hydrate is added in the form of an aqueous solution with a concentration of 30wt%;

[0063] Step 2: Mix epoxy resin, toughening agent, cellulose and diluent, and stir for 30 minutes; add silver powder, silver / graphene composite material and adhesion promoter in batches, grind for 30 minutes, and ultrasonically disperse for 24 hours; add curing agent, accelerator, anti-settling agent and leveling defoamer, mix, grind for 30 minutes, and the grinding speed is 500r / min to obtain conductive silver paste, which includes the following mass components: 68 parts of silver powder, 12 parts of silver / graphene composite material, 10 parts of epoxy resin, 3 parts of cellulose, 2 parts of curing agent, 0.1 parts of accelerator, 10 parts of diluent, 3 parts of toughening agent, 0.5 parts of adhesion promoter, 0.5 parts of anti-settling agent and 1 part of leveling defoamer; the silver powder includes 20wt% nano silver particles and 80wt% micron silver flakes.

[0064] Embodiment 2: A method for preparing a graphene-doped conductive silver paste, comprising the following process:

[0065] Step 1:

[0066] 1.1. Mix graphene oxide and deionized water, disperse them by ultrasonication for 45 minutes, add sodium borohydride, and pre-reduce them at 82°C for 50 minutes; cool, centrifuge, wash, and dry to obtain reduced graphene oxide; the ratio of graphene oxide, sodium borohydride, and deionized water is 100 mg / 120 mg / 100 mL;

[0067] The reduced graphene oxide was ultrasonically dispersed in deionized water for 45 minutes, hydrochloric acid was added and mixed, sulfanilic acid and sodium nitrite were added in sequence, and the mixture was stirred and mixed for 120 minutes at 2°C; the mixture was filtered, washed, and dried at 60°C to obtain sulfonated graphene; the ratio of reduced graphene oxide, deionized water, and hydrochloric acid (0.05M) was 100 mg / 100 mL / 50 mL; the mass ratio of reduced graphene oxide, sulfanilic acid, and sodium nitrite was 10:27.0:13.5;

[0068] Deionized water was added and ultrasonic dispersion was performed for 45 minutes to obtain a graphene dispersion liquid; the concentration of the graphene dispersion liquid was 50 mg / 100 mL;

[0069] 1.2. Add polyvinyl pyrrolidone to the graphene dispersion and mix it ultrasonically for 75 minutes; add 52% of the component weight of silver nitrate, adjust the system pH to 6.0, and mix it ultrasonically for 10 hours; place it at 98°C, stir and slowly add 58% of the component weight of hydrazine hydrate, add it within 30 minutes, and react for 3 hours;

[0070] Slowly add the remaining components of silver nitrate and sodium chloride, raise the temperature to 175°C, and stir to react for 3 hours; slowly add the remaining component of hydrazine hydrate, and continue to react for 6 hours;

[0071] Cooling, centrifuging at a speed of 7800r / min for 18min, washing the precipitate with anhydrous ethanol and deionized water, and vacuum drying at 45°C for 18h to obtain a silver / graphene composite material; the mass ratio of sulfonated graphene and silver nitrate is 1:2.5; the mass ratio of silver nitrate, polyvinyl pyrrolidone, hydrazine hydrate, and sodium chloride is 10:27.5:6.2:0.13; silver nitrate is added in the form of an aqueous solution at a concentration of 5wt%; hydrazine hydrate is added in the form of an aqueous solution at a concentration of 30wt%;

[0072] Step 2: Mix epoxy resin, toughening agent, cellulose and diluent, and stir for 45 minutes; add silver powder, silver / graphene composite material and adhesion promoter in batches, grind for 45 minutes, and ultrasonically disperse for 24 hours; add curing agent, accelerator, anti-settling agent and leveling defoamer, mix, grind for 45 minutes, and the grinding speed is 500r / min to obtain conductive silver paste, which includes the following mass components: 64 parts of silver powder, 16 parts of silver / graphene composite material, 10 parts of epoxy resin, 3 parts of cellulose, 2 parts of curing agent, 0.1 parts of accelerator, 10 parts of diluent, 3 parts of toughening agent, 0.5 parts of adhesion promoter, 0.5 parts of anti-settling agent and 1 part of leveling defoamer; the silver powder includes 25wt% nano silver particles and 75wt% micron silver flakes.

