Environmentally friendly aerated concrete block and preparation method thereof

By using modified titanium dioxide and silica-alumina porous microspheres in air-entrained concrete blocks, the density and uniformity of the pore structure of the blocks are improved, the problems of poor strength and weather resistance in the existing technology are solved, and air-entrained concrete blocks are realized. High strength and improved weather resistance of concrete blocks.

CN118561580BActive Publication Date: 2024-10-22HUNAN HEHENG ASSEMBLY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411046962.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-22
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing aerated concrete blocks have unreasonable raw material composition, resulting in uneven pore sizes and poor strength and weather resistance, which affects their application.

Method used

Using components such as modified titanium dioxide and silica-aluminum porous microspheres, through the preparation process of modified titanium dioxide and the preparation method of air-entrained concrete blocks, the density and uniformity of pore structure are improved, thereby improving strength and weather resistance.

Benefits of technology

Significantly improves the compressive strength and weather resistance of aerated concrete blocks, enhancing their early and long-term performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention belongs to the field of building materials, and in particular to a kind of environmentally friendly aerated concrete block and its preparation method. The environmentally friendly aerated concrete block comprises the following raw materials in parts by weight: 50-65 parts of cement, 30-40 parts of quicklime, 8-15 parts of gypsum, 6-12 parts of fly ash, 9-12 parts of modified titanium dioxide, 3-7 parts of silicon-aluminum porous microspheres, 2-4 parts of water reducers, 4-8 parts of foaming agents, and 100-120 parts of water. There is gelled material on the surface of modified titanium dioxide particles, so that the connection between particles is relatively tight, and there is good bonding stability during the preparation process of aerated concrete blocks, which is conducive to improving the compactness of aerated concrete blocks, and then improving the strength and weather resistance of aerated concrete blocks. Silicon-aluminum porous microspheres produce hydrogen through hydration reaction, and can form a more uniform pore structure during the preparation process of aerated concrete blocks, thereby improving the compressive strength and weather resistance of aerated concrete blocks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of building materials, and particularly relates to an environmentally friendly aerated concrete building block and a preparation method thereof. Background Art

[0002] At present, the demand for the development of green buildings, building materials and prefabricated buildings is becoming stronger and stronger. Green building materials with environmental protection as their mark have become the key object to promote the development of the construction industry. Aerated concrete has attracted much attention from the construction industry due to its light weight, strong thermal insulation performance, good fireproof effect and the ability to be processed into products of different sizes. It has become a new type of green building material that is rapidly promoted and developed in most countries and is widely used in masonry structures and frame structures of industrial and civil buildings.

[0003] Compared with traditional building materials such as sintered bricks, aerated concrete blocks can reduce the waste of resources and reduce environmental pollution, and can also accelerate the development of my country's construction industry. In addition, aerated concrete blocks have the advantages of strong plasticity, planing and sawing, and good processing characteristics. Due to the unreasonable composition and proportion of raw materials, the aerated concrete blocks prepared by the prior art have problems such as uneven pore size, poor strength and weather resistance, which affect their application. Based on this, it is necessary to further improve the performance of aerated concrete blocks. Summary of the invention

[0004] The first object of the present invention is to provide an environmentally friendly aerated concrete block having excellent strength and weather resistance.

[0005] The second object of the present invention is to provide a method for preparing an environmentally friendly aerated concrete block, which is simple and easy to operate.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] An environmentally friendly aerated concrete block comprises the following raw materials in parts by weight: 50-65 parts of cement, 30-40 parts of quicklime, 8-15 parts of gypsum, 6-12 parts of fly ash, 9-12 parts of modified titanium dioxide, 3-7 parts of silicon-aluminum porous microspheres, 2-4 parts of water reducing agent, 4-8 parts of foaming agent, and 100-120 parts of water;

[0008] The preparation process of the modified titanium dioxide is as follows:

[0009] (1) adding titanium dioxide and a silane coupling agent into an ethanol aqueous solution, stirring for reaction, and purifying to obtain silane coupling agent-modified titanium dioxide;

[0010] (2) adding sodium periodate solution to the guar gum solution and stirring evenly, and performing oxidation reaction in the dark. After the reaction is completed, the reaction solution is purified to obtain aldehyded guar gum;

[0011] (3) Add the silane coupling agent modified titanium dioxide of step (1) and the aldehyde-modified guar gum of step (2) into deionized water, heat and react under stirring conditions, and purify to obtain modified titanium dioxide.

