Preparation method of high temperature resistant polyurethane elastomer
By using isosorbide and bisphenol A to synthesize polyether polyols, and introducing an aryl imide structure through an acid anhydride compound chain extension reaction, the problem of insufficient heat resistance of polyurethane elastomers is solved, and the high temperature performance is significantly improved. and excellent mechanical properties.
Patent Information
- Application Number
- CN202411029039.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The heat resistance of polyurethane elastomer is insufficient, which limits its application in high-temperature environments. Existing modification methods such as inorganic filler modification and cross-linking modification have problems such as complicated operations or harmful to the human body.
Isosorbide and bisphenol A are used as composite starters to synthesize polyether polyol, and through the chain extension reaction of acid anhydride compounds, an imide structure containing an aromatic group is introduced to improve the high temperature resistance of polyurethane elastomer.
The high temperature resistance and mechanical properties of polyurethane elastomer are significantly improved, the process is simple and easy to operate, and it is suitable for large-scale production.
Smart Images

Figure CN118562092B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane, and in particular relates to a method for preparing a high-temperature resistant polyurethane elastomer. Background Art
[0002] Polyurethane elastomer is a high molecular polymer between rubber and plastic. It has both the high strength of plastic and the elasticity and toughness of rubber. With its good comprehensive performance, it has been widely used in chemical, building materials, metallurgy, automobile and other fields. Its biggest feature is that the hardness, flexibility, heat resistance and wear resistance of the material can be adjusted within a large range. This feature is due to its unique internal two-phase structure of soft and hard segments. Due to thermodynamic incompatibility, microphase separation will occur between the soft and hard segments, each forming an independent micro-region. The hard segment micro-region is dispersed in the soft segment micro-region in the form of rigid particles, which plays a role of physical cross-linking, thereby enhancing the heat resistance, wear resistance and mechanical properties of the material. The soft segment micro-region, as a matrix, provides the material with flexibility, resilience and good low-temperature performance. However, a significant shortcoming of polyurethane elastomer is its heat resistance, and its upper limit of short-term use temperature is only 120°C. This limitation greatly affects its application potential in special fields such as engineering accessories, electronic appliances, aerospace, and national defense.
[0003] At present, researchers often enhance the heat resistance of polyurethane elastomers by modifying them. Common modification methods include silicone modification, inorganic filler modification, and cross-linking modification. Chinese patent CN109096733A improves the heat resistance of polyurethane elastomers by mixing polyurethane elastomers, inorganic fillers, and other additives. However, this method cannot guarantee the dispersion state of inorganic fillers during the mixing process, which easily causes the loss of mechanical properties of polyurethane elastomers and reduces the wear resistance of polyurethane elastomers; Chinese patent CN111187508A generates a prepolymer by mixing polyether polyol and diatomaceous earth powder with isocyanate, and adds silicon carbide powder with a layer of nickel and chromium to mix together to obtain a heat-resistant polyurethane elastomer. However, this method has a complicated operation process and is difficult to scale up production. In addition, chromium and nickel are carcinogens and are harmful to the human body. Summary of the invention
[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide a method for preparing a high temperature resistant polyurethane elastomer, using isosorbide and bisphenol A as composite initiators to synthesize a polyether polyol with high temperature resistance. Isosorbide is a rigid, non-toxic bio-based raw material derived from glucose, and its molecular structure contains two anti-connected tetrahydrofuran rings, which can significantly improve the strength and thermal stability of the polymer. The aromatic ring and carbon-oxygen chain structure of bisphenol A provide specific rigidity and toughness for the polymer, which can effectively improve the stability of the polymer structure. An anhydride compound containing an aromatic structure is selected as a chain extender, and an aromatic imide structure is introduced into the main chain after the reaction, which greatly enhances the high temperature resistance of the polyurethane elastomer under the action of multiple heat-resistant groups.