[0073] Embodiment 3: A method for preparing a graphene-doped conductive silver paste, comprising the following process:

[0074] Step 1:

[0075] 1.1. Mix graphene oxide and deionized water, disperse them by ultrasonication for 60 minutes, add sodium borohydride, and pre-reduce them at 85°C for 45 minutes; cool, centrifuge, wash, and dry to obtain reduced graphene oxide; the ratio of graphene oxide, sodium borohydride, and deionized water is 100 mg / 130 mg / 100 mL;

[0076] The reduced graphene oxide was ultrasonically dispersed in deionized water for 60 minutes, hydrochloric acid was added and mixed, sulfanilic acid and sodium nitrite were added in sequence, and the mixture was stirred and mixed for 150 minutes at 0°C; the mixture was filtered, washed, and dried at 60°C to obtain sulfonated graphene; the ratio of reduced graphene oxide, deionized water, and hydrochloric acid (0.05M) was 100 mg / 100 mL / 50 mL; the mass ratio of reduced graphene oxide, sulfanilic acid, and sodium nitrite was 10:41.7:20;

[0077] Deionized water was added and ultrasonic dispersion was performed for 60 minutes to obtain a graphene dispersion liquid; the concentration of the graphene dispersion liquid was 50 mg / 100 mL;

[0078] 1.2. Add polyvinyl pyrrolidone to the graphene dispersion and mix ultrasonically for 120 minutes; add 55% of the component weight of silver nitrate, adjust the system pH to 6.0, and mix ultrasonically for 12 hours; place at 100°C, stir and slowly add 60% of the component weight of hydrazine hydrate, add within 30 minutes, and react for 1 hour;

[0079] Slowly add the remaining components of silver nitrate and sodium chloride, raise the temperature to 195°C, and stir to react for 2 hours; slowly add the remaining component of hydrazine hydrate, and continue to react for 7 hours;

[0080] The mixture was cooled and centrifuged at a speed of 8000 r / min for 15 min. The precipitate was washed with anhydrous ethanol and deionized water and dried under vacuum at 60° C. for 12 h to obtain a silver / graphene composite material. The mass ratio of sulfonated graphene to silver nitrate was 1:4. The mass ratio of silver nitrate, polyvinyl pyrrolidone, hydrazine hydrate and sodium chloride was 10:30:6.4:0.15. Silver nitrate was added in the form of an aqueous solution at a concentration of 5 wt %; hydrazine hydrate was added in the form of an aqueous solution at a concentration of 30 wt %;

[0081] Step 2: Mix epoxy resin, toughening agent, cellulose and diluent, and stir for 60 minutes; add silver powder, silver / graphene composite material and adhesion promoter in batches, grind for 60 minutes, and ultrasonically disperse for 24 hours; add curing agent, accelerator, anti-settling agent and leveling defoamer, mix, grind for 60 minutes, and the grinding speed is 500r / min to obtain conductive silver paste, which includes the following mass components: 60 parts of silver powder, 20 parts of silver / graphene composite material, 10 parts of epoxy resin, 3 parts of cellulose, 2 parts of curing agent, 0.1 parts of accelerator, 10 parts of diluent, 3 parts of toughening agent, 0.5 parts of adhesion promoter, 0.5 parts of anti-settling agent and 1 part of leveling defoamer; the silver powder includes 30wt% nano silver particles and 70wt% micron silver flakes.

