A composite coating sprayed on the surface of carbon fiber material and preparation method thereof

By spraying aluminum enamel, NiCr and Cr2O3 coatings on the surface of carbon fiber materials, the problem of insufficient wear resistance and hardness of carbon fiber materials is solved, the impact resistance and wear resistance are improved, and the cost is reduced. It is suitable for carbon fiber rollers application.

CN118563322BActive Publication Date: 2024-11-19CHINA MACHINE KAIBO SURFACE TECHNOLOGY (JIANGSU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411045790.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The wear resistance and hardness of the composite coating on the surface of existing carbon fiber materials have not yet reached a satisfactory level, making it difficult to maintain performance in high temperature and corrosion environments, and is costly.

Method used

The surface of the carbon fiber material is sprayed with aluminum enamel powder slurry, NiCr powder and Cr2O3 powder in turn to form an aluminum enamel coating, NiCr coating and Cr2O3 coating of specific thicknesses to improve the material's oxidation resistance, high temperature resistance and wear resistance.

Benefits of technology

It significantly improves the impact resistance and wear resistance of carbon fiber materials, reduces the cost of parts, and is suitable as a replacement for steel rollers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563322B_ABST
    Figure CN118563322B_ABST
Patent Text Reader

Abstract

The present invention provides a composite coating sprayed on the surface of a carbon fiber material and a preparation method thereof, and relates to the technical field of material plating. The preparation method sequentially sprays aluminum enamel powder slurry, NiCr powder and Cr2O3 powder on the surface of the carbon fiber material to sequentially form coatings of corresponding materials, thereby greatly improving the impact resistance and wear resistance of the carbon fiber material, and is suitable for large-scale promotion and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material plating, and in particular to a composite coating sprayed on the surface of a carbon fiber material and a preparation method thereof. Background Art

[0002] Rollers, also known as rollers, are cylindrical parts, divided into driving rollers and driven rollers. They are widely used in various transmission and conveying systems such as rotary screen printing machines, digital printers, mining conveying equipment, papermaking and packaging machinery. Rollers in the traditional roller industry are generally made of steel, which has disadvantages such as large mass and large inertia. Due to the lack of wear resistance on the roller surface, long-term use is very likely to damage the roller surface and generate friction noise.

[0003] In the prior art, a lightweight roller is used, the matrix of which is made of carbon fiber. The carbon fiber has a low density and light weight, which is equivalent to one-fourth of the density of steel, and can effectively reduce weight. But relatively speaking, carbon fiber is more brittle and has poor impact resistance. Although it has high strength and rigidity, carbon fiber materials are expensive and difficult to repair, and have poor wear resistance. It is easily broken by external force and impact. It is easy to produce colloid cracking. Nowadays, the common method is to spray a wear-resistant and high-hardness coating on the surface of carbon fiber through a thermal spraying process. It is equivalent to putting a layer of armor on the surface of carbon fiber, which can effectively improve the impact resistance and wear resistance of carbon fiber, and can replace steel rollers and other parts, greatly reducing costs.

[0004] CN112871608A discloses a method for preparing a carbon fiber composite material coating and a carbon fiber composite device, the method comprising the following steps: first, surface treatment of a carbon fiber composite material substrate, cleaning and polishing the surface layer of the carbon fiber composite material substrate; second, applying putty, applying putty on the surface layer of the surface-treated carbon fiber composite material substrate to form a putty layer; third, spraying a mid-coat paint, spraying a mid-coat paint on the surface layer of the putty layer to form a mid-coat paint layer; finally, spraying a topcoat, spraying a topcoat on the surface layer of the mid-coat paint layer to form a topcoat paint layer. The preparation method optimizes the process manufacturing process of preparing a carbon fiber composite material coating, shortens the processing cycle, and reduces the processing cost.

[0005] CN117210781A discloses a method for plasma spraying ZrO on the surface of carbon fiber. 2 Coating method, including preparation of thermal spray powder, preparation of carbon fiber material, sandblasting pretreatment of carbon fiber material, filling of thermal spray powder, NiCrAlY primer thermal spray, ZrO 2 The surface layer is thermally sprayed and polished. The coating made by this method has good high temperature resistance and corrosion resistance, which can meet the service requirements of carbon fiber materials in high temperature and corrosive environments.

[0006] CN117626639A discloses a method for preparing a carbon fiber composite coating and a carbon fiber composite material. The preparation method comprises coating a transition layer on the surface of the carbon fiber; coating a polysilazane layer on the transition layer; and subjecting the carbon fiber coated with the polysilazane layer to high-temperature cracking under preset conditions to obtain a carbon fiber composite coating comprising a ceramic outer layer; wherein the transition layer is configured to prevent cracks in the ceramic outer layer from extending toward the surface of the carbon fiber.

[0007] However, the wear resistance and hardness of the composite coating on the surface of the above-mentioned carbon fiber material need to be further improved. Summary of the invention

[0008] In view of the problems existing in the prior art, the present invention provides a composite coating sprayed on the surface of a carbon fiber material and a preparation method thereof, wherein aluminum enamel powder slurry, NiCr powder and Cr are sprayed on the surface of the carbon fiber material in sequence. 2 O 3 Powder is added to obtain a composite coating, which not only ensures that the carbon fiber material does not deform, but also improves the hardness and wear resistance of the carbon fiber material, and is suitable for large-scale promotion and application.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a method for preparing a composite coating sprayed on the surface of a carbon fiber material, the preparation method comprising the following steps:

[0011] (1) Spraying aluminum enamel powder slurry on the surface of the carbon fiber material to form an aluminum enamel coating with a thickness of 0.08~0.1mm;

[0012] (2) plasma spraying NiCr powder on the aluminum enamel coating to form a NiCr coating with a thickness of 0.08-0.1 mm;

[0013] (3) Plasma spraying Cr on the NiCr coating 2 O 3 Powder, forming a Cr film with a thickness of 0.15~0.2mm 2 O 3 coating.

[0014] The composite coating sprayed on the surface of the carbon fiber material described in the present invention first sprays aluminum enamel powder slurry on the surface of the carbon fiber material, and the formed aluminum enamel coating serves as a bonding layer or a primer layer, which can improve the bonding strength between the working layer and the workpiece. In addition, the aluminum enamel coating has better antioxidant ability, corrosion resistance and high temperature resistance than the base material, plays a shielding role between the working coating and the base, and can minimize the degree of oxidation or corrosion of the base caused by the inherent pores of the thermal spray coating. The present invention sprays aluminum enamel powder slurry on the surface of the carbon fiber material, which does not generate high temperature and can effectively prevent the base carbon fiber material from melting and deforming due to high temperature.

