Material preparation method of fully plasticized roller support for coal mine transportation and roller support
By combining nylon and polyvinyl chloride blends with flame retardant and antistatic agent, a high-strength, lightweight, corrosion-resistant fully plasticized roller bracket was prepared, which solved the problems of large quality and easy corrosion of steel components. It achieves noise reduction, corrosion resistance, flame retardant and anti-static effects.
Patent Information
- Application Number
- CN202411035382.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The steel components of the existing roller frame for coal mine transportation are of high quality, inconvenient installation, easy to corrode during use, and strong corrosiveness in high humidity and high heat environments, resulting in high noise, short service life, and failure to effectively reduce static electricity and fires risk.
The fully plasticized roller bracket is prepared by blending nylon and polyvinyl chloride. Through melt blending and injection molding, organic-inorganic hybrid flame retardant and organic compound antistatic agent are added to form high strength, lightweight and corrosion-resistant , flame retardant and antistatic roller bracket.
The roller bracket is achieved with high strength, light weight, corrosion resistance, noise reduction, flame retardant and anti-static effects, reducing installation difficulty and noise, improving service life, and maintaining stability in high humidity and high heat environments.
Smart Images

Figure CN118562289B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of coal mine mechanical equipment, and relates to a material preparation method for a fully plasticized idler support for coal mine transportation, and also relates to a fully plasticized idler support for coal mine transportation. Background Art
[0002] Among them, both underground or open-pit coal mining require belt conveyors to achieve the transfer and transportation of coal. Belt conveyors are widely used conveying equipment in the mining field and are important supporting equipment for mechanized fully-mechanized coal mining. A belt conveyor includes a bottom support, an idler frame, idlers, and a conveyor belt. At present, steel welded parts are used in coal mines to process supports, idler frames, and idlers, and the conveyor belt is realized by the calendering process of a polymer polyvinyl chloride (PVC) modified material. During the operation of the belt conveyor, there are several aspects of potential safety hazards: First, the steel components of the idler frame are heavy, and injuries and scratches often occur during the installation process. Second, the deviation hazard of the conveyor belt, and the friction between the edge of the conveyor belt and the frame will exacerbate the wear and tear of the conveyor belt and tear it, thereby triggering production safety accidents and equipment accidents.
[0003] Therefore, the vast majority of coal mine enterprises design the belt conveyor idler frame in a "pin" shape or a "one" shape. Three idlers are assembled on the idler frame and form a suspended structure. At the same time, the two side idlers and the middle idler form an acute angle, and the surfaces of the two side idlers are slightly higher than the surface of the middle idler, so that the idlers and the conveyor belt form a "U" - shaped transport trough to help reduce belt contact wear and deviation. Among them, Qi Chuangang's "Research on the Serialization Design of the Upper Idler Frame of Belt Conveyors" in the 2nd issue of the "Coal Mine Mechanical and Electrical" journal in 2017, He Jianan of a certain coal marketing group's "Improvement and Application Analysis of the Buffer Idler Frame of Coal Mine Belt Conveyors" in the 10th issue of the "Mechanical Management and Development" journal in 2020, and Li Zhiming et al.'s "Research on the Engineering Optimization of the Long - distance Coal Ash Two - way Transportation System in Alpine Ecologically Fragile Areas" in the 12th issue of the 54th volume of the "Coal Engineering" journal in 2022 all optimize the structure of the transportation mechanism to improve belt wear during transportation, reduce transportation energy consumption, and increase the service life of idlers. However, the idler frames and idlers adopted in the above - mentioned designs are all steel parts. During the coal transportation process, the conveyor belt is subjected to continuous and non - periodic external forces. Due to the direct impact on the idler frame and idlers, the steel components do not have good buffering effects, thus bringing obvious noise and the probability of idler frame damage. At the same time, all current steel - structured idler frames are prone to corrosion in the high - humidity and acid - base environment of underground coal mines, resulting in a decrease in service strength. In addition, the above - mentioned steel - structured idler frames are heavy in quality, bringing great inconvenience to use and installation.