[0082] Comparative Example 1: A method for preparing a graphene-doped conductive silver paste, comprising the following process:

[0083] Step 1:

[0084] 1.1. Disperse graphene oxide in deionized water by ultrasonic for 30 min, add hydrochloric acid and mix, add sulfanilic acid and sodium nitrite in turn, stir and mix at 5°C for 100 min; filter, wash, and dry at 60°C to obtain sulfonated graphene; the ratio of graphene oxide, deionized water, and hydrochloric acid (0.05M) is 100 mg / 100 mL / 50 mL; the mass ratio of graphene oxide, sulfanilic acid, and sodium nitrite is 10:13.0:7;

[0085] Deionized water was added and ultrasonic dispersion was performed for 30 minutes to obtain a graphene dispersion liquid; the concentration of the graphene dispersion liquid was 50 mg / 100 mL;

[0086] 1.2. Add polyvinyl pyrrolidone to the graphene dispersion and mix ultrasonically for 30 minutes; add 50% of the component weight of silver nitrate, adjust the system pH to 6.0, and mix ultrasonically for 8 hours; place at 95°C, stir and slowly add 55% of the component weight of hydrazine hydrate, add within 30 minutes, and react for 4 hours;

[0087] Slowly add the remaining components of silver nitrate and sodium chloride, raise the temperature to 160°C, and stir to react for 4 hours; slowly add the remaining component of hydrazine hydrate, and continue to react for 4 hours;

[0088] Cooling, centrifuging at a speed of 7500r / min for 20min, washing the precipitate with anhydrous ethanol and deionized water, and vacuum drying at 30°C for 24h to obtain a silver / graphene composite material; the mass ratio of sulfonated graphene and silver nitrate is 1:1; the mass ratio of silver nitrate, polyvinyl pyrrolidone, hydrazine hydrate, and sodium chloride is 10:25:6.0:0.12; silver nitrate is added in the form of an aqueous solution with a concentration of 5wt%; hydrazine hydrate is added in the form of an aqueous solution with a concentration of 30wt%;

[0089] Step 2 is the same as in Example 1, to obtain a conductive silver paste.

[0090] Comparative Example 2: A method for preparing a graphene-doped conductive silver paste, comprising the following processes:

[0091] Step 1: Mix graphene oxide and deionized water, and disperse them by ultrasonic for 30 minutes to obtain a graphene dispersion; the concentration of the graphene dispersion is 50 mg / 100 mL;

[0092] Add polyvinyl pyrrolidone to the graphene dispersion and mix ultrasonically for 30 minutes; add 50% of the component weight of silver nitrate, adjust the system pH to 6.0, and mix ultrasonically for 8 hours; place at 95°C, stir and slowly add 55% of the component weight of hydrazine hydrate, add it within 30 minutes, and react for 4 hours;

[0093] Slowly add the remaining components of silver nitrate and sodium chloride, raise the temperature to 160°C, and stir to react for 4 hours; slowly add the remaining component of hydrazine hydrate, and continue to react for 4 hours;

[0094] Cooling, centrifuging at a speed of 7500r / min for 20min, washing the precipitate with anhydrous ethanol and deionized water, and vacuum drying at 30°C for 24h to obtain a silver / graphene composite material; the mass ratio of graphene oxide and silver nitrate is 1:1; the mass ratio of silver nitrate, polyvinyl pyrrolidone, hydrazine hydrate, and sodium chloride is 10:25:6.0:0.12; silver nitrate is added in the form of an aqueous solution with a concentration of 5wt%; hydrazine hydrate is added in the form of an aqueous solution with a concentration of 30wt%;

[0095] Step 2 is the same as in Example 1, to obtain a conductive silver paste.

[0096] Comparative Example 3: A method for preparing a graphene-doped conductive silver paste, comprising the following processes:

[0097] Step 1: Mix graphene oxide and deionized water, and disperse them by ultrasonic for 30 minutes to obtain a graphene dispersion; the concentration of the graphene dispersion is 50 mg / 100 mL;

[0098] Add dodecylbenzenesulfonic acid and polyvinyl pyrrolidone to the graphene dispersion, and mix them ultrasonically for 30 minutes; add silver nitrate, adjust the pH of the system to 6.0, and mix them ultrasonically for 8 hours; stir and add hydrazine hydrate, raise the temperature to 160°C, and stir and react for 8 hours;

[0099] Cooling, centrifuging at a speed of 7500r / min for 20min, washing the precipitate with anhydrous ethanol and deionized water, and vacuum drying at 30°C for 24h to obtain a silver / graphene composite material; the mass ratio of graphene oxide and silver nitrate is 1:1; the mass ratio of silver nitrate, sodium dodecylbenzene sulfonate, polyvinyl pyrrolidone, hydrazine hydrate, and sodium chloride is 10:1:25:6.0:0.12; silver nitrate is added in the form of an aqueous solution at a concentration of 5wt%; hydrazine hydrate is added in the form of an aqueous solution at a concentration of 30wt%;

[0100] Step 2 is the same as in Example 1, to obtain a conductive silver paste.