[0012] Preferably, in step (3), the mass ratio of the formaldehyded guar gum to the silane coupling agent modified titanium dioxide is 1:4-8; the heating temperature is 60-70° C., and the heating time is 40-60 min.

[0013] Preferably, in step (1), the dosage ratio of titanium dioxide, silane coupling agent and ethanol aqueous solution is 1 g: 1-2 mL: 8-10 mL; and the concentration of the ethanol aqueous solution is 90%.

[0014] Preferably, the silane coupling agent is KH570 or KH580.

[0015] Preferably, the stirring reaction temperature in step (1) is 90-100° C., and the reaction time is 1.5-2.5 h.

[0016] Preferably, in step (2), the volume ratio of the sodium periodate solution to the guar gum solution is 1:10-12; the concentration of the guar gum solution is 0.02-0.03 g / mL, and the concentration of the sodium periodate solution is 0.040-0.050 g / mL; and the oxidation reaction time is 11-13 h.

[0017] Preferably, the water reducer is aminosulfonic acid high-efficiency water reducer; and the foaming agent is dichlorotetrafluoroethane.

[0018] The method for preparing the above-mentioned environmentally friendly aerated concrete blocks comprises the following steps:

[0019] a. Mix cement, quicklime, gypsum, fly ash, modified titanium dioxide, water reducer and water in proportion by weight, then add a foaming agent and silica-alumina porous microspheres and mix well to obtain a concrete block slurry;

[0020] b. Pour the concrete block slurry of step a into a mold, pre-curing to obtain a concrete block body, demolding and segmenting, and then steam curing to obtain.

[0021] Preferably, the pre-curing temperature in step b is 60-70° C., and the pre-curing time is 4-5 h.

[0022] Preferably, the steam curing in step b is carried out at a temperature of 160-180° C., a pressure of 1-2 MPa, and a time of 10-11 h.

[0023] Compared with the prior art, the beneficial effects of the present invention are mainly:

[0024] The environmentally friendly aerated concrete blocks of the present invention are added with modified titanium dioxide, silicon-aluminum porous microspheres and other ingredients. Among them, there is a gelled substance on the surface of the modified titanium dioxide particles, which makes the connection between the particles relatively tight, has good bonding stability during the preparation of the aerated concrete blocks, is conducive to improving the compactness of the aerated concrete blocks, and then improves the strength and weather resistance of the aerated concrete blocks. The silicon-aluminum porous microspheres produce hydrogen through hydration reaction, and can form a more uniform pore structure during the preparation of the aerated concrete blocks, thereby improving the compressive strength and weather resistance of the aerated concrete blocks. DETAILED DESCRIPTION

[0025] The technical scheme of the present invention is further described below in conjunction with specific embodiments. However, it should be understood by those skilled in the art that the following examples are only used to illustrate the present invention and should not be regarded as limiting the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, unless otherwise specified, are conventional products obtained through commercial channels.

[0026] 1. Preparation Example

[0027] Preparation Example 1

[0028] This preparation example provides a modified titanium dioxide, and the detailed preparation process is as follows:

[0029] (1) Add 15 g of titanium dioxide and 15 mL of KH570 into 135 mL of ethanol aqueous solution (the concentration of the ethanol aqueous solution is 90%), stir and react at 95°C for 2 h, and obtain silane coupling agent-modified titanium dioxide after centrifugation, washing, and drying.

[0030] (2) Dissolve 0.44 g of sodium periodate in 10 g of deionized water to obtain a sodium periodate aqueous solution, dissolve 2 g of guar gum in 100 g of deionized water to obtain a guar gum aqueous solution, add the sodium periodate aqueous solution dropwise to the guar gum aqueous solution and stir evenly, stir the mixed solution in a light-proof environment for 12 h to carry out an oxidation reaction, and after the reaction is completed, pour the reaction solution into a dialysis bag and dialyze for 8 h, and freeze-dry to obtain aldehyded guar gum.

[0031] (3) According to the mass ratio of formaldehyde-modified guar gum to silane coupling agent-modified titanium dioxide of 1:4, silane coupling agent-modified titanium dioxide and formaldehyde-modified guar gum are added into deionized water, and the mixture is heated at 65° C. with stirring for 50 min. After the heating, the mixture is filtered, washed, and vacuum dried to obtain modified titanium dioxide.