[0004] Therefore, the upgrading and transformation of roller frames used for underground coal mine transportation, especially the functionalization of high strength, light weight, corrosion resistance, noise reduction, and anti-static and flame retardant requirements, will have important safety, efficiency and economic benefits. At present, there are few reports on the relevant patents and literature on the development of roller frames with high strength, light weight, corrosion resistance, noise reduction, flame retardant and anti-static requirements in the process of underground coal mine transportation. Summary of the invention
[0005] The purpose of the present invention is to provide a material preparation method for a fully plasticized roller support for coal mine transportation, which solves the problems of large steel structure mass, high noise during use, and easy corrosion in a high humidity and high heat environment of the existing roller support.
[0006] Another object of the present invention is to provide a fully plasticized roller support for coal mine transportation, which achieves the effects of high strength, light weight and corrosion resistance of the roller support for coal mine transportation.
[0007] The first technical solution adopted by the present invention is a material preparation method of a fully plasticized roller support for coal mine transportation, including the preparation of a nylon blend and a polyvinyl chloride blend;
[0008] The nylon blend is prepared by melt blending nylon, an organic-inorganic hybrid flame retardant and an organic compound antistatic agent; the nylon is one of nylon 6, nylon 66 and nylon 610; the organic-inorganic hybrid flame retardant is one of MXene / pentabromodiphenyl ether, MXene / tris(2-chloropropyl) phosphate, and MXene / 2,2-bis(chloromethyl)cyclopropane; the organic compound antistatic agent is one of siloxane / polyoxyethylene ether, aminopropyl polydimethylsiloxane / epichlorohydrin, and graphite / polyoxyethylene ether;
[0009] The polyvinyl chloride blend is prepared by melt blending polyvinyl chloride, a reinforcing agent, an antioxidant and an antistatic agent.
[0010] The first technical solution of the present invention is also characterized in that:
[0011] The components in the nylon blend include, by mass percentage, 85% to 100% nylon, 5% to 10% organic-inorganic hybrid flame retardant, and 3% to 5% organic compound antistatic agent, and the sum of the mass percentages of the above components is 100%.
[0012] The organic-inorganic hybrid flame retardant is prepared by a hydrothermal method, the hydrothermal temperature is 130°C~180°C, and the hydrothermal reaction time is 24h~48h.
[0013] The melt blending temperature for preparing the nylon blend is 240°C to 280°C.
[0014] The components in the polyvinyl chloride blend include, by mass percentage, polyvinyl chloride 65% to 100%, reinforcing agent 15% to 25%, antioxidant 3% to 5%, and antistatic agent 2% to 5%, and the sum of the mass percentages of the above components is 100%.
[0015] The polyvinyl chloride is one of the rigid polyvinyl chloride prepared by the suspension method or the rigid polyvinyl chloride prepared by the slurry method; the reinforcing agent is one of calcium carbonate, mica powder, and talc; the antioxidant is one of butylated hydroxyanisole, tert-butylhydroquinone, graphite / dilauryl thiodipropionate, and MXene / dilauryl thiodipropionate; the antistatic agent is one of graphite, copper powder, and graphite / polyoxyethylene ether.
[0016] The melt blending temperature for preparing the polyvinyl chloride blend is 180°C~220°C.
[0017] The second technical solution adopted by the present invention is a fully plasticized roller support for coal mine transportation, which is prepared by the material preparation method of the fully plasticized roller support for coal mine transportation of the present invention. The fully plasticized roller support for coal mine transportation includes a beam, side plates are respectively arranged at both ends of the beam, a middle section support is arranged on the beam, the middle section support runs through the beam, and the middle section support and the beam are interference fit, the side plates and the middle section support are both made of nylon blend by injection molding, and the beam is made of polyvinyl chloride blend by extrusion.
[0018] The second technical solution of the present invention is also characterized in that:
[0019] The nylon blend of the side panels and the middle bracket is dried at 120℃~150℃ for 4h~8h before injection molding, and then injection molded. The injection pressure is 300MPa~500MPa, the injection temperature is 250℃~280℃, and the pressure is maintained after injection molding for 30s~60s.