[0005] The technical solution adopted by the present invention is as follows:
[0006] The method for preparing the high temperature resistant polyurethane elastomer comprises the following steps:
[0007] (1) adding diisocyanate and polyether polyol in a molar ratio of (2-2.2):1 into a nitrogen-protected reaction vessel, and reacting at a temperature-insulated temperature to obtain a polyurethane prepolymer;
[0008] (2) adding an anhydride compound chain extender to the polyurethane prepolymer prepared in step (1), mixing well and then pouring into a preheated mold to continue the reaction. After the reaction is completed, the mold is opened and ripened to obtain a high temperature resistant polyurethane elastomer;
[0009] The polyether polyol uses isosorbide and bisphenol A in a molar ratio of (1-4):1 as a composite initiator, contains a furan ring and a benzene ring structure in the molecular structure, has a functionality of 2, and a number average molecular weight of 790-1205 g / mol.
[0010] In the step (1), the diisocyanate is one of diphenylmethane-4,4'-diisocyanate (MDI) and para-phenylene diisocyanate (PPDI).
[0011] In the step (1), the temperature of the heat preservation reaction is 75-90°C and the time is 1.5-3h.
[0012] In the step (2), the anhydride compound chain extender is one of 3,4,9,10-tetracarboxylic anhydride or 1,4,5,8-naphthalenetetracarboxylic anhydride.
[0013] In the step (2), the molar ratio of the anhydride compound chain extender to the polyurethane prepolymer is (0.5-1):2.
[0014] In the step (2), the process of continuing the reaction is: first, keep the temperature at 78-85°C for 2-3 hours, and then raise the temperature to 123-127°C for 2-3 hours.
[0015] In the step (2), the aging temperature is 85-95°C.
[0016] In the step (1), the preparation method of the polyether polyol comprises the following steps: using isosorbide and bisphenol A as a composite initiator, adding the composite initiator and the DMC catalyst into a high-pressure reactor, performing nitrogen replacement, heating to 80-100°C, evacuating to -0.09 MPa, dehydrating for 1-2 hours, adding propylene oxide in an amount of 16-22 wt.% of the total mass of the composite initiator to initiate a polymerization reaction, and after successful initiation, continuously adding propylene oxide into the high-pressure reactor by a high-pressure pump, catalyzing the propylene oxide to perform ring-opening polymerization under the action of the DMC catalyst, and obtaining the polyether polyol.
[0017] The amount of the DMC catalyst added is 200-500 ppm, preferably 250-300 ppm, based on the total mass of the polyether polyol.
[0018] The temperature of the ring-opening polymerization is 120-145°C, preferably 125-135°C.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The present invention uses bio-based raw materials isosorbide and bisphenol A as composite initiators and adopts a bimetallic catalyst system to catalyze the ring-opening polymerization of alkylene oxide to obtain polyether polyols. The two furan rings in isosorbide and the aromatic ring and carbon-oxygen chain structure of bisphenol A can significantly improve the rigidity and toughness of the polyether polyols, provide excellent mechanical properties, and effectively improve the stability of the polymer structure, greatly improving the high temperature resistance of the product;
[0021] (2) The present invention introduces an imide structure containing an aromatic group into the main chain of the polyurethane by a chain extension reaction between an anhydride compound and an isocyanate group. The aromatic group and the polyimide have the properties of high thermal stability and high mechanical strength, which further enhances the mechanical properties and thermal stability of the product;
[0022] (3) The present invention selects isosorbide and bisphenol A as composite initiators, polymerizes them with alkylene oxide under a bimetallic catalytic system to obtain a polyether polyol having an aromatic ring and a furan ring structure, reacts with isocyanate to form a prepolymer, and introduces an aromatic imide structure through an acid anhydride reaction. Under the action of multiple heat-resistant groups, a polyurethane elastomer with high temperature resistance and excellent mechanical properties is obtained. The process is simple and easy to operate, and is convenient for large-scale production and conversion. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The thermogravimetric curves of the polyurethane elastomers prepared in the examples and comparative examples are shown in FIG. DETAILED DESCRIPTION
[0024] The present invention is further described below with reference to the embodiments, but they do not limit the implementation of the present invention.
[0025] The raw materials used in the examples and comparative examples are conventional commercially available raw materials unless otherwise specified, and the process methods used in the examples and comparative examples are conventional methods in the art unless otherwise specified.