[0032] Preparation Example 2

[0033] This preparation example provides a modified titanium dioxide, and the detailed preparation process is as follows:

[0034] (1) Add 10 g of titanium dioxide and 20 mL of KH580 into 100 mL of ethanol aqueous solution (the concentration of the ethanol aqueous solution is 90%), stir and react at 90°C for 2.5 h, centrifuge, wash and dry to obtain silane coupling agent-modified titanium dioxide.

[0035] (2) Dissolve 0.40 g of sodium periodate in 10 g of deionized water to obtain a sodium periodate aqueous solution, dissolve 3.6 g of guar gum in 120 g of deionized water to obtain a guar gum aqueous solution, add the sodium periodate aqueous solution dropwise to the guar gum aqueous solution and stir evenly, stir the mixed solution in a light-proof environment for 13 h to carry out an oxidation reaction, and after the reaction is completed, pour the reaction solution into a dialysis bag and dialyze for 8 h, and freeze-dry to obtain aldehyded guar gum.

[0036] (3) According to the mass ratio of formaldehyde-modified guar gum to silane coupling agent-modified titanium dioxide of 1:5, silane coupling agent-modified titanium dioxide and formaldehyde-modified guar gum are added into deionized water, and the mixture is heated at 60° C. with stirring for 60 min. After the heating, the mixture is filtered, washed, and vacuum dried to obtain modified titanium dioxide.

[0037] Preparation Example 3

[0038] This preparation example provides a modified titanium dioxide, and the detailed preparation process is as follows:

[0039] (1) Add 10 g of titanium dioxide and 12 mL of KH570 into 80 mL of ethanol aqueous solution (the concentration of the ethanol aqueous solution is 90%), stir and react at 100 °C for 1.5 h, centrifuge, wash and dry to obtain silane coupling agent-modified titanium dioxide.

[0040] (2) Dissolve 0.5 g of sodium periodate in 10 g of deionized water to obtain a sodium periodate aqueous solution, dissolve 2.75 g of guar gum in 110 g of deionized water to obtain a guar gum aqueous solution, add the sodium periodate aqueous solution dropwise to the guar gum aqueous solution and stir evenly, stir the mixed solution in a light-proof environment for 11 h to carry out an oxidation reaction, and after the reaction is completed, pour the reaction solution into a dialysis bag and dialyze for 8 h, and freeze-dry to obtain aldehyded guar gum.

[0041] (3) According to the mass ratio of formaldehyde-modified guar gum to silane coupling agent-modified titanium dioxide of 1:8, silane coupling agent-modified titanium dioxide and formaldehyde-modified guar gum are added into deionized water, and the mixture is heated at 70°C with stirring for 40 min. After the heating, the mixture is filtered, washed, and vacuum dried to obtain modified titanium dioxide.

[0042] 2. Examples

[0043] Example 1

[0044] The present embodiment provides an environmentally friendly aerated concrete block, which is composed of the following raw materials in parts by weight: 62 parts of cement, 39 parts of quicklime, 12 parts of gypsum, 9 parts of fly ash, 10 parts of modified titanium dioxide obtained in Preparation Example 1, 6 parts of silica-alumina porous microspheres, 3 parts of aminosulfonic acid high-efficiency water reducing agent, 6 parts of dichlorotetrafluoroethane, and 110 parts of water.

[0045] This embodiment also provides a method for preparing the above-mentioned environmentally friendly aerated concrete blocks, and the specific preparation process is as follows:

[0046] a. Mix cement, quicklime, gypsum, fly ash, modified titanium dioxide, water reducer and water in the above weight ratio, then add a foaming agent and silicon-aluminum porous microspheres and mix well to obtain a concrete block slurry;

[0047] b. Pour the concrete block slurry of step a into a mold, heat it to 65°C and pre-cure it for 4.5 hours to obtain a concrete block body, demold the aerated concrete block body and divide it, place it in an autoclave, increase the pressure to 1.5MPa and heat it to 170°C at a rate of 3°C / min, steam cure it for 10.5 hours, and cool it to room temperature to obtain an environmentally friendly aerated concrete block.