[0020] The beam is extruded through an extruder and water-cooled after extrusion. The extrusion temperature is 190°C to 230°C, the extruder speed is 60rpm to 120rpm, and the water cooling time is 30s to 90s.
[0021] The beneficial effects of the present invention are:
[0022] The material preparation method of the fully plasticized roller support for coal mine transportation of the present invention is based on the high specific strength and high corrosion resistance of plastics. At the same time, it takes advantage of the easy composite modification and functional advantages of plastic materials to achieve the high strength, light weight, corrosion resistance, noise reduction, flame retardancy and antistatic effects of the roller support material for coal mine transportation.
[0023] The fully plasticized roller support for coal mine transportation of the present invention adopts injection molding and extrusion processes and combines plastic composite modification technology. The roller support is mainly aimed at the problems of inconvenient installation caused by the large steel structure mass of the existing roller support, high noise during use, and easy corrosion in a high humidity and high heat environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic structural diagram of a fully plasticized roller support for coal mine transportation according to the present invention;
[0025] Figure 2 The present invention is a flow chart for preparing the side plates and the middle bracket of the fully plasticized roller bracket for coal mine transportation;
[0026] Figure 3 This is a flow chart for preparing the beam of the fully plasticized roller support for coal mine transportation of the present invention;
[0027] Figure 4 This is a comparison diagram of the mechanical properties of the nylon blend used for the side plates and the middle bracket of the fully plasticized roller bracket for coal mine transportation of the present invention;
[0028] Figure 5 This is a comparison chart of the flame retardant properties of the nylon blend used for the side plates and the middle bracket of the fully plasticized roller bracket for coal mine transportation of the present invention;
[0029] Figure 6 This is a comparison chart of the tensile properties of the polyvinyl chloride blend used for the beam of the fully plasticized roller support for coal mine transportation of the present invention;
[0030] Figure 7 This is a comparison chart of the flame retardant properties of the polyvinyl chloride blend used for the beam of the fully plasticized roller support for coal mine transportation of the present invention;
[0031] Figure 8 This is the electron microscope image of the flame retardant, where Figure 8 (a) is a single MXene flame retardant electron microscope image. Figure 8 (b) is an electron micrograph of the organic-inorganic hybrid flame retardant of the present invention;
[0032] Fig. 9 The figure is a comparison chart of the tensile properties of nylon added with graphite powder and the organic composite antistatic agent of the present invention respectively.
[0033] In the figure, 1-1. side plate; 1-2. middle section support; 1-3. beam; 1-4. transport roller. DETAILED DESCRIPTION
[0034] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0035] Example 1
[0036] This embodiment provides a material preparation method for a fully plasticized roller support for coal mine transportation, including the preparation of a nylon blend and a polyvinyl chloride blend;
[0037] The nylon blend is prepared by melt blending nylon 6, MXene / pentabromodiphenyl ether and siloxane / polyoxyethylene ether. The melt blending temperature for preparing the nylon blend is 240° C. The components in the nylon blend include, by mass percentage, 85% nylon 6, 10% MXene / pentabromodiphenyl ether and 5% siloxane / polyoxyethylene ether.
[0038] MXene / pentabromodiphenyl ether was prepared by hydrothermal method with hydrothermal temperature of 130 °C and hydrothermal reaction time of 24 h.
[0039] The polyvinyl chloride blend is prepared by melt-blending rigid polyvinyl chloride prepared by a suspension method, calcium carbonate, butylated hydroxyanisole and graphite. The melt-blending temperature for preparing the polyvinyl chloride blend is 180° C. The components in the polyvinyl chloride blend include, by mass percentage, 65% of rigid polyvinyl chloride prepared by a suspension method, 25% of calcium carbonate, 5% of butylated hydroxyanisole and 5% of graphite.