[0015] Furthermore, the thermal expansion coefficient of the aluminum enamel coating of the present invention is between that of the base carbon fiber material and the intermediate NiCr coating, and it has sufficient toughness under mechanical and thermal loads, and can "buffer" the stress generated by the different thermal expansion coefficients of the base carbon fiber material and the intermediate NiCr coating, thereby avoiding deformation of the carbon fiber. The NiCr coating acts as a bonding agent as an intermediate layer and has excellent high-temperature oxidation resistance. Finally, the Cr coating is sprayed by plasma spraying. 2 O 3 Powder forming Cr 2 O 3 coating, the Cr 2 O 3 The coating is a ceramic coating with the characteristics of high thermal conductivity, low friction coefficient, high hardness and excellent wear resistance, reducing friction damage.

[0016] The aluminum enamel coating described in the present invention has a thickness of 0.08-0.1 mm as a base layer, and the NiCr coating has a thickness of 0.08-0.1 mm as an intermediate layer. Both of them have a relatively thin thickness, which effectively prevents the carbon fiber from being deformed by oxidation reaction due to high temperature. When the thickness of the aluminum enamel coating and the NiCr coating is relatively thin, they cannot well isolate the high temperature of plasma spraying, which will cause the carbon fiber to deform. When the thickness of the aluminum enamel coating and the NiCr coating is relatively thick, the preparation cost of the composite coating on the surface of the carbon fiber material will increase, and the economic benefit will be poor. Cr 2 O 3 The coating thickness is 0.15~0.2mm. As a surface layer, this thicker surface layer can significantly improve the wear resistance of carbon fiber materials. 2 O 3 The coating thickness is thin, the wear resistance of carbon fiber material is poor, the service life is reduced, and frequent replacement is required; when Cr 2 O 3 The thicker the coating is, the higher the preparation cost of the composite coating on the surface of the carbon fiber material will be, and the poorer the economic benefits will be. 2 O 3 If the coating is too thick, the coating bonding strength will be reduced, and there is a risk of coating peeling during use.

[0017] The thickness of the aluminum enamel coating of the present invention is 0.08-0.1 mm, for example, it can be 0.08 mm, 0.085 mm, 0.088 mm, 0.09 mm, 0.095 mm, 0.098 mm or 0.1 mm, etc., but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable;

[0018] The thickness of the NiCr coating is 0.08-0.1 mm, for example, it can be 0.08 mm, 0.085 mm, 0.088 mm, 0.09 mm, 0.095 mm, 0.098 mm or 0.1 mm, etc., but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable;

[0019] Cr 2 O 3 The thickness of the coating is 0.15 to 0.2 mm, for example, it can be 0.15 mm, 0.16 mm, 0.17 mm, 0.175 mm, 0.18 mm, 0.19 mm or 0.2 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the carbon fiber material in step (1) is subjected to ultrasonic cleaning and sandblasting in sequence before being sprayed with aluminum enamel powder. The ultrasonic cleaning is used to remove oil stains and contamination on the surface of the carbon fiber; the sandblasting is used to increase the surface roughness of the carbon fiber material, improve the surface adhesion, make the aluminum enamel coating more easily adhere to its surface, and increase its durability.

[0021] Preferably, the temperature of the ultrasonic cleaning treatment is 55-65°C, for example, 55°C, 58°C, 60°C, 62°C, 64°C or 65°C, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0022] The cleaning time is ≥ 0.5 h, for example, it can be 0.5 h, 0.6 h, 0.8 h, 0.9 h, 1 h or 1.5 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the ultrasonic cleaning is followed by drying.

[0024] Preferably, the drying temperature is 90-110° C., for example, 90° C., 95° C., 98° C., 100° C., 105° C. or 110° C., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0025] The time is ≥ 1.5 h, for example, it can be 1.5 h, 1.6 h, 1.8 h, 1.9 h, 2 h or 2.5 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the sandblasting process uses white corundum with a particle size of 60 mesh.

[0027] Preferably, the line speed of the sandblasting process is 10 m / min, and the stepping speed is 10 mm.

[0028] Preferably, the sandblasting distance is 180-200 mm, for example, 180 mm, 185 mm, 190 mm, 195 mm, 198 mm or 200 mm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, the pressure of the sandblasting treatment is 0.15 MPa. Under such a relatively small sandblasting pressure, the damage to the surface of the carbon fiber can be effectively reduced, and the surface roughening effect can be achieved.

[0030] Preferably, the roughness Ra of the carbon fiber material after sandblasting is 2~4μm, for example, it can be 2μm, 2.2μm, 2.5μm, 3μm, 3.5μm or 4μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the raw materials constituting the aluminum enamel powder slurry in step (1) include aluminum powder, enamel powder and a binder.

[0032] Preferably, the purity of the aluminum powder is ≥99.5%, for example, it can be 99.5%, 99.6%, 99.7%, 99.8%, 99.85% or 99.9%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the particle size of the aluminum powder is 15-45 μm, for example, 15 μm, 18 μm, 20 μm, 30 μm, 40 μm or 45 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, in terms of mass percentage, the raw materials of the enamel powder include: 50% to 51% SiO 2 , for example, it can be 50%, 50.2%, 50.4%, 50.6%, 50.8% or 51%, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] 8.5%~9.5%Al 2O 3 For example, it can be 8.5%, 8.8%, 9%, 9.1%, 9.3% or 9.5%, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] 10.5%~11.5%B 2 O 3 For example, it can be 10.5%, 10.8%, 11%, 11.2%, 11.4% or 11.5%, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] 9%~10%Na 2 O, for example, can be 9%, 9.2%, 9.4%, 9.5%, 9.8% or 10%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] 10.5%~11.5%CaO, for example, can be 10.5%, 10.8%, 11%, 11.2%, 11.4% or 11.5%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] and 9.5% to 10.5% MgO, for example, 9.5%, 9.7%, 10%, 10.2%, 10.4% or 10.5%, etc., but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] The SiO 2 The main function is to enhance the hardness and corrosion resistance of the enamel surface, making the enamel coating more durable and practical. 2 It has a certain polarity and can interact with the solvent to form adhesion, thereby increasing the viscosity and rheology of the slurry. 2 It can significantly improve the fluidity and uniformity of the slurry, making the coating smoother and fuller. 2 O 3 Used as an additive to improve the hardness, wear resistance, heat resistance and corrosion resistance of the coating.

[0041] Preferably, in terms of mass percentage, the composition of the binder includes: 3% to 4% CrO 3 , for example, it can be 3%, 3.3%, 3.5%, 3.7%, 3.9% or 4%, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] 3%~4%MgO, for example, can be 3%, 3.3%, 3.5%, 3.7%, 3.9% or 4%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] 8%~9%H 3 PO 4 And, for example, it can be 8%, 8.1%, 8.3%, 8.5%, 8.8% or 9%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] 84%~85%H 2 O, for example, it can be 84%, 84.2%, 84.5%, 84.6%, 84.8% or 85%, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] The composition of the binder of the present invention includes CrO 3 It can enhance the bonding strength of the adhesive, making it more stable and strong. This is because chromium can form a dense oxide layer with metal materials, so that the particles at the metal interface are more closely bonded to each other. MgO can increase the viscosity and consistency of the adhesive, making the adhesive easier to bond and apply, and has good tensile strength and heat resistance.