[0101] Comparative Example 4: A method for preparing a graphene-doped conductive silver paste, comprising the following processes:

[0102] The epoxy resin, toughening agent, cellulose and diluent are mixed and stirred for 30 minutes; silver powder, graphene oxide and adhesion promoter are added in batches, ground for 30 minutes, and ultrasonically dispersed for 24 hours; curing agent, promoter, anti-settling agent and leveling defoaming agent are added and mixed, and ground for 30 minutes at a grinding speed of 500r / min to obtain a conductive silver paste, which includes the following mass components: 68 parts of silver powder, 12 parts of graphene oxide, 10 parts of epoxy resin, 3 parts of cellulose, 2 parts of curing agent, 0.1 parts of promoter, 10 parts of diluent, 3 parts of toughening agent, 0.5 parts of adhesion promoter, 0.5 parts of anti-settling agent and 1 part of leveling defoaming agent; the silver powder includes 20wt% of nano silver particles and 80wt% of micron silver flakes.

[0103] Experiment: The conductive silver paste obtained in Examples 1-3 and Comparative Examples 1-4 was printed and coated, and then placed at 100° C. for curing for 30 minutes to obtain samples. The properties of the samples were tested and the test results were recorded:

[0104] Conductive performance test: The mesh number of the printed screen is 100 mesh, the substrate is PET film, and the size of the cured sample is 2mm×2mm; the conductivity test is carried out using a four-probe tester, and the square resistance of the sample is used as the experimental indicator;

[0105] Mechanical properties test: A universal tensile testing machine is used to detect the maximum breaking force of the sample and obtain the shear strength of the sample.

[0106]

[0107] According to the data in the above table, we can clearly draw the following conclusions:

[0108] The conductive silver paste obtained in Examples 1-3 is compared with the conductive silver paste obtained in Comparative Examples 1-4. The test results show that:

[0109] Compared with the comparative example, the printed and cured samples of the conductive silver paste obtained in Examples 1-3 have lower resistivity and higher shear strength data, which fully demonstrates that the present invention achieves improvement in the conductive properties and mechanical strength of the conductive silver paste.

[0110] Compared with Example 1, the sulfonated graphene in Comparative Example 1 was not pre-reduced, and more defects existed in the graphene of the silver / graphene composite material, thereby reducing the conductivity of the sample.

[0111] The graphene dispersion in Comparative Example 2 is a graphene oxide dispersion, and the prepared silver / graphene composite material is graphene oxide deposited with nanosilver particles, which does not produce a π electron conjugation effect, and the interface performance between silver atoms and graphene is relatively poor, resulting in a decrease in the conductivity and mechanical properties of the sample.

[0112] The graphene dispersion in Comparative Example 3 is a graphene oxide dispersion, and sodium dodecylbenzene sulfonate is added to the preparation components of the silver / graphene composite material, which is mutually exclusive with graphene. There is an interaction between sodium dodecylbenzene sulfonate and polyvinyl pyrrolidone molecules, and the sodium dodecylbenzene sulfonate complexed silver competes with the reduction of silver ions, thereby forming a composite material of silver nanoparticles and graphene oxide. Most of the silver nanoparticles are not loaded on the surface of the graphene, further affecting the conductivity and mechanical properties of the sample.

[0113] In Comparative Example 4, the silver / graphene composite material in the conductive silver paste is replaced with graphene oxide. The conductive fillers such as silver powder and graphene oxide in the conductive silver paste agglomerate, which destroys the conductive path and makes the connection between the fillers fragile, resulting in a decrease in the mechanical strength and conductive properties of the sample.