[0040] The present embodiment also provides a fully plasticized roller support for coal mine transportation, which is prepared by the material preparation method of the fully plasticized roller support for coal mine transportation of the present embodiment. The fully plasticized roller support for coal mine transportation includes a beam 1-3, and side panels 1-1 are respectively provided at both ends of the beam 1-3. A middle section bracket 1-2 is provided on the beam 1-3, and the middle section bracket 1-2 runs through the beam 1-3, and the middle section bracket 1-2 is interference fit with the beam 1-3. The side panels 1-1 and the middle section bracket 1-2 are both made of nylon blend by injection molding, and the beam 1-3 is made of polyvinyl chloride blend by extrusion.
[0041] The nylon blend of the side plate 1-1 and the middle bracket 1-2 is dried at 120°C for 8 hours before injection molding, and then injection molded at an injection pressure of 300MPa and an injection temperature of 250°C. After injection molding, the pressure is maintained for 30s.
[0042] Beam 1-3 is extruded through an extruder and water-cooled after extrusion. The extrusion temperature is 190° C., the extruder speed is 60 rpm, and the water cooling time is 30 s.
[0043] Example 2
[0044] This embodiment provides a material preparation method for a fully plasticized roller support for coal mine transportation, including the preparation of a nylon blend and a polyvinyl chloride blend;
[0045] The nylon blend is prepared by melt blending nylon, an organic-inorganic hybrid flame retardant and an organic compound antistatic agent. The melt blending temperature for preparing the nylon blend is 280°C. The components in the nylon blend include, by mass percentage, 92% nylon 66, 5% MXene / tris(2-chloropropyl) phosphate, and 3% aminopropyl polydimethylsiloxane / epichlorohydrin.
[0046] The organic-inorganic hybrid flame retardant was prepared by a hydrothermal method with a hydrothermal temperature of 180°C and a hydrothermal reaction time of 24 h.
[0047] The polyvinyl chloride blend is prepared by melt-blending rigid polyvinyl chloride prepared by a slurry method, mica powder, tert-butylhydroquinone and copper powder. The melt-blending temperature for preparing the polyvinyl chloride blend is 220° C. The components in the polyvinyl chloride blend include, by mass percentage, 80% rigid polyvinyl chloride prepared by a slurry method, 15% mica powder, 3% tert-butylhydroquinone and 2% copper powder.
[0048] The present embodiment also provides a fully plasticized roller support for coal mine transportation, which is prepared by the material preparation method of the fully plasticized roller support for coal mine transportation of the present embodiment. The fully plasticized roller support for coal mine transportation includes a beam 1-3, and side panels 1-1 are respectively provided at both ends of the beam 1-3. A middle section bracket 1-2 is provided on the beam 1-3, and the middle section bracket 1-2 runs through the beam 1-3, and the middle section bracket 1-2 is interference fit with the beam 1-3. The side panels 1-1 and the middle section bracket 1-2 are both made of nylon blend by injection molding, and the beam 1-3 is made of polyvinyl chloride blend by extrusion.
[0049] The nylon blend of the side plate 1-1 and the middle bracket 1-2 is dried at 150°C for 4 hours before injection molding, and then injection molded at an injection pressure of 500MPa and an injection temperature of 280°C. After injection molding, the pressure is maintained for 60s.
[0050] Beam 1-3 was extruded through an extruder and water-cooled after extrusion. The extrusion temperature was 230° C., the extruder speed was 120 rpm, and the water-cooling time was 90 s.
[0051] Example 3
[0052] This embodiment provides a material preparation method for a fully plasticized roller support for coal mine transportation, including the preparation of a nylon blend and a polyvinyl chloride blend;
[0053] The nylon blend is made of nylon 610, and the components in the nylon blend are included according to mass percentage, and nylon 610 is 100%;
[0054] The polyvinyl chloride blend is made of rigid polyvinyl chloride prepared by a suspension method. The components in the polyvinyl chloride blend include, by weight percentage, 100% of the rigid polyvinyl chloride prepared by the suspension method.