[0046] Preferably, the aluminum powder and enamel powder in the aluminum enamel powder slurry are mixed in a mass ratio of 4:1 to form a mixed powder, so that the aluminum enamel coating after curing has better bonding strength and higher permeability.

[0047] Preferably, the mass concentration of the binder in the aluminum enamel powder slurry is 15% to 16%, for example, it can be 15%, 15.2%, 15.5%, 15.7%, 15.9% or 16%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] Preferably, the mass ratio of the mixed powder to the binder in the aluminum enamel powder slurry is 1:1. When the mixed powder content is too high, the prepared slurry will be too thick and difficult to spray evenly, affecting the surface quality and uniformity of the coating; when the mixed powder content is too low, the prepared slurry will easily flow, reducing the coating concentration.

[0049] Preferably, the process parameters for spraying the aluminum enamel powder slurry in step (1) include:

[0050] The spraying line speed is 10 mm / min, the spraying step is 10 mm, and the spraying distance is 130-150 mm, for example, it can be 130 mm, 135 mm, 140 mm, 145 mm, 148 mm or 150 mm, etc., but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0051] The spraying pressure is 0.3~0.4MPa, for example, it can be 0.3MPa, 0.31MPa, 0.33MPa, 0.35MPa, 0.37MPa or 0.4MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] The present invention preferably has a spraying line speed of 10 mm / min and a spraying step of 10 mm, so that when the aluminum enamel powder slurry is sprayed by a robot, the thickness of the slurry is uniform.

[0053] Preferably, the process of spraying the aluminum enamel powder slurry includes repeated spraying and drying processes in sequence, and the number of repetitions can be set according to actual conditions, and finally the required thickness of the aluminum enamel coating is achieved.

[0054] Preferably, the temperature of the drying treatment is 90-110°C, for example, it can be 90°C, 95°C, 98°C, 100°C, 105°C or 110°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] Preferably, the drying treatment time is ≥ 1 h, for example, it can be 1 h, 1.2 h, 1.5 h, 1.8 h, 2 h or 2.5 h, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0056] Preferably, a curing treatment is performed after the last drying treatment at a temperature of 280-310°C, for example, 280°C, 285°C, 288°C, 290°C, 300°C or 310°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] The time is ≥ 1 h, for example, it can be 1 h, 1.2 h, 1.5 h, 1.8 h, 2 h or 2.5 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0058] Preferably, the NiCr powder in step (2) comprises Ni 20 Cr powder.

[0059] Preferably, the particle size of the Ni powder is 15-45 μm, for example, 15 μm, 18 μm, 20 μm, 30 μm, 40 μm or 45 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0060] Preferably, the particle size of the Cr powder is 15-45 μm, for example, 15 μm, 18 μm, 20 μm, 30 μm, 40 μm or 45 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] Preferably, the process parameters of the plasma spraying NiCr powder include:

[0062] The argon gas flow rate is 49-51 NLPM, for example, it can be 49 NLPM, 49.3 NLPM, 49.5 NLPM, 50 NLPM or 51 NLPM, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0063] The hydrogen flow rate is 9-11 NLPM, for example, it can be 9 NLPM, 9.5 NLPM, 10 NLPM, 10.5 NLPM or 11 NLPM, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0064] The voltage is 65-70V, for example, it can be 65V, 66V, 67V, 68V, 69V or 70V, but is not limited to the listed values. Other values ​​not listed within the range are also applicable.

[0065] The current 550~600A can be, for example, 550A, 560A, 570A, 580A or 600A, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0066] The powder feeding rate is 48-50 g / min, for example, it can be 48 g / min, 48.5 g / min, 49 g / min, 49.5 g / min, 49.8 g / min or 50 g / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0067] The spraying distance is 115-120 mm, for example, it can be 115 mm, 116 mm, 117 mm, 118 mm, 119 mm or 120 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0068] The spraying angle is 90°, and the line speed is 130-140 m / min, for example, it can be 130 m / min, 133 m / min, 135 m / min, 138 m / min, 139 m / min or 140 m / min, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0069] The stepping is 3.5 to 4.0 mm, for example, it can be 3.5 mm, 3.6 mm, 3.7 mm, 3.8 mm, 3.9 mm or 4.0 mm, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0070] The temperature is ≤200°C, for example, it can be 200°C, 190°C, 180°C, 170°C, 150°C, 130°C or 100°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0071] The present invention preferably sets the temperature of the plasma sprayed NiCr powder to ≤ 200°C because, although the temperature resistance of carbon fiber is relatively high, its performance will also change with the change of temperature. In a high temperature environment, carbon fiber may oxidize, pyrolyze, crack, etc., resulting in a decrease in its performance. When the temperature of carbon fiber exceeds 300°C, its strength begins to decrease significantly, and it is prone to oxidation reaction at high temperature, reducing its durability. Therefore, the substrate temperature needs to be controlled during thermal spraying.

[0072] The present invention preferably sets the linear velocity of the plasma sprayed NiCr powder to 130-140 m / min. During the spraying process, the temperature of the workpiece can be controlled by adjusting the moving speed of the spray gun. With such a high linear velocity, the spray gun moves faster on the surface of the workpiece and sprays multiple times according to the required coating thickness. In this way, the heat sprayed by the spray gun will be evenly distributed on the entire workpiece, and local hot spots will not be generated.

[0073] The present invention preferably sets the stepping of the plasma sprayed NiCr powder to 3.5-4.0 mm. Too small a stepping will result in a longer spraying time and the workpiece will be easily overheated; too large a stepping will result in uneven coating coverage.

[0074] Preferably, in step (3), Cr 2 O 3 The purity of the powder is ≥99.5%, for example, it can be 99.5%, 99.6%, 99.7%, 99.8%, 99.85% or 99.9%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0075] Preferably, the Cr 2 O 3The particle size of the powder is 15-45 μm, for example, it can be 15 μm, 18 μm, 20 μm, 30 μm, 40 μm or 45 μm, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0076] Preferably, the plasma sprayed Cr 2 O 3 The process parameters of the powder include:

[0077] The argon gas flow rate is 49-51 NLPM, for example, it can be 49 NLPM, 49.3 NLPM, 49.5 NLPM, 50 NLPM or 51 NLPM, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0078] The hydrogen flow rate is 9-11 NLPM, for example, it can be 9 NLPM, 9.5 NLPM, 10 NLPM, 10.5 NLPM or 11 NLPM, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0079] The voltage is 70-75V, for example, it can be 70V, 71V, 72V, 73V, 74V or 75V, but is not limited to the listed values. Other values ​​not listed within the range are also applicable.