[0048] Example 2

[0049] The present embodiment provides an environmentally friendly aerated concrete block, which is composed of the following raw materials in parts by weight: 50 parts of cement, 30 parts of quicklime, 15 parts of gypsum, 6 parts of fly ash, 12 parts of modified titanium dioxide obtained in Preparation Example 2, 3 parts of silica-alumina porous microspheres, 2 parts of aminosulfonic acid high-efficiency water reducing agent, 8 parts of dichlorotetrafluoroethane, and 100 parts of water.

[0050] This embodiment also provides a method for preparing the above-mentioned environmentally friendly aerated concrete blocks, and the specific preparation process is as follows:

[0051] a. Mix cement, quicklime, gypsum, fly ash, modified titanium dioxide, water reducer and water in the above weight ratio, then add a foaming agent and silicon-aluminum porous microspheres and mix well to obtain a concrete block slurry;

[0052] b. Pour the concrete block slurry of step a into a mold, heat it to 60°C and pre-cure it for 5 hours to obtain a concrete block body, demold the aerated concrete block body and divide it, then place it in an autoclave, increase the pressure to 1 MPa and heat it to 160°C at a rate of 3°C / min, steam cure it for 11 hours, and cool it to room temperature to obtain an environmentally friendly aerated concrete block.

[0053] Example 3

[0054] The present embodiment provides an environmentally friendly aerated concrete block, which is composed of the following raw materials in parts by weight: 65 parts of cement, 40 parts of quicklime, 8 parts of gypsum, 12 parts of fly ash, 9 parts of modified titanium dioxide obtained in Preparation Example 3, 7 parts of silica-alumina porous microspheres, 4 parts of aminosulfonic acid high-efficiency water reducing agent, 4 parts of dichlorotetrafluoroethane, and 120 parts of water.

[0055] This embodiment also provides a method for preparing the above-mentioned environmentally friendly aerated concrete blocks, and the specific preparation process is as follows:

[0056] a. Mix cement, quicklime, gypsum, fly ash, modified titanium dioxide, water reducer and water in the above weight ratio, then add a foaming agent and silicon-aluminum porous microspheres and mix well to obtain a concrete block slurry;

[0057] b. Pour the concrete block slurry of step a into a mold, heat it to 70°C and pre-cure it for 4 hours to obtain a concrete block body, demold the aerated concrete block body and divide it, then place it in an autoclave, increase the pressure to 2MPa and heat it to 180°C at a rate of 3°C / min, steam cure it for 10 hours, and cool it to room temperature to obtain an environmentally friendly aerated concrete block.

[0058] 3. Comparative Examples

[0059] Comparative Example 1

[0060] This comparative example provides an environmentally friendly aerated concrete block, which is composed of the following raw materials in parts by weight: 62 parts of cement, 39 parts of quicklime, 12 parts of gypsum, 9 parts of fly ash, 10 parts of titanium dioxide, 6 parts of silica-alumina porous microspheres, 3 parts of aminosulfonic acid high-efficiency water reducing agent, 6 parts of dichlorotetrafluoroethane, and 110 parts of water, and the rest is the same as in Example 1.

[0061] Comparative Example 2

[0062] This comparative example provides an environmentally friendly aerated concrete block, which is composed of the following raw materials in parts by weight: 62 parts of cement, 39 parts of quicklime, 12 parts of gypsum, 9 parts of fly ash, 8 parts of titanium dioxide, 2 parts of guar gum, 6 parts of silica-alumina porous microspheres, 3 parts of aminosulfonic acid high-efficiency water reducing agent, 6 parts of dichlorotetrafluoroethane, and 110 parts of water, and the rest is the same as in Example 1.

[0063] Comparative Example 3

[0064] This comparative example provides an environmentally friendly aerated concrete block, which is composed of the following raw materials in parts by weight: 62 parts of cement, 39 parts of quicklime, 12 parts of gypsum, 9 parts of fly ash, 10 parts of modified titanium dioxide obtained in Preparation Example 1, 6 parts of aluminum powder, 3 parts of aminosulfonic acid high-efficiency water reducing agent, 6 parts of dichlorotetrafluoroethane, and 110 parts of water, and the rest is the same as Example 1.