[0055] The present embodiment also provides a fully plasticized roller support for coal mine transportation, which is prepared by the material preparation method of the fully plasticized roller support for coal mine transportation of the present embodiment. The fully plasticized roller support for coal mine transportation includes a beam 1-3, and side panels 1-1 are respectively provided at both ends of the beam 1-3. A middle section bracket 1-2 is provided on the beam 1-3, and the middle section bracket 1-2 runs through the beam 1-3, and the middle section bracket 1-2 is interference fit with the beam 1-3. The side panels 1-1 and the middle section bracket 1-2 are both made of nylon blend by injection molding, and the beam 1-3 is made of polyvinyl chloride blend by extrusion.
[0056] The nylon blend of the side plate 1-1 and the middle bracket 1-2 is dried at 130°C for 5 hours before injection molding, and then injection molded at an injection pressure of 450MPa and an injection temperature of 260°C. After injection molding, the pressure is maintained for 45s.
[0057] Beam 1-3 is extruded through an extruder and water-cooled after extrusion. The extrusion temperature is 200° C., the extruder speed is 80 rpm, and the water cooling time is 60 s.
[0058] Example 4
[0059] This embodiment provides a material preparation method for a fully plasticized roller support for coal mine transportation, including the preparation of a nylon blend and a polyvinyl chloride blend;
[0060] The nylon blend is prepared by melt blending nylon 610, MXene / tris(2-chloropropyl) phosphate and aminopropyl polydimethylsiloxane / epichlorohydrin. The melt blending temperature for preparing the nylon blend is 270°C. The components in the nylon blend include, by mass percentage, 88% nylon 610, 8% MXene / tris(2-chloropropyl) phosphate, and 4% aminopropyl polydimethylsiloxane / epichlorohydrin.
[0061] MXene / tri(2-chloropropyl) phosphate was prepared by a hydrothermal method with a hydrothermal temperature of 150°C and a hydrothermal reaction time of 30 h. The hydrothermal method was used to achieve high-pressure and high-temperature in-situ intercalation.
[0062] The polyvinyl chloride blend is prepared by melt blending slurry-process rigid polyvinyl chloride, talc, MXene / dilauryl thiodipropionate and graphite / polyoxyethylene ether. The melt blending temperature for preparing the polyvinyl chloride blend is 210°C. The components in the polyvinyl chloride blend include, by mass percentage, slurry-process rigid polyvinyl chloride 73%, talc 20%, MXene / dilauryl thiodipropionate 4%, and graphite / polyoxyethylene ether 3%.
[0063] This embodiment also provides a fully plasticized roller support for coal mine transportation, which is prepared by the material preparation method of the fully plasticized roller support for coal mine transportation of this embodiment. Figure 1As shown, the fully plasticized roller support for coal mine transportation includes a beam 1-3, side plates 1-1 are respectively provided at both ends of the beam 1-3, a middle section support 1-2 is provided on the beam 1-3, the middle section support 1-2 runs through the beam 1-3, and the middle section support 1-2 and the beam 1-3 are interference fit, the side plates 1-1, the middle section support 1-2 and the beam 1-3 constitute a fully plasticized roller support, the side plates 1-1 and the middle section support 1-2 have card grooves, and the transport rollers 1-4 are assembled with the side plates 1-1 and the middle section support 1-2 through the card grooves to realize transportation.
[0064] like Figure 2 As shown, the side plate 1-1 and the middle bracket 1-2 are both made of nylon blend by injection molding. The nylon blend of the side plate 1-1 and the middle bracket 1-2 is dried at 145°C for 6 hours before injection molding, and then injection molded. The injection molding pressure is 400MPa, the injection molding temperature is 268°C, and the pressure is maintained after injection molding for 55s.
[0065] like Figure 3 As shown, beam 1-3 is made of polyvinyl chloride blend by extrusion. Beam 1-3 is extruded by an extruder and water-cooled after extrusion. The extrusion temperature is 210° C., the extruder speed is 88 rpm, and the water cooling time is 76 s.