[0080] The current 550~600A can be, for example, 550A, 560A, 570A, 580A or 600A, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0081] The powder feeding rate is 40-42 g / min, for example, it can be 40 g / min, 40.5 g / min, 41 g / min, 41.5 g / min, 41.8 g / min or 42 g / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0082] The spraying distance is 105-110 mm, for example, it can be 105 mm, 106 mm, 107 mm, 108 mm, 109 mm or 110 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0083] The spraying angle is 90°, and the line speed is 160~170m / min, for example, it can be 160m / min, 162m / min, 164m / min, 166m / min, 168m / min or 170m / min, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0084] The stepping is 6.0-6.5 mm, for example, it can be 6.0 mm, 6.1 mm, 6.2 mm, 6.3 mm, 6.4 mm or 6.5 mm, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0085] Preferably, the preparation method further comprises: 2 O 3 The coating is subjected to rough grinding and fine grinding in sequence.

[0086] Preferably, the process parameters of the rough grinding include: abrasive particle size of 125~150 mesh, for example, it can be 125 mesh, 128 mesh, 130 mesh, 140 mesh or 150 mesh, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0087] The grinding wheel speed is 25-30 m / s, for example, it can be 25 m / s, 26 m / s, 27 m / s, 28 m / s or 30 m / s, but it is not limited to the listed values, and other values ​​not listed in the range are also applicable. The workpiece speed is 0.3 m / s.

[0088] The moving speed is 20-30 cm / s, for example, it can be 20 cm / s, 22 cm / s, 24 cm / s, 28 cm / s or 30 cm / s, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0089] The longitudinal grinding amount is 30-50 μm, for example, it can be 30 μm, 35 μm, 40 μm, 43 μm, 45 μm or 50 μm, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0090] Preferably, the process parameters of the fine grinding include: abrasive particle size 380~400 mesh, for example, it can be 380 mesh, 385 mesh, 390 mesh, 395 mesh or 400 mesh, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0091] The grinding wheel speed is 25-30 m / s, for example, it can be 25 m / s, 26 m / s, 27 m / s, 28 m / s or 30 m / s, but it is not limited to the listed values, and other values ​​not listed in the range are also applicable. The workpiece speed is 0.5 m / s.

[0092] The moving speed is 5 to 10 cm / s, for example, it can be 5 cm / s, 6 cm / s, 7 cm / s, 8 cm / s or 10 cm / s, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0093] The longitudinal grinding amount is 5 to 10 μm, for example, it can be 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0094] Preferably, the Cr 2 O 3 The roughness of the coating Ra≤0.8μm, for example, it can be 0.8μm, 0.75μm, 0.7μm, 0.6μm, 0.5μm or 0.3μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0095] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0096] (1) After ultrasonic cleaning and sandblasting of the carbon fiber material, aluminum enamel powder slurry is sprayed on the surface of the carbon fiber material to form an aluminum enamel coating with a thickness of 0.08-0.1 mm;

[0097] The roughness Ra of the carbon fiber material after sandblasting is 2-4 μm;

[0098] The raw materials of the aluminum enamel powder slurry include aluminum powder, enamel powder and a binder; the purity of the aluminum powder is ≥99.5%; the particle size of the aluminum powder is 15-45 μm;

[0099] In terms of mass percentage, the raw materials of the enamel powder include: 50% to 51% SiO 2 、8.5%~9.5%Al 2 O 3 10.5%~11.5%B 2 O 3 、9%~10%Na 2 O, 10.5%~11.5%CaO and 9.5%~10.5%MgO;

[0100] In terms of mass percentage, the composition of the binder includes: 3% to 4% CrO 3 、3%~4%MgO、8%~9%H 3 PO 4 and 84%~85%H 2 O;

[0101] The aluminum powder and enamel powder in the aluminum enamel powder slurry are formed into a mixed powder in a mass ratio of 4:1; the mass concentration of the binder in the aluminum enamel powder slurry is 15% to 16%; the mass ratio of the mixed powder to the binder in the aluminum enamel powder slurry is 1:1;

[0102] The process parameters of spraying aluminum enamel powder slurry include:

[0103] Spraying line speed 10m / min, spraying step 10mm, spraying distance 130~150mm, spraying pressure 0.3~0.4MPa;

[0104] The process of spraying the aluminum enamel powder slurry includes spraying and drying treatments which are repeated in sequence; the temperature of the drying treatment is 100±10°C; the time of the drying treatment is ≥1h; after the last drying treatment, a curing treatment is performed at a temperature of 280~310°C for a time of ≥1h;

[0105] (2) plasma spraying NiCr powder on the aluminum enamel coating to form a NiCr coating with a thickness of 0.08-0.1 mm;

[0106] The NiCr powder includes Ni 20 Cr powder; the particle size of the Ni powder is 15~45μm; the particle size of the Cr powder is 15~45μm;

[0107] The process parameters of the plasma spraying NiCr powder include: argon flow rate 49~51NLPM, hydrogen flow rate 9~11NLPM, voltage 65~70V, current 550~600A, powder feeding rate 48~50g / min, spraying distance 115~120mm, spraying angle 90°, line speed 130~140m / min, step 3.5~4.0mm, temperature ≤200°C;

[0108] (3) Plasma spraying Cr on the NiCr coating 2 O 3 Powder, forming a Cr film with a thickness of 0.15~0.2mm 2 O 3 coating;

[0109] The Cr 2 O 3 The purity of the powder is ≥99.5%; the Cr 2 O 3 The particle size of the powder is 15~45μm;

[0110] The plasma sprayed Cr 2 O 3 The process parameters of the powder include: argon flow rate 49~51NLPM, hydrogen flow rate 9~11NLPM, voltage 70~75V, current 550~600A, powder feeding rate 40~42g / min, spraying distance 105~110mm, spraying angle 90°, line speed 160~170m / min, stepping 6.0~6.5mm;

[0111] The preparation method further comprises the step of 2 O 3The coating is subjected to rough grinding and fine grinding in sequence.

[0112] In a second aspect, the present invention further provides a composite coating sprayed on the surface of a carbon fiber material, wherein the composite coating is prepared by the method for preparing a composite coating sprayed on the surface of a carbon fiber material according to the first aspect.

[0113] The composite coating sprayed on the surface of the carbon fiber material of the present invention comprises aluminum enamel coating, NiCr coating and Cr 2 O 3 The coating can effectively improve the impact resistance and wear resistance of carbon fiber materials and significantly reduce the cost of parts made of carbon fiber materials.

[0114] Compared with the prior art, the present invention has at least the following beneficial effects:

[0115] The preparation method of the composite coating sprayed on the surface of the carbon fiber material provided by the present invention is simple to operate, and aluminum enamel powder slurry, NiCr powder and Cr are sprayed on the surface of the carbon fiber material in sequence. 2 O 3 The powder is then coated with corresponding materials of a specific thickness, which greatly improves the impact resistance and wear resistance of the carbon fiber material. It is suitable as a carbon fiber roller to replace the existing steel roller. BRIEF DESCRIPTION OF THE DRAWINGS

[0116] Figure 1 It is a schematic diagram of the composite coating sprayed on the surface of the carbon fiber material provided by the present invention.