[0026] Some of the raw materials used in the examples and comparative examples are described as follows:
[0027] INOVOL C204N, purchased from Shandong Yinuowei New Materials Co., Ltd. (functionality 2, initiator is propylene glycol, number average molecular weight 400 g / mol);
[0028] Isosorbide was purchased from Shandong Tianli Pharmaceutical Co., Ltd.;
[0029] Bisphenol A was purchased from Shanghai Sinopec Mitsui Chemicals Co., Ltd.;
[0030] 3,4,9,10-Tetracarboxylic anhydride, purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd.;
[0031] 1,4,5,8-Naphthalenetetracarboxylic anhydride was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0032] Example 1
[0033] The preparation method of the polyether polyol comprises the following steps:
[0034] 68.4 g of bisphenol A, 102.2 g of isosorbide and 0.16 g of DMC catalyst were added to a high-pressure reactor. After nitrogen replacement for 3 times, the temperature was raised to 100°C, evacuated to -0.09 MPa, dehydrated for 2 h, and then heated to 125°C. 35 g of propylene oxide was added dropwise to initiate the polymerization reaction. After successful initiation, when the pressure dropped to -0.08 MPa, 594.4 g of propylene oxide was slowly added to the high-pressure reactor by a high-pressure pump. The pressure during the polymerization reaction was controlled to be less than 0.30 MPa. After the addition was completed, the internal pressure reaction was carried out for 2 h, and the monomer removal was carried out for 0.5 h to obtain a polyether polyol with a functionality of 2, a hydroxyl value of 139.6 mgKOH / g, a viscosity of 660 mPa·s at 25°C, a pH of 6.4, an acid value of 0.013 mgKOH / g, and a number average molecular weight of 804 g / mol.
[0035] The method for preparing the high temperature resistant polyurethane elastomer comprises the following steps:
[0036] (1) 117.3 g of diphenylmethane-4,4'-diisocyanate and 188.6 g of polyether polyol were added to a nitrogen-protected reaction vessel, and the temperature was raised to 75°C for 3 h to obtain a polyurethane prepolymer with an -NCO% content of 6.37 wt.% and a number average molecular weight of 1304 g / mol;
[0037] (2) Take 180 g of the polyurethane prepolymer prepared in step (1), add 21.64 g of 3,4,9,10-tetracarboxylic anhydride thereto, mix well and pour into a mold, first keep the temperature at 78°C for reaction for 3 h, then raise the temperature to 123°C for reaction for 3 h, after the reaction is completed, open the mold and place it on a hot plate at 85°C for maturation, and after maturation, a high temperature resistant polyurethane elastomer is obtained.
[0038] Example 2
[0039] The preparation method of the polyether polyol comprises the following steps:
[0040] 114g of bisphenol A, 73g of isosorbide and 0.4g of DMC catalyst were added to the autoclave. After nitrogen replacement for 3 times, the temperature was raised to 100°C, evacuated to -0.09MPa, dehydrated for 2h, and then heated to 120°C. 30g of propylene oxide was added dropwise to initiate the polymerization reaction. After successful initiation, when the pressure dropped to -0.08MPa, 583g of propylene oxide was slowly added to the autoclave by a high-pressure pump. The pressure during the polymerization reaction was controlled to be less than 0.30MPa. After the addition was completed, the internal pressure reaction was carried out for 2h, and the monomer removal was carried out for 0.5h to obtain a polyether polyol with a functionality of 2, a hydroxyl value of 141.5mgKOH / g, a viscosity of 1015mPa·s at 25°C, a pH of 6.5, an acid value of 0.02mgKOH / g, and a number average molecular weight of 793g / mol.
[0041] The method for preparing the high temperature resistant polyurethane elastomer comprises the following steps:
[0042] (1) Add 104 g of diphenylmethane-4,4'-diisocyanate and 150 g of polyether polyol into a nitrogen-protected reaction vessel, heat to 90°C and react for 2 h to obtain a polyurethane prepolymer with an -NCO% content of 6.35 wt.% and a number average molecular weight of 1293 g / mol;
[0043] (2) Take 160 g of the polyurethane prepolymer prepared in step (1), add 8.3 g of 1,4,5,8-naphthalenetetracarboxylic anhydride thereto, mix well and pour into a mold, first keep the temperature at 85°C for 2 h, then raise the temperature to 127°C for 2 h, open the mold after the reaction is completed, and place it on a hot plate at 95°C for maturation. After maturation, a high-temperature resistant polyurethane elastomer is obtained.