[0065] 4. Experimental Examples

[0066] Experimental Example 1

[0067] This experimental example tests the strength of the environmentally friendly aerated concrete blocks obtained in Examples 1-3 and Comparative Examples 1-3, and the testing process is as follows:

[0068] The environmentally friendly aerated concrete blocks prepared in Examples 1-3 and Comparative Examples 1-3 were respectively made into 10 standard specimens of 4 cm × 4 cm × 16 cm, and each standard specimen was placed under the curing conditions of room temperature 20°C and 95% RH for 3d and 28d, and the compressive strength and flexural strength of each specimen at 3d and 28d were recorded. The compressive strength and flexural strength were tested in accordance with the provisions of GB / T11968-2020, and the compressive strength and flexural strength values ​​were the average values ​​of the 10 standard specimens. The results are shown in Table 1.

[0069] Table 1

[0070]

[0071] It can be seen from Table 1 that when the specimens were cured for 3 days under the same environment, the compressive strength of the specimens of Examples 1 to 3 was higher than that of Comparative Examples 1 to 3. The above results show that the environmentally friendly aerated concrete blocks provided by the present invention have higher early strength.

[0072] When each specimen was cured for 28 days under the same environment, the compressive strength and flexural strength of the specimens of Examples 1-3 were significantly higher than those of Comparative Examples 1-2. Further analysis shows that, compared with Examples 1-3, Comparative Examples 1-2 changed the formula of the environmentally friendly aerated concrete blocks. Among them, the formula of the environmentally friendly aerated concrete blocks of Comparative Example 1 uses titanium dioxide instead of modified titanium dioxide; the formula of the environmentally friendly aerated concrete blocks of Comparative Example 2 uses titanium dioxide and guar gum instead of modified titanium dioxide. It can be seen from the above that the modified titanium dioxide of the present invention can improve the strength of environmentally friendly aerated concrete blocks.

[0073] When each specimen was cured for 28 days under the same environment, the compressive strength and flexural strength of the specimens of Examples 1-3 were higher than those of Comparative Example 3. Further analysis shows that compared with Examples 1-3, the formula of the environmentally friendly aerated concrete blocks of Comparative Example 3 uses aluminum powder instead of silica-alumina porous microspheres. It can be seen from the above that silica-alumina porous microspheres can improve the strength of environmentally friendly aerated concrete blocks. This is because compared with the use of aluminum powder, the silica-alumina porous microspheres of the present invention produce hydrogen through hydration reaction, and can form a more uniform pore structure during the preparation process of aerated concrete blocks, thereby improving the strength performance of aerated concrete blocks. In summary, the environmentally friendly aerated concrete blocks of the present invention have excellent strength performance.

[0074] Experimental Example 2

[0075] This experimental example tests the weather resistance of the environmentally friendly aerated concrete blocks prepared in Examples 1-3 and Comparative Examples 1-3, and the testing process is as follows:

[0076] The environmentally friendly aerated concrete blocks prepared in Examples 1-3 and Comparative Examples 1-3 were respectively made into 4cm×4cm×16cm standard test pieces, 10 of each, to test the thermal conductivity, water absorption and frost resistance of each test piece.

[0077] Thermal conductivity: The thermal conductivity of the environmentally friendly aerated concrete blocks prepared in Examples 1-3 and Comparative Examples 1-3 was tested in accordance with the provisions of GB / T11968-2020. The final result was the average value of 10 standard specimens. The results are shown in Table 2.

[0078] Water absorption rate: The water absorption rate of the environmentally friendly aerated concrete blocks prepared in Examples 1-3 and Comparative Examples 1-3 was tested in accordance with the provisions of GB / T11969-2020. The final result was the average value of 10 standard test pieces. The results are shown in Table 2.

[0079] Frost resistance: According to the provisions of GB / T11968-2020, the mass loss rate and post-freezing compressive strength of the environmentally friendly aerated concrete blocks prepared in Examples 1-3 and Comparative Examples 1-3 were tested after 15 freeze-thaw cycles. The final result is the average value of 10 standard specimens. The results are shown in Table 2.