[0117] In the figure: 1-carbon fiber material; 2-aluminum enamel coating; 3-NiCr coating; 4-Cr 2 O 3 coating. DETAILED DESCRIPTION

[0118] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0119] The present invention provides a method for preparing a composite coating sprayed on the surface of a carbon fiber material, the preparation method comprising the following steps:

[0120] (1) Spraying aluminum enamel powder slurry on the surface of the carbon fiber material to form an aluminum enamel coating with a thickness of 0.08~0.1mm;

[0121] (2) plasma spraying NiCr powder on the aluminum enamel coating to form a NiCr coating with a thickness of 0.08-0.1 mm;

[0122] (3) Plasma spraying Cr on the NiCr coating 2 O 3Powder, forming a Cr film with a thickness of 0.15~0.2mm 2 O 3 coating.

[0123] The schematic diagram of the composite coating on the surface of the carbon fiber material obtained by the preparation method of the present invention is as follows Figure 1 As shown, from inside to outside, there are carbon fiber material 1, aluminum enamel coating 2, NiCr coating 3 and Cr 2 O 3 Coating 4.

[0124] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0125] Example 1

[0126] This embodiment provides a method for preparing a composite coating sprayed on the surface of a carbon fiber material, the preparation method comprising the following steps:

[0127] (1) After ultrasonic cleaning and sandblasting of the carbon fiber material, aluminum enamel powder slurry is sprayed on the surface of the carbon fiber material to form an aluminum enamel coating with a thickness of 0.09 mm;

[0128] The temperature of the ultrasonic cleaning treatment is 62°C, and the cleaning time is 0.9h; the ultrasonic cleaning treatment is followed by drying; the drying temperature is 100°C, and the time is 1.8h; the sandblasting treatment uses white corundum with a particle size of 60 mesh; the line speed of the sandblasting treatment is 10m / min, and the step is 10mm; the distance of the sandblasting treatment is 195mm; the pressure of the sandblasting treatment is 0.15MPa; the roughness Ra of the carbon fiber material after the sandblasting treatment is 2.5μm;

[0129] The raw materials of the aluminum enamel powder slurry include aluminum powder, enamel powder and a binder; the purity of the aluminum powder is 99.7%; the particle size of the aluminum powder is 30 μm;

[0130] In terms of mass percentage, the raw materials of the enamel powder include: 50.4% SiO 2 、8.5%Al 2 O 3 10.8%B 2 O 3 、9.4%Na 2 O, 11.2% CaO and 9.7% MgO;

[0131] In terms of mass percentage, the composition of the binder includes: 3% CrO 3 、4%MgO、8.5%H 3 PO4 and 84.5% H 2 O;

[0132] The aluminum powder and enamel powder in the aluminum enamel powder slurry are formed into a mixed powder in a mass ratio of 4:1; the mass concentration of the binder in the aluminum enamel powder slurry is 15.5%; the mass ratio of the mixed powder to the binder in the aluminum enamel powder slurry is 1:1;

[0133] The process parameters of spraying aluminum enamel powder slurry include:

[0134] Spraying line speed 10mm / min, spraying step 10mm, spraying distance 135mm, spraying pressure 0.33MPa;

[0135] The process of spraying the aluminum enamel powder slurry includes spraying and drying processes which are repeated in sequence for 2 times; the temperature of the drying process is 98° C.; the time of the drying process is 2 hours; after the last drying process, a curing process is performed at a temperature of 288° C. for 1 hour;

[0136] (2) plasma spraying NiCr powder on the aluminum enamel coating to form a NiCr coating with a thickness of 0.088 mm;

[0137] The NiCr powder includes Ni 20 Cr powder; the particle size of the Ni powder is 40 μm; the particle size of the Cr powder is 30 μm;

[0138] The process parameters of the plasma spraying of NiCr powder include: argon flow rate 49.5NLPM, hydrogen flow rate 9.5NLPM, voltage 67V, current 580A, powder feeding rate 49g / min, spraying distance 118mm, spraying angle 90°, line speed 135m / min, stepping 3.7mm, temperature ≤200°C;

[0139] (3) Plasma spraying Cr on the NiCr coating 2 O 3 powder, forming a 0.17mm thick Cr 2 O 3 coating;

[0140] The Cr 2 O 3 The purity of the powder is 99.5%; the Cr 2 O 3 The particle size of the powder is 20 μm;

[0141] The plasma sprayed Cr 2 O 3The process parameters of the powder include: argon flow rate 50NLPM, hydrogen flow rate 10.5NLPM, voltage 73V, current 560A, powder feeding rate 41.5g / min, spraying distance 107mm, spraying angle 90°, line speed 166m / min, stepping 6.3mm;

[0142] The preparation method further comprises the step of 2 O 3 The coating is subjected to rough grinding and fine grinding in sequence; the process parameters of the rough grinding include: abrasive grain size 140 mesh, grinding wheel speed 27m / s; workpiece speed 0.3m / s; moving speed 22cm / s, longitudinal grinding amount 35μm;

[0143] The process parameters of the fine grinding include: abrasive grain size 390 mesh, grinding wheel speed 27m / s; workpiece speed 0.5m / s, moving speed 8cm / s, longitudinal grinding amount 7μm; Cr after fine grinding 2 O 3 The roughness Ra of the coating is 0.8 μm.

[0144] Example 2

[0145] This embodiment provides a method for preparing a composite coating sprayed on the surface of a carbon fiber material, the preparation method comprising the following steps:

[0146] (1) After ultrasonic cleaning and sandblasting of the carbon fiber material, aluminum enamel powder slurry is sprayed on the surface of the carbon fiber material to form an aluminum enamel coating with a thickness of 0.08 mm;

[0147] The temperature of the ultrasonic cleaning treatment is 65°C, and the cleaning time is 0.9h; the ultrasonic cleaning treatment is followed by drying; the drying temperature is 110°C, and the time is 2h; the sandblasting treatment uses white corundum with a particle size of 60 mesh; the line speed of the sandblasting treatment is 10m / min, and the step is 10mm; the distance of the sandblasting treatment is 200mm; the pressure of the sandblasting treatment is 0.15MPa; the roughness Ra of the carbon fiber material after the sandblasting treatment is 4μm;

[0148] The raw materials of the aluminum enamel powder slurry include aluminum powder, enamel powder and a binder; the purity of the aluminum powder is 99.8%; the particle size of the aluminum powder is 15 μm;

[0149] In terms of mass percentage, the raw materials of the enamel powder include: 50% SiO 2 、9.5%Al 2 O 3 11.5%B 2 O 3 、9%Na 2O, 10.5% CaO and 9.5% MgO;

[0150] In terms of mass percentage, the composition of the binder includes: 4% CrO 3 、3%MgO、9%H 3 PO 4 and 84% H 2 O;

[0151] The aluminum powder and enamel powder in the aluminum enamel powder slurry are formed into a mixed powder in a mass ratio of 4:1; the mass concentration of the binder in the aluminum enamel powder slurry is 15%; the mass ratio of the mixed powder to the binder in the aluminum enamel powder slurry is 1:1;