[0044] Example 3
[0045] The preparation method of the polyether polyol comprises the following steps:
[0046] 45.6 g of bisphenol A, 116.8 g of isosorbide and 0.3 g of DMC catalyst were added to a high-pressure reactor. After nitrogen replacement for 3 times, the temperature was raised to 100°C, evacuated to -0.09 MPa, dehydrated for 2 h, and then heated to 145°C. 30 g of propylene oxide was added dropwise to initiate the polymerization reaction. After successful initiation, when the pressure dropped to -0.08 MPa, 807.6 g of propylene oxide was slowly added to the high-pressure reactor by a high-pressure pump. The pressure during the polymerization reaction was controlled to be less than 0.30 MPa. After the addition was completed, the internal pressure reaction was carried out for 2 h, and the monomer removal was carried out for 0.5 h to obtain a polyether polyol with a functionality of 2, a hydroxyl value of 112.5 mgKOH / g, a viscosity of 624 mPa·s at 25°C, a pH of 6.3, an acid value of 0.017 mgKOH / g, and a number average molecular weight of 997 g / mol.
[0047] The method for preparing the high temperature resistant polyurethane elastomer comprises the following steps:
[0048] (1) 37.07 g of p-phenylene diisocyanate and 110 g of polyether polyol were added to a nitrogen-protected reaction vessel, and the temperature was raised to 80° C. for 2.5 h to obtain a polyurethane prepolymer with an -NCO% content of 6.45 wt.% and a number average molecular weight of 1317 g / mol;
[0049] (2) Take 120 g of the polyurethane prepolymer prepared in step (1), add 17.86 g of 3,4,9,10-tetracarboxylic anhydride thereto, mix well and pour into a mold, first keep the temperature at 80°C for 2 h, then raise the temperature to 124°C for 2 h, open the mold after the reaction is completed, and place it on a hot plate at 90°C for maturation. After maturation, a high-temperature resistant polyurethane elastomer is obtained.
[0050] Example 4
[0051] The preparation method of the polyether polyol comprises the following steps:
[0052] 57g of bisphenol A, 109.5g of isosorbide and 0.48g of DMC catalyst were added to the autoclave. After nitrogen replacement for 3 times, the temperature was raised to 100°C, evacuated to -0.09MPa, dehydrated for 2h, and then the temperature was raised to 130°C. 35g of propylene oxide was added dropwise to initiate the polymerization reaction. After successful initiation, when the pressure dropped to -0.08MPa, 998.5g of propylene oxide was slowly added to the autoclave by a high-pressure pump. The pressure during the polymerization reaction was controlled to be less than 0.30MPa. After the addition was completed, the internal pressure reaction was carried out for 2h, and the monomer removal was carried out for 0.5h to obtain a polyether polyol with a functionality of 2, a hydroxyl value of 93.2mgKOH / g, a viscosity of 597mPa·s at 25°C, a pH of 6.7, an acid value of 0.022mgKOH / g, and a number average molecular weight of 1204g / mol.
[0053] The method for preparing the high temperature resistant polyurethane elastomer comprises the following steps:
[0054] (1) Add 50 g of p-phenylene diisocyanate and 175 g of polyether polyol into a nitrogen-protected reaction vessel, heat to 85° C. and react for 1.5 h to obtain a polyurethane prepolymer with an -NCO% content of 5.53 wt.% and a number average molecular weight of 1524 g / mol;
[0055] (2) Take 130 g of the polyurethane prepolymer prepared in step (1), add 13.37 g of 3,4,9,10-tetracarboxylic anhydride thereto, mix well and pour into a mold, first keep the temperature at 82°C for 2 h, then raise the temperature to 125°C for 2 h, after the reaction is completed, open the mold and place it on a hot plate at 92°C for aging, and after aging, a high temperature resistant polyurethane elastomer is obtained.