[0114] It can be seen from the above that the preparation process of the conductive silver paste and the arrangement of the components used in the present invention can promote the comprehensive improvement of its conductive performance and mechanical strength.

[0115] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0116] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a graphene-doped conductive silver paste, Features: Including the following processes: Mix epoxy resin, toughening agent, cellulose and diluent, and stir for 30 to 60 minutes; Add silver powder, graphene and adhesion promoter in batches, grind for 30-60 min, and ultrasonically disperse for 24 h; Add curing agent, accelerator, anti-settling agent and leveling defoamer, mix and grind for 30 to 60 minutes to obtain conductive silver paste; The graphene is compounded with silver to form a silver / graphene composite material; The silver / graphene composite material is prepared by the following process: Add polyvinyl pyrrolidone to the graphene dispersion and mix ultrasonically for 30 to 120 minutes; add 50% to 55% of the component weight of silver nitrate, adjust the system pH to 6.0±0.2, and mix ultrasonically for 8 to 12 hours; place at 95 to 100° C., stir and slowly add 55% to 60% of the component weight of hydrazine hydrate, add within 30 minutes, and react for 2 to 4 hours; Slowly add the remaining components of silver nitrate and sodium chloride, raise the temperature to 160-195° C., and stir to react for 2-4 hours; slowly add the remaining component of hydrazine hydrate, and continue to react for 4-7 hours to obtain a silver / graphene composite material; The graphene dispersion is prepared by the following process: Mix graphene oxide and deionized water, perform ultrasonic dispersion for 30 to 60 minutes, add sodium borohydride, and perform pre-reduction at 80 to 85° C. for 45 to 60 minutes to obtain reduced graphene oxide; The reduced graphene oxide is dispersed in deionized water by ultrasonic for 30 to 60 minutes, hydrochloric acid is added and mixed, sulfanilic acid and sodium nitrite are added in sequence, and the mixture is stirred at 0 to 5° C. for 100 to 150 minutes to obtain sulfonated graphene; Deionized water was added and ultrasonic dispersion was performed for 30 to 60 minutes to obtain a graphene dispersion.

2. A method for preparing a graphene-doped conductive silver paste according to claim 1, Features: The conductive silver paste comprises the following components by mass: 60 to 68 parts of silver powder, 12 to 20 parts of graphene, 10 to 20 parts of a binder and 9.0 to 16.4 parts of an auxiliary agent; The binder comprises 8 to 12 parts of epoxy resin, 0 to 12 parts of cellulose, 1.6 to 2.4 parts of curing agent and 0.06 to 0.12 parts of accelerator.

3. The method for preparing a graphene-doped conductive silver paste according to claim 2, Features: The auxiliary agent comprises 5 to 10 parts of diluent, 2.5 to 3.5 parts of toughening agent, 0.4 to 0.6 parts of adhesion promoter, 0.5 to 0.8 parts of anti-settling agent and 0.5 to 1.5 parts of leveling defoaming agent.

4. The method for preparing a graphene-doped conductive silver paste according to claim 1, Features: The mass ratio of graphene oxide to silver nitrate is 1:(1-4); The mass ratio of silver nitrate, polyvinyl pyrrolidone, hydrazine hydrate and sodium chloride is 10: (25-30): (6.0-6.4): (0.12-0.15).

5. The method for preparing a graphene-doped conductive silver paste according to claim 1, Features: The mass ratio of graphene oxide to sodium borohydride is 1:(1.1-1.3).

6. The method for preparing a graphene-doped conductive silver paste according to claim 1, Features: The mass ratio of reduced graphene oxide, sulfanilic acid and sodium nitrite is 10:(13.0-41.7):(7-20).

7. A graphene-doped conductive silver paste prepared according to the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Self-assembly preparation method of gas-liquid interface of silver nanowire / graphene polymer composite film

    CN104927073A

  • Conductive silver paste doped with graphene / nano-silver composite powder and preparation method thereof

    CN117711671A

  • Titanium dioxide / sulfonated graphene oxide / ag nanoparticle composite membrane and preparation and application thereof

    US20190126211A1

  • Conducting nanocomposite matrix and uses thereof

    WO2014089708A1