[0152] The process parameters of spraying aluminum enamel powder slurry include:

[0153] Spraying line speed 10mm / min, spraying step 10mm, spraying distance 130mm, spraying pressure 0.4MPa;

[0154] The process of spraying the aluminum enamel powder slurry includes spraying and drying treatments which are repeated three times in sequence; the temperature of the drying treatment is 110° C.; the time of the drying treatment is 1 hour; after the last drying treatment, a curing treatment is performed at a temperature of 280° C. for 1 hour;

[0155] (2) plasma spraying NiCr powder on the aluminum enamel coating to form a NiCr coating with a thickness of 0.1 mm;

[0156] The NiCr powder includes Ni 20 Cr powder; the particle size of the Ni powder is 45 μm; the particle size of the Cr powder is 45 μm;

[0157] The process parameters of the plasma spraying of NiCr powder include: argon flow rate 51NLPM, hydrogen flow rate 11NLPM, voltage 65V, current 550A, powder feeding rate 50g / min, spraying distance 120mm, spraying angle 90°, line speed 140m / min, stepping 4.0mm, and temperature 200°C;

[0158] (3) Plasma spraying Cr on the NiCr coating 2 O 3 Powder, forming a 0.2mm thick Cr 2 O 3 coating;

[0159] The Cr 2 O 3 The purity of the powder is 99.5%; the Cr 2 O 3 The particle size of the powder is 15 μm;

[0160] The plasma sprayed Cr 2 O 3 The process parameters of the powder include: argon flow rate 49NLPM, hydrogen flow rate 9NLPM, voltage 75V, current 600A, powder feeding rate 40g / min, spraying distance 110mm, spraying angle 90°, line speed 160m / min, stepping 6.5mm;

[0161] The preparation method further comprises the step of 2 O 3 The coating is subjected to rough grinding and fine grinding in sequence; the process parameters of the rough grinding include: abrasive grain size 150 mesh, grinding wheel speed 30m / s; workpiece speed 0.3m / s; moving speed 30cm / s, longitudinal grinding amount 50μm;

[0162] The process parameters of the fine grinding include: abrasive grain size 400 mesh, grinding wheel speed 25m / s; workpiece speed 0.5m / s, moving speed 10cm / s, longitudinal grinding amount 10μm; Cr after fine grinding 2 O 3 The roughness Ra of the coating is 0.8 μm.

[0163] Example 3

[0164] This embodiment provides a method for preparing a composite coating sprayed on the surface of a carbon fiber material, the preparation method comprising the following steps:

[0165] (1) After ultrasonic cleaning and sandblasting of the carbon fiber material, aluminum enamel powder slurry is sprayed on the surface of the carbon fiber material to form an aluminum enamel coating with a thickness of 0.1 mm;

[0166] The temperature of the ultrasonic cleaning treatment is 55°C, and the cleaning time is 0.5h; the ultrasonic cleaning treatment is followed by drying; the drying temperature is 90°C, and the time is 1.5h; the sandblasting treatment uses white corundum with a particle size of 60 mesh; the line speed of the sandblasting treatment is 10m / min, and the step is 10mm; the distance of the sandblasting treatment is 180mm; the pressure of the sandblasting treatment is 0.15MPa; the roughness Ra of the carbon fiber material after the sandblasting treatment is 2μm;

[0167] The raw materials of the aluminum enamel powder slurry include aluminum powder, enamel powder and a binder; the purity of the aluminum powder is 99.5%; the particle size of the aluminum powder is 45 μm;

[0168] In terms of mass percentage, the raw materials of the enamel powder include: 51% SiO 2 、8.5%Al 2 O 3 10.5%B2 O 3 、9%Na 2 O, 10.5% CaO and 10.5% MgO;

[0169] In terms of mass percentage, the composition of the binder includes: 3.5% CrO 3 、3.5%MgO、8%H 3 PO 4 and 85% H 2 O;

[0170] The aluminum powder and enamel powder in the aluminum enamel powder slurry are formed into a mixed powder in a mass ratio of 4:1; the mass concentration of the binder in the aluminum enamel powder slurry is 16%; the mass ratio of the mixed powder to the binder in the aluminum enamel powder slurry is 1:1;

[0171] The process parameters of spraying aluminum enamel powder slurry include:

[0172] Spraying line speed 10mm / min, spraying step 10mm, spraying distance 150mm, spraying pressure 0.3MPa;

[0173] The process of spraying the aluminum enamel powder slurry includes spraying and drying treatments which are repeated in sequence for 2 times; the temperature of the drying treatment is 90° C.; the time of the drying treatment is ≥ 1 hour; after the last drying treatment, a curing treatment is performed at a temperature of 310° C. for 1.8 hours;

[0174] (2) plasma spraying NiCr powder on the aluminum enamel coating to form a NiCr coating with a thickness of 0.08 mm;

[0175] The NiCr powder includes Ni 20 Cr powder; the particle size of the Ni powder is 15 μm; the particle size of the Cr powder is 15 μm;

[0176] The process parameters of the plasma spraying of NiCr powder include: argon flow rate 49NLPM, hydrogen flow rate 9NLPM, voltage 70V, current 600A, powder feeding rate 48g / min, spraying distance 115mm, spraying angle 90°, line speed 140m / min, stepping 3.5mm, and temperature 180°C;

[0177] (3) Plasma spraying Cr on the NiCr coating 2 O 3 Powder, forming a 0.15mm thick Cr 2 O 3 coating;

[0178] The Cr 2 O 3The purity of the powder is 99.6%; the Cr 2 O 3 The particle size of the powder is 45 μm;

[0179] The plasma sprayed Cr 2 O 3 The process parameters of the powder include: argon flow rate 51NLPM, hydrogen flow rate 11NLPM, voltage 70V, current 550A, powder feeding rate 42g / min, spraying distance 105mm, spraying angle 90°, line speed 170m / min, stepping 6.0mm;

[0180] The preparation method further comprises the step of 2 O 3 The coating is subjected to rough grinding and fine grinding in sequence; the process parameters of the rough grinding include: abrasive grain size 125 mesh, grinding wheel speed 25m / s; workpiece speed 0.3m / s; moving speed 20cm / s, longitudinal grinding amount 30μm;

[0181] The process parameters of the fine grinding include: abrasive grain size 380 mesh, grinding wheel speed 30m / s; workpiece speed 0.5m / s, moving speed 5cm / s, longitudinal grinding amount 5μm; Cr after fine grinding 2 O 3 The roughness Ra of the coating is 0.6 μm.

[0182] Example 4

[0183] This embodiment provides a method for preparing a composite coating sprayed on the surface of a carbon fiber material. The preparation method includes the following steps: (1) the composition of the aluminum enamel powder slurry; the aluminum enamel powder in the enamel powder is 2 O 3 Except that the mass percentage of is 7%, the rest is the same as that of Example 1.