[0056] Comparative Example 1
[0057] The preparation method of the polyether polyol comprises the following steps:
[0058] 228g of bisphenol A and 0.04g of DMC catalyst were added to a pressure-resistant container. After nitrogen replacement for 3 times, the temperature was raised to 100°C for dehydration for 2h, and the temperature was raised to 130°C for initiation by adding 35g of propylene oxide dropwise. After the pressure dropped to -0.08MPa, 537g of propylene oxide liquid was added. The pressure was controlled to be less than 0.30MPa during the reaction. The internal pressure was reacted for 2h, and the monomer removal was performed for 0.5h to obtain bisphenol A polyether polyol with a functionality of 2, a hydroxyl value of 140.8mgKOH / g, a viscosity of 2107mPa·s at 25°C, a pH of 5.5, an acid value of 0.063mgKOH / g, and a number average molecular weight of 797g / mol.
[0059] The method for preparing the high temperature resistant polyurethane elastomer comprises the following steps:
[0060] (1) 120 g of bisphenol A polyether polyol and 75.28 g of diphenylmethane-4,4'-diisocyanate were mixed, and the temperature was raised to 80°C and kept for 3 h to obtain a prepolymer with an -NCO% content of 6.46 wt.% and a number average molecular weight of 1297 g / mol;
[0061] (2) Take 120 g of prepolymer, add 7.88 g of BDO, stir evenly, pour into a mold at a mold temperature of 110°C, and cure to obtain a polyurethane elastomer.
[0062] Comparative Example 2
[0063] The preparation method of the polyether polyol comprises the following steps:
[0064] 200g of C204N, 73g of isosorbide and 0.4g of DMC catalyst were added to the autoclave. After nitrogen replacement for 3 times, the temperature was raised to 100°C, evacuated to -0.09MPa, dehydrated for 2h, and then heated to 130°C. 30g of propylene oxide was added dropwise to initiate the polymerization reaction. After successful initiation, when the pressure dropped to -0.08MPa, 697g of propylene oxide was slowly added to the autoclave by a high-pressure pump. The pressure during the polymerization reaction was controlled to be less than 0.30MPa. After the addition was completed, the internal pressure reaction was carried out for 2h, and the monomer removal was carried out for 0.5h to obtain a polyether polyol with a functionality of 2, a hydroxyl value of 112.88mgKOH / g, a viscosity of 498mPa·s at 25°C, a pH of 6.8, an acid value of 0.013mgKOH / g, and a number average molecular weight of 994g / mol.
[0065] The method for preparing the high temperature resistant polyurethane elastomer comprises the following steps:
[0066] (1) Add 48.3 g of p-phenylene diisocyanate and 150 g of polyether polyol into a nitrogen-protected reaction vessel, heat to 85° C. and react for 1.5 h to obtain a polyurethane prepolymer with an -NCO% content of 6.42 wt.% and a number average molecular weight of 1314 g / mol;
[0067] (2) Take 130 g of the polyurethane prepolymer prepared in step (1), add 15.51 g of 3,4,9,10-tetracarboxylic anhydride thereto, mix well and pour into a mold, first keep the temperature at 82°C for 2 h, then raise the temperature to 125°C for 2 h, open the mold after the reaction is completed, and place it on a hot plate at 92°C for aging, to obtain a polyurethane elastomer.
[0068] With reference to GB / T528-2009, mechanical properties of the polyurethane elastomers prepared in Examples 1 to 4 and Comparative Examples 1 to 2 were tested, and the test results are shown in Table 1.
[0069] Table 1 Mechanical properties test results
[0070]
[0071] It can be seen from the data in Table 1 that in Examples 1 to 4, as the molecular weight of the polyether polyol used to prepare the polyurethane elastomer decreases, the proportion of the hard segment in the molecular structure increases, and the mechanical properties of the obtained polyurethane elastomer gradually improve. This is because the mixed initiator of the polyether polyol itself has a large number of rigid structures, which have a synergistic effect with each other. And because the chain extender used in the polyurethane elastomer also contains a large number of rigid structures, the proportion of the hard segment content in the polyurethane elastomer is also increased, the size of the hard segment micro-region is increased, and the degree of mixing of the hard segment and the soft segment is reduced, resulting in an increase in the degree of microphase separation, so that the obtained polyurethane elastomer has very excellent mechanical properties. Under the condition that the molecular weight of the selected polyether polyol is similar, the comparative example is compared with the embodiment, due to the difference in the polyether polyol initiator or the difference in the chain extender, the molecular structure of the polyurethane elastomer finally obtained is different, and thus its mechanical properties are significantly different from those of the embodiment.