[0066] Under the conditions of relative humidity of 55%~85% and temperature of 40~60℃, the side panels, middle brackets and beams will not rust within 3~5 years; compared with existing steel structure transportation parts, the noise during use is reduced by 30%~60%.
[0067] Compared with existing flame retardants, the organic-inorganic hybrid flame retardant of the present invention is one of MXene / pentabromodiphenyl ether, MXene / tris(2-chloropropyl) phosphate, and MXene / 2,2-bis(chloromethyl)cyclopropane. Its advantage is that the conductive particle MXene is used as the carrier material, and the organic component is effectively intercalated with MXene by using a hydrothermal preparation process. Therefore, the hybrid flame retardant can not only improve the conductivity of nylon, but also effectively improve the dispersibility of the organic component in the nylon matrix, reduce the amount of flame retardant, and ensure the plasticity and strength of the final injection molded part.
[0068] Compared with the existing antistatic agents which all use conductive particles, such as graphite powder, copper powder and carbon black, the organic compound antistatic agent of the present invention is one of siloxane / polyoxyethylene ether, aminopropyl polydimethylsiloxane / epichlorohydrin and graphite / polyoxyethylene ether. The compound antistatic agent uses organic as the main component, has high conductivity, good compatibility with nylon materials, and does not deteriorate the mechanical properties of injection molded parts.
[0069] The side panels and brackets are made of nylon blend injection molding, which can achieve rapid molding and short molding cycle. The injection mold is convenient for arranging reinforcement ribs and adjusting the reinforcement ribs to improve the mechanical properties of the injection molded parts. The beam is made of polyvinyl chloride blend extrusion, which is convenient for continuous molding of hollow pipes and has high production efficiency.
[0070] Performance test
[0071] like Figure 4 As shown in the figure, a universal testing machine was used to perform tensile tests on dumbbell-shaped specimens (national standard type I specimen size) prepared by injection molding of nylon and its composite materials, with a tensile rate of 50 mm / min and a test standard of GB / T 1447-2005. The results showed that the tensile strength of pure nylon specimens reached about 135 MPa, and the strain reached 10.2%; when antistatic agent and flame retardant were added to nylon respectively, the tensile strength of the specimens was maintained at about 115 MPa, and the strain was between 6% and 9%; when antistatic agent and flame retardant were added to nylon at the same time, the tensile strength of the specimens remained basically unchanged, and only the strain dropped to about 5%.
[0072] like Figure 5 As shown in the figure, the oxygen index tester was used to test the combustion oxygen index of rectangular strip samples (10mm×4mm×100mm) prepared by injection molding of nylon and its composite materials. The test standard is GB / T 2406.1-2008. The results show that the combustion oxygen demand index of pure nylon sample is 20.3, indicating that nylon is easy to burn in the air; when flame retardant and antistatic agent are added to nylon respectively, the combustion oxygen demand index of the sample is increased to 25.2 and 21.3 respectively, indicating that the modified nylon composite material is not easy to burn in the air; when antistatic and flame retardant are added to nylon at the same time, the combustion oxygen demand index of the sample reaches 26.4, further improving the combustion oxygen demand index.
[0073] like Figure 6As shown in the figure, the dumbbell-shaped specimens (national standard type I specimen size) prepared by injection molding of polyvinyl chloride (PVC) and its composite materials were subjected to tensile tests using a universal testing machine, with a tensile rate of 50 mm / min and a test standard of GB / T 1447-2005. The results show that the tensile strength and tensile modulus of pure PVC specimens are about 74.8 MPa and 4.5 GPa respectively; when the reinforcing agent is added to PVC, the tensile strength and tensile modulus of the specimen are increased to 83.7 MPa and 6.4 GPa respectively; when the antistatic agent is added to PVC, the tensile strength and tensile modulus of the specimen are maintained at 81.7 MPa and 8.4 GPa respectively; when the antioxidant is added to PVC, the tensile strength and tensile modulus of the specimen are 82.2 MPa and 7.3 GPa respectively; when the reinforcing agent, antistatic agent and antioxidant are added to PVC at the same time, the tensile strength and tensile modulus of the specimen are still significantly higher than those of pure PVC, which are 83.0 MPa and 6.8 GPa respectively.