[0184] Example 5

[0185] This embodiment provides a method for preparing a composite coating sprayed on the surface of a carbon fiber material. The preparation method includes the following steps: (1) the composition of the aluminum enamel powder slurry; the aluminum enamel powder in the enamel powder is 2 O 3 Except that the mass percentage of is 12%, the rest are the same as in Example 1.

[0186] Example 6

[0187] This embodiment provides a method for preparing a composite coating sprayed on the surface of a carbon fiber material. The preparation method is the same as that of Embodiment 1 except that the mass percentage of MgO in the raw material binder constituting the aluminum enamel powder slurry in step (1) is 1%.

[0188] Example 7

[0189] This embodiment provides a method for preparing a composite coating sprayed on the surface of a carbon fiber material. The preparation method is the same as that of Embodiment 1 except that the mass percentage of MgO in the constituent raw materials of the binder in step (1) is 6%.

[0190] Example 8

[0191] This embodiment provides a method for preparing a composite coating sprayed on the surface of a carbon fiber material. The preparation method is the same as that of Embodiment 1 except that the temperature of plasma spraying NiCr powder in step (2) is 250° C.

[0192] Comparative Example 1

[0193] The present comparative example provides a composite coating sprayed on the surface of a carbon fiber material and a preparation method thereof. The preparation method is the same as Example 1 except that the spraying of the aluminum enamel powder slurry in step (1) is replaced by a sandblasting roughening treatment, wherein the operating parameters of the sandblasting roughening treatment include sand particle model: 120 mesh white corundum, sandblasting pressure 0.1 MPa, and sandblasting distance 200 mm.

[0194] In this comparative example, the surface of the carbon fiber material after sandblasting and roughening is smoother than that of the aluminum enamel coating, which is not conducive to good mechanical interlocking of the NiCr coating.

[0195] Comparative Example 2

[0196] This comparative example provides a composite coating sprayed on the surface of a carbon fiber material and a preparation method thereof. The preparation method is the same as Example 1 except that step (1) of spraying the aluminum enamel powder slurry is omitted and step (2) is directly performed.

[0197] In this comparative example, since no aluminum enamel coating is formed, stress is generated due to the difference in thermal expansion coefficients between the carbon fiber material and the intermediate layer NiCr coating, and the carbon fiber material is deformed.

[0198] Comparative Example 3

[0199] This comparative example provides a composite coating sprayed on the surface of a carbon fiber material and a preparation method thereof. The preparation method is the same as Example 1 except that the thickness of the aluminum enamel coating in step (1) is 0.05 mm.

[0200] Comparative Example 4

[0201] This comparative example provides a composite coating sprayed on the surface of a carbon fiber material and a preparation method thereof. The preparation method is the same as Example 1 except that the thickness of the aluminum enamel coating in step (1) is 0.2 mm.

[0202] Comparative Example 5

[0203] This comparative example provides a composite coating sprayed on the surface of a carbon fiber material and a preparation method thereof. The preparation method includes the following steps: 2 O 3 Except that the thickness of the coating is 0.05 mm, the rest is the same as that of Example 1.

[0204] Comparative Example 6

[0205] This comparative example provides a composite coating sprayed on the surface of a carbon fiber material and a preparation method thereof. The preparation method includes the following steps: 2 O 3 Except that the thickness of the coating is 0.5 mm, the rest is the same as that of Example 1.

[0206] The hardness of the composite coatings obtained in the above embodiments and comparative examples was measured by a micro-Vickers hardness test method; the wear resistance of the composite coatings obtained in the above embodiments and comparative examples was measured by a reciprocating wear test method. The results are shown in Table 1.

[0207] From Table 1 we can see that:

[0208] (1) It can be seen from Examples 1 to 3 that the Vickers hardness of the composite coating obtained by the method for preparing the composite coating sprayed on the surface of the carbon fiber material provided by the present invention can reach above 1564, and the friction coefficient can reach below 0.24, which greatly improves the impact resistance and wear resistance of the carbon fiber material;

[0209] (2) Combining Examples 1 and 4-5, it can be seen that the enamel powder of the raw materials of the aluminum enamel powder slurry in Example 4 contains Al 2 O 3 The mass percentage of is low, which will lead to a significant reduction in the Vickers hardness of the obtained composite coating, which is 1308, and the friction coefficient is 0.38; Example 5 Composition of aluminum enamel powder slurry raw material enamel powder Al 2 O 3 The mass percentage of is high, the Vickers hardness of the obtained composite coating is improved and the wear resistance is improved, but the preparation cost of the composite coating on the surface of the carbon fiber material will be increased, and the economic benefit is poor;

[0210] (3) Combining Example 1 with Examples 6 and 7, it can be seen that the mass percentage of MgO in the raw material binder of the aluminum enamel powder slurry of Example 6 is relatively low, which has little effect on the Vickers hardness and friction coefficient of the obtained composite coating, but leads to the deterioration of the bonding force between the aluminum enamel coating and the carbon fiber material; the mass percentage of MgO in the raw material binder of the aluminum enamel powder slurry of Example 7 is relatively high, which will increase the preparation cost of the composite coating on the surface of the carbon fiber material, and the economic benefit is poor;

[0211] (4) Combining Example 1 and Example 8, it can be seen that the temperature of plasma spraying NiCr powder in Example 8 is relatively high, the Vickers hardness and wear resistance of the obtained composite coating deteriorate, and the carbon fiber is oxidized, pyrolyzed, cracked, etc.;

[0212] (5) It can be seen from Example 1 and Comparative Example 1 that the surface of the carbon fiber material after sandblasting roughening in Comparative Example 1 is smoother than that of the aluminum enamel coating, which is not conducive to good mechanical interlocking of the NiCr coating; the Vickers hardness and friction coefficient of the obtained composite coating do not change much;

[0213] (6) It can be seen from Example 1 and Comparative Example 2 that in Comparative Example 2, step (1) of spraying the aluminum enamel powder slurry is not performed, and step (2) is performed directly, which results in a lower Vickers hardness of the obtained composite coating, which is 1330, and a friction coefficient of 0.41;

[0214] (7) It can be seen from Example 1 and Comparative Examples 3-4 that the aluminum enamel coating in Comparative Example 3 is too thin to well insulate the high temperature of plasma spraying, which will cause deformation of the carbon fiber. The Vickers hardness of the obtained composite coating is reduced to 1370, and the friction coefficient is 0.42. The aluminum enamel coating in Comparative Example 4 is too thick, which will increase the preparation cost of the composite coating on the surface of the carbon fiber material, resulting in poor economic benefits.

[0215] (8) Combining Example 1 with Comparative Examples 5 and 6, it can be seen that Cr 2 O 3 The thin coating thickness will lead to a significant reduction in the Vickers hardness of the composite coating, which is only 1356, and the friction coefficient is 0.38; 2 O 3 The thicker the coating is, the lower the Vickers hardness of the obtained composite coating will be, which will increase the preparation cost of the composite coating on the surface of the carbon fiber material and result in poor economic benefits.