[0072] The high temperature resistance of the polyurethane elastomers prepared in Examples 1 to 4 and Comparative Examples 1 to 2 was tested using a differential thermogravimetric analyzer. The test results are as follows: Figure 1 As shown, Figure 1 The feature information is shown in Table 2.
[0073] Table 2 Heat resistance test results
[0074]
[0075] Note: T / 5% is the temperature at which the polyurethane elastomer decomposes by 5%; T / 20% is the temperature at which the polyurethane elastomer decomposes by 20%; T / 50% is the temperature at which the polyurethane elastomer decomposes by 50%; T / 80% is the temperature at which the polyurethane elastomer decomposes by 80%.
[0076] from Figure 1 It can be seen from the data in Table 2 that the heat resistance of the polyurethane elastomer prepared by the method of the present invention is greatly improved. This is because the polyurethane elastomer synthesized with isosorbide and bisphenol A as raw materials has structures such as furan rings, aromatic rings and carbon oxygen chains, which increases the proportion of hard segments in the elastomer and can improve the high temperature resistance of the product. In addition, the imide ring and aromatic ring introduced by the anhydride compound are on the same plane, producing a conjugated effect, which improves the heat resistance stability of the polyurethane elastomer. Under the comprehensive effect of multiple heat-resistant groups, the polyurethane elastomer finally obtained has excellent heat resistance.
Claims
1. A method for preparing a high temperature resistant polyurethane elastomer, characterized in that: The following steps are involved: (1) adding diisocyanate and polyether polyol in a molar ratio of (2-2.2):1 into a reaction container, and reacting at a temperature-insulating state to obtain a polyurethane prepolymer; (2) adding an anhydride compound chain extender to the polyurethane prepolymer obtained in step (1), mixing well and then pouring into a mold to continue the reaction. After the reaction is completed, the mold is opened and ripened to obtain a high temperature resistant polyurethane elastomer; The polyether polyol is a composite initiator of isosorbide and bisphenol A in a molar ratio of (1-4):1, has a functionality of 2, and a number average molecular weight of 790-1205 g / mol; The acid anhydride compound chain extender is one of 3,4,9,10-tetracarboxylic anhydride and 1,4,5,8-naphthalenetetracarboxylic anhydride.
2. The method for preparing a high temperature resistant polyurethane elastomer according to claim 1, characterized in that: In the step (1), the diisocyanate is one of diphenylmethane-4,4'-diisocyanate or p-phenylene diisocyanate.
3. The method for preparing a high temperature resistant polyurethane elastomer according to claim 1, characterized in that: In the step (1), the temperature of the heat preservation reaction is 75-90°C and the time is 1.5-3h.
4. The method for preparing a high temperature resistant polyurethane elastomer according to claim 1, characterized in that: In the step (2), the molar ratio of the anhydride compound chain extender to the polyurethane prepolymer is (0.5-1):
2.
5. The method for preparing a high temperature resistant polyurethane elastomer according to claim 1, characterized in that: In the step (2), the process of continuing the reaction is: first, keep the temperature at 78-85°C for 2-3 hours, and then raise the temperature to 123-127°C for 2-3 hours.
6. The method for preparing a high temperature resistant polyurethane elastomer according to claim 1, characterized in that: In the step (2), the aging temperature is 85-95°C.
7. The method for preparing a high temperature resistant polyurethane elastomer according to claim 1, characterized in that: In the step (1), the method for preparing the polyether polyol comprises the following steps: using isosorbide and bisphenol A as composite initiators, catalyzing propylene oxide to undergo ring-opening polymerization under the action of a DMC catalyst, thereby obtaining the polyether polyol.
8. The method for preparing a high temperature resistant polyurethane elastomer according to claim 7, characterized in that: The added amount of the DMC catalyst is 200-500 ppm of the total mass of the polyether polyol.
9. The method for preparing a high temperature resistant polyurethane elastomer according to claim 7, characterized in that: The temperature of the ring-opening polymerization is 120-145°C.