[0080] Table 2

[0081]

[0082] It is known from Table 2 that compared with Examples 1-3, the thermal conductivity, water absorption, mass loss rate of blocks after 15 freeze-thaw cycles and post-freezing compressive strength of the environmentally friendly aerated concrete blocks obtained in Example 1-2 are significantly reduced, and the thermal conductivity, water absorption, mass loss rate of blocks after 15 freeze-thaw cycles and post-freezing compressive strength of the environmentally friendly aerated concrete blocks obtained in Example 2 are reduced. That is, compared with Examples 1-3, the weather resistance of the environmentally friendly aerated concrete blocks obtained in Example 1-2 is poor. Further analysis shows that compared with Examples 1-3, titanium dioxide or a mixture of titanium dioxide and aldehyde-modified guar gum is used in the environmentally friendly aerated concrete block formula of Example 1-2 to replace modified titanium dioxide. It can be seen from the above that the modified titanium dioxide of the present invention can improve the weather resistance of environmentally friendly aerated concrete blocks.

[0083] Compared with Examples 1-3, the thermal conductivity, water absorption, mass loss rate of the blocks after 15 freeze-thaw cycles, and post-freezing compressive strength of the environmentally friendly aerated concrete blocks prepared in Example 3 are significantly reduced. Further analysis shows that compared with Examples 1-3, aluminum powder is used instead of silicon-aluminum porous microspheres in the formula of the environmentally friendly aerated concrete blocks of Example 3. It can be seen from the above that silicon-aluminum porous microspheres will affect the weather resistance of aerated concrete blocks. In summary, the environmentally friendly aerated concrete blocks of the present invention have excellent weather resistance.

[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. The basic principles and main features of the present invention have been described above with specific implementation schemes. On the basis of the present invention, some modifications or replacements may be made thereto, but these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of protection claimed by the present invention.

Claims

1. An environmentally friendly aerated concrete block, characterized in that: The raw materials include the following parts by weight: 50-65 parts of cement, 30-40 parts of quicklime, 8-15 parts of gypsum, 6-12 parts of fly ash, 9-12 parts of modified titanium dioxide, 3-7 parts of silicon-aluminum porous microspheres, 2-4 parts of water reducing agent, 4-8 parts of foaming agent, and 100-120 parts of water; The preparation process of the modified titanium dioxide is as follows: (1) adding titanium dioxide and a silane coupling agent into an ethanol aqueous solution, stirring for reaction, and purifying to obtain silane coupling agent-modified titanium dioxide; (2) adding sodium periodate solution to the guar gum solution and stirring evenly, and performing oxidation reaction in the dark. After the reaction is completed, the reaction solution is purified to obtain aldehyded guar gum; (3) adding the silane coupling agent modified titanium dioxide of step (1) and the formaldehyde-modified guar gum of step (2) into deionized water, heating and reacting under stirring conditions, and purifying to obtain modified titanium dioxide; The amount ratio of titanium dioxide, silane coupling agent and ethanol aqueous solution in step (1) is 1 g: 1-2 mL: 8-10 mL; the concentration of the ethanol aqueous solution is 90%; the temperature of the stirring reaction in step (1) is 90-100° C., and the reaction time is 1.5-2.5 h; The volume ratio of the sodium periodate solution to the guar gum solution in step (2) is 1:10-12; the concentration of the guar gum solution is 0.02-0.03 g / mL, and the concentration of the sodium periodate solution is 0.040-0.050 g / mL; the oxidation reaction time is 11-13 h; In step (3), the mass ratio of the aldehyde-modified guar gum to the silane coupling agent-modified titanium dioxide is 1:4-8; the heating temperature is 60-70°C and the heating time is 40-60 minutes; The silane coupling agent is KH570 or KH580; the water reducer is aminosulfonic acid high-efficiency water reducer; and the foaming agent is dichlorotetrafluoroethane.

2. The method for preparing an environmentally friendly aerated concrete block according to claim 1, characterized in that: The following steps are involved: a. Mix cement, quicklime, gypsum, fly ash, modified titanium dioxide, water reducer and water in proportion by weight, then add a foaming agent and silica-alumina porous microspheres and mix well to obtain a concrete block slurry; b. Pour the concrete block slurry of step a into a mold, pre-curing to obtain a concrete block body, demolding and segmenting, and then steam curing to obtain.

3. The method for preparing an environmentally friendly aerated concrete block according to claim 2, characterized in that: The pre-curing temperature in step b is 60-70° C., and the pre-curing time is 4-5 hours.

4. The method for preparing the environmentally friendly aerated concrete block according to claim 3, characterized in that: The steam curing temperature in step b is 160-180° C., the pressure is 1-2 MPa, and the time is 10-11 h.