[0216] It is stated that the above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a composite coating sprayed on the surface of a carbon fiber material, characterized in that: The preparation method comprises the following steps: (1) Spraying aluminum enamel powder slurry on the surface of the carbon fiber material to form an aluminum enamel coating with a thickness of 0.08~0.1mm; The raw materials of the aluminum enamel powder slurry include aluminum powder, enamel powder and a binder; In terms of mass percentage, the raw materials of the enamel powder include: 50% to 51% SiO2, 8.5% to 9.5% Al2O3, 10.5% to 11.5% B2O3, 9% to 10% Na2O, 10.5% to 11.5% CaO and 9.5% to 10.5% MgO; In terms of mass percentage, the raw materials of the binder include: 3% to 4% CrO3, 3% to 4% MgO, 8% to 9% H3PO4 and 84% to 85% H2O; (2) plasma spraying NiCr powder on the aluminum enamel coating to form a NiCr coating with a thickness of 0.08-0.1 mm; (3) Plasma spraying Cr2O3 powder on the NiCr coating to form a Cr2O3 coating with a thickness of 0.15-0.2 mm.

2. The preparation method according to claim 1, characterized in that: Step (1) The carbon fiber material is subjected to ultrasonic cleaning and sandblasting in sequence before being sprayed with aluminum enamel powder; The roughness Ra of the carbon fiber material after sandblasting is 2-4 μm.

3. The preparation method according to claim 1, characterized in that: The purity of the aluminum powder in step (1) is ≥99.5%; The particle size of the aluminum powder is 15-45 μm; The aluminum enamel powder slurry contains aluminum powder and enamel powder in a mass ratio of 4:1 to form a mixed powder; The mass concentration of the binder in the aluminum enamel powder slurry is 15% to 16%; The mass ratio of the mixed powder to the binder in the aluminum enamel powder slurry is 1:

1.

4. The preparation method according to claim 1, characterized in that: The process parameters for spraying the aluminum enamel powder slurry in step (1) include: Spraying line speed 10mm / min, spraying step 10mm, spraying distance 130~150mm, spraying pressure 0.3~0.4MPa; The process of spraying the aluminum enamel powder slurry includes spraying and drying processes which are repeated in sequence; The temperature of the drying process is 90-110°C; The drying time is ≥ 1h; After the last drying treatment, the curing treatment is carried out at a temperature of 280~310℃ and a time of ≥1h.

5. The preparation method according to claim 1, characterized in that: The NiCr powder in step (2) includes Ni 20 Cr powder; The process parameters of the plasma spraying NiCr powder include: Argon flow rate 49~51NLPM, hydrogen flow rate 9~11NLPM, voltage 65~70V, current 550~600A, powder feeding rate 48~50g / min, spraying distance 115~120mm, spraying angle 90°, line speed 130~140m / min, step 3.5~4.0mm, temperature ≤200℃.

6. The preparation method according to claim 1, characterized in that: The purity of the Cr2O3 powder in step (3) is ≥99.5%; The particle size of the Cr2O3 powder is 15-45 μm; The process parameters of the plasma spraying Cr2O3 powder include: Argon flow rate 49~51NLPM, hydrogen flow rate 9~11NLPM, voltage 70~75V, current 550~600A, powder feeding rate 40~42g / min, spraying distance 105~110mm, spraying angle 90°, linear speed 160~170m / min, stepping 6.0~6.5mm.

7. The preparation method according to claim 1, characterized in that: The preparation method also includes sequentially performing rough grinding and fine grinding on the Cr2O3 coating.

8. The preparation method according to claim 7, characterized in that: The roughness of the Cr2O3 coating after fine grinding is Ra≤0.8μm.

9. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: (1) After ultrasonic cleaning and sandblasting of the carbon fiber material, aluminum enamel powder slurry is sprayed on the surface of the carbon fiber material to form an aluminum enamel coating with a thickness of 0.08-0.1 mm; The roughness Ra of the carbon fiber material after sandblasting is 2-4 μm; The raw materials of the aluminum enamel powder slurry include aluminum powder, enamel powder and a binder; the purity of the aluminum powder is ≥99.5%; the particle size of the aluminum powder is 15-45 μm; In terms of mass percentage, the raw materials of the enamel powder include: 50% to 51% SiO2, 8.5% to 9.5% Al2O3, 10.5% to 11.5% B2O3, 9% to 10% Na2O, 10.5% to 11.5% CaO and 9.5% to 10.5% MgO; In terms of mass percentage, the raw materials of the binder include: 3% to 4% CrO3, 3% to 4% MgO, 8% to 9% H3PO4 and 84% to 85% H2O; The aluminum powder and enamel powder in the aluminum enamel powder slurry are formed into a mixed powder in a mass ratio of 4:1; the mass concentration of the binder in the aluminum enamel powder slurry is 15% to 16%; the mass ratio of the mixed powder to the binder in the aluminum enamel powder slurry is 1:1; The process parameters of spraying aluminum enamel powder slurry include: Spraying line speed 10m / min, spraying step 10mm, spraying distance 130~150mm, spraying pressure 0.3~0.4MPa; The process of spraying the aluminum enamel powder slurry includes spraying and drying treatments which are repeated in sequence; the temperature of the drying treatment is 90-110° C.; the time of the drying treatment is ≥1h; after the last drying treatment, a curing treatment is performed at a temperature of 280-310° C. for a time of ≥1h; (2) plasma spraying NiCr powder on the aluminum enamel coating to form a NiCr coating with a thickness of 0.08-0.1 mm; The NiCr powder includes Ni 20 Cr powder; the process parameters of the plasma spraying NiCr powder include: argon flow rate 49~51NLPM, hydrogen flow rate 9~11NLPM, voltage 65~70V, current 550~600A, powder feeding rate 48~50g / min, spraying distance 115~120mm, spraying angle 90°, line speed 130~140m / min, step 3.5~4.0mm, temperature ≤200℃; (3) plasma spraying Cr2O3 powder on the NiCr coating to form a Cr2O3 coating with a thickness of 0.15-0.2 mm; performing rough grinding and fine grinding on the Cr2O3 coating in sequence, wherein the roughness Ra of the Cr2O3 coating after fine grinding is ≤0.8 μm; The purity of the Cr2O3 powder is ≥99.5%; the particle size of the Cr2O3 powder is 15-45 μm; The process parameters of the plasma spraying of Cr2O3 powder include: argon flow rate 49~51NLPM, hydrogen flow rate 9~11NLPM, voltage 70~75V, current 550~600A, powder feeding rate 40~42g / min, spraying distance 105~110mm, spraying angle 90°, linear speed 160~170m / min, and stepping 6.0~6.5mm.

10. A composite coating sprayed on the surface of a carbon fiber material, characterized in that: The composite coating is prepared by the method for preparing a composite coating sprayed on the surface of a carbon fiber material according to any one of claims 1 to 9.