[0074] like Figure 7 As shown in the figure, the flame retardant grade of rectangular strip specimens (10mm×5mm×100mm) prepared by injection molding of PVC and its composite materials were tested using the UL94 standard test and requirements. The results showed that the flame retardant grade of pure PVC specimens reached V0 level, which means that the sample burned without flame for more than 10 seconds after the test flame was taken away. When the reinforcing agent was added to PVC, the flame retardant grade of the specimen reached V0 level; when the antistatic agent was added to PVC, the flame retardant grade of the specimen reached V0 level; when the antioxidant was added to PVC, the flame retardant grade of the specimen reached V0 level; when the reinforcing agent, antistatic agent and antioxidant were added to PVC at the same time, the flame retardant grade of the specimen reached V0 level, indicating that PVC and its composite materials have good flame retardant properties.
[0075] like Figure 8 As shown in Figure 2, scanning electron micrographs of single MXene flame retardant and MXene / hybrid pentabromodiphenyl ether flame retardant prepared by hydrothermal method were taken. The results showed that: Figure 8 As shown in (a), a single MXene flame retardant sheet is thicker and has a smoother surface; Figure 8 As shown in (b), the sheet of MXene hybrid pentabromodiphenyl ether flame retardant prepared by hydrothermal method becomes thinner, and a layer of organic pentabromodiphenyl ether is coated on the surface of the sheet, which will effectively improve the dispersion effect of MXene / hybrid pentabromodiphenyl ether flame retardant in nylon, while giving play to the synergistic flame retardant advantages of MXene and pentabromodiphenyl ether. Therefore, under the same flame retardant index requirements, the amount of MXene / hybrid pentabromodiphenyl ether flame retardant in nylon injection molded parts can be reduced, thereby ensuring the plasticity and strength of the final injection molded parts.
[0076] like Fig. 9As shown in the figure, a dumbbell-shaped specimen (national standard type I specimen size) prepared by injection molding of nylon modified by adding 3% of graphite powder, siloxane / polyoxyethylene ether, aminopropyl polydimethylsiloxane / epichlorohydrin or graphite / polyoxyethylene ether compound antistatic agent was subjected to tensile test using a universal testing machine, with a tensile rate of 50mm / min and a test standard of GB / T1447-2005. The results showed that after adding 3% of graphite powder, the tensile strength of the nylon specimen decreased from about 135MPa to about 90MPa, while the tensile strength of the nylon composite material after adding 3% of siloxane / polyoxyethylene ether, aminopropyl polydimethylsiloxane / epichlorohydrin or graphite / polyoxyethylene ether compound antistatic agent remained at about 120MPa, 115MPa and 110MPa respectively. At the same time, the addition of graphite powder improves the tensile modulus of nylon composites. The tensile modulus of nylon modified by siloxane / polyoxyethylene ether, aminopropyl polydimethylsiloxane / epichlorohydrin or graphite / polyoxyethylene ether compound antistatic agent can be maintained at about 6GPa, which is only slightly lower than the tensile modulus of pure nylon. This shows that the addition of compound antistatic agent has less effect on the tensile strength of nylon than graphite powder, which is beneficial to ensure the mechanical properties of nylon injection molded parts.
[0077] From the above content, it can be known that the fully plasticized roller support for coal mine transportation of the present invention, the overall roller support adopts high specific strength plastic, the side plates and the middle section support adopt nylon, and the beam adopts self-extinguishing polyvinyl chloride. Compared with the existing steel structure roller support, the overall quality is reduced by 50~70%; the nylon blend is modified by an organic-inorganic flame retardant, and the flame retardant has the effects of conductivity, flame retardancy and reinforcement, and its flame retardancy level reaches V0; the organic-inorganic flame retardant is prepared by hydrothermal synthesis, which can significantly improve the intercalation and stripping effect of MXene, not only utilizing the dispersion of the flame retardant in the nylon matrix, but also significantly improving its flame retardant efficiency; the overall fully plasticized roller support adopts a nylon and polyvinyl chloride blend, and compared with the existing steel structure roller support, it has the advantages of noise reduction, corrosion resistance, flame retardancy and antistatic in the process of coal mine transportation.
Claims
1. A material preparation method for a fully plasticized roller support for coal mine transportation, characterized in that: Including the preparation of nylon blends and polyvinyl chloride blends; The nylon blend is prepared by melt blending nylon, an organic-inorganic hybrid flame retardant and an organic compound antistatic agent; the nylon is one of nylon 6, nylon 66 and nylon 610; the organic-inorganic hybrid flame retardant is one of MXene / pentabromodiphenyl ether, MXene / tris(2-chloropropyl) phosphate, and MXene / 2,2-bis(chloromethyl)cyclopropane; the organic compound antistatic agent is one of siloxane / polyoxyethylene ether, aminopropyl polydimethylsiloxane / epichlorohydrin, and graphite / polyoxyethylene ether; The components in the nylon blend include, by mass percentage, 85% to 100% nylon, 5% to 10% organic-inorganic hybrid flame retardant, and 3% to 5% organic compound antistatic agent, and the sum of the mass percentages of the above components is 100%; The polyvinyl chloride blend is prepared by melt blending polyvinyl chloride, a reinforcing agent, an antioxidant and an antistatic agent; The components in the polyvinyl chloride blend include, by mass percentage, 65% to 100% polyvinyl chloride, 15% to 25% reinforcing agent, 3% to 5% antioxidant, and 2% to 5% antistatic agent, and the sum of the mass percentages of the above components is 100%; The polyvinyl chloride is one of rigid polyvinyl chloride prepared by a suspension method or a rigid polyvinyl chloride prepared by a slurry method; the reinforcing agent is one of calcium carbonate, mica powder, and talc; the antioxidant is one of butylated hydroxyanisole, tert-butylhydroquinone, graphite / dilauryl thiodipropionate, and MXene / dilauryl thiodipropionate; the antistatic agent is one of graphite, copper powder, and graphite / polyoxyethylene ether.
2. The material preparation method of the fully plasticized roller support for coal mine transportation according to claim 1 is characterized in that: The organic-inorganic hybrid flame retardant is prepared by a hydrothermal method, the hydrothermal temperature is 130° C. to 180° C., and the hydrothermal reaction time is 24 h to 48 h.
3. The material preparation method of the fully plasticized roller support for coal mine transportation according to claim 1 is characterized in that: The melt blending temperature for preparing the nylon blend is 240°C to 280°C.
4. The material preparation method of the fully plasticized roller support for coal mine transportation according to claim 1 is characterized in that: The melt blending temperature for preparing the polyvinyl chloride blend is 180°C to 220°C.
5. A fully plasticized roller support for coal mine transportation, prepared by the material preparation method of the fully plasticized roller support for coal mine transportation according to any one of claims 1 to 4, the fully plasticized roller support for coal mine transportation comprising a beam (1-3), side plates (1-1) are respectively arranged at both ends of the beam (1-3), a middle section support (1-2) is arranged on the beam (1-3), the middle section support (1-2) runs through the beam (1-3), and the middle section support (1-2) and the beam (1-3) are interference fit, characterized in that: The side panels (1-1) and the middle bracket (1-2) are both made of nylon blend by injection molding, and the beam (1-3) is made of polyvinyl chloride blend by extrusion; The nylon blend of the side plate (1-1) and the middle bracket (1-2) is dried at 120°C to 150°C for 4h to 8h before injection molding, and then injection molded at an injection molding pressure of 300MPa to 500MPa and an injection molding temperature of 250°C to 280°C. After injection molding, the pressure is maintained for a holding time of 30s to 60s. The beam (1-3) is extruded by an extruder and water-cooled after extrusion. The extrusion temperature is 190° C. to 230° C., the extruder speed is 60 rpm to 120 rpm, and the water-cooling time is 30 s to 90 s.