A para-aramid spinning aid and its preparation method and application
By using a spinning oil agent including polyfatty acid esters, polyol fatty acid esters, polyol/caster oil and ethylene oxide condensation, additives of activity enhancers of epoxy resins, The problem of insufficient bonding strength between para-aramid fiber and resin is solved, and efficient fiber surface modification and interface shear strength improvement without washing is achieved.
Patent Information
- Application Number
- CN202411052369.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The existing para-aramid fiber spinning additives have shortcomings in improving the bonding strength between fiber and resin, and downstream washing is required during the processing process, resulting in increased environmental pollution and cost.
Using an additive formula containing a spinning oil agent, an activity enhancer and deionized water, the spinning oil agent consists of polyfatty acid esters, polyol fatty acid esters, polyol/castor oil and ethylene oxide condensate, Polyol ether phosphate potassium salt, activity enhancer includes coupling agent and epoxy resin, and the para-aramid spinning additive is formed after homogenization and uniform treatment, which is used for oiling operation of para-aramid fibers. Avoid downstream washing treatment.
Without downstream washing treatment, the wetting property of the fiber surface resin and the chemical linking effect between the fiber and the resin are significantly improved, the interface shear strength between the fiber and the resin is enhanced, and the interlayer shear strength of the composite material is improved. and impact resistance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to a para-aramid spinning auxiliary agent and a preparation method and application thereof, belonging to the technical field of para-aramid fiber spinning auxiliary agents. Background Art
[0002] Para-aramid fiber has the advantages of high strength, high modulus, light weight, good impact resistance, etc., and has significant advantages in aerospace, bulletproof protection and other application fields. However, due to the presence of benzene ring structure in the para-aramid molecular chain, it has a strong inhibitory effect on the hydrogen atoms on the amide bond (-CONH), resulting in very few active sites on the fiber surface. In the downstream application process, it manifests as poor wettability and weak bonding force, which affects the bonding effect between it and the matrix. However, the interface is the key area for achieving stress transfer, and weak interlaminar shear strength is not conducive to improving the overall performance of the composite material, thus limiting the widespread use of aramid fiber in composite materials.
[0003] Since para-aramid fiber has extremely high requirements for fiber bundling and wear resistance during processing, it is usually treated with spinning oil during processing. Chinese patent application CN103590252A discloses a spinning oil for polyester fiber and its preparation method, the oil includes trimethylolpropane tridecyl ester, polyoxyethylene lauryl phosphate methyl salt, castor oil polyoxyethylene ester, nonionic surfactant, fatty acid polyoxyethylene ester, ionized water, etc. By using the oil, the fiber surface can be made smoother and softer, and the generation of static electricity can be reduced. Chinese patent application CN117587626A discloses a stock solution oiling type para-aramid spinning oil, including a smoothing agent, an emulsifier, an antistatic agent and an antioxidant, which can provide good wettability, smoothness, permeability, antistatic property and unwinding performance. However, the main components of these existing aramid fiber oils are ester and ether compounds, which are difficult to react with the resin matrix to produce chemical bonds. They can only play a lubricating and antistatic effect, and also hinder the direct contact between the fiber and the resin matrix, which has a counterproductive effect on the bonding effect. Therefore, the interface adhesion between the oiled aramid fiber and the resin matrix is poor, and it is easy to delaminate and peel. And this part of the oil often needs to be washed off in downstream applications, which easily generates a large amount of wastewater, causing environmental pollution and rising costs.
[0004] In addition, in order to improve the interfacial bonding strength between aramid and resin, physical modification and chemical modification methods are mainly used to improve the surface activity of aramid fibers. However, these methods are often complicated, have high requirements on equipment, and involve high costs, which are not conducive to large-scale production. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a para-aramid spinning aid and a preparation method and application thereof. The spinning aid can not only meet the bundling, wear resistance, antistatic and other requirements required for the production of para-aramid, but also improve the interface shear strength between the para-aramid fiber and the resin without the need for downstream water washing treatment.
[0006] The technical solution of the present invention to solve the above technical problems is as follows: a para-aramid spinning aid, wherein the components and mass percentages of the spinning aid are:
[0007] Spinning oil: 15.0-20.0 wt%;
[0008] Activity enhancer: 1.0-5.0 wt%;
[0009] Deionized water: 75.0-84.0 wt%; the total weight of each component is 100%;
[0010] The spinning oil comprises polyhydric fatty acid ester, polyhydric alcohol fatty acid ester, polyhydric alcohol / castor oil and ethylene oxide condensate, and polyhydric alcohol ether phosphate potassium salt;
[0011] The activity enhancer includes a coupling agent and an epoxy resin.
[0012] Furthermore, the mass percentages of the various components of the spinning oil in the spinning aid are: 10-12 wt% of polybasic fatty acid ester, 2-4 wt% of polyol fatty acid ester, 1-5 wt% of polyol / castor oil and ethylene oxide condensate, and 1-2 wt% of polyol ether phosphate potassium salt.
[0013] Furthermore, the mass percentages of the components of the active enhancer in the spinning aid are: coupling agent 0.5-3wt%, epoxy resin 0.5-2wt%.
[0014] Furthermore, the polybasic fatty acid ester is at least one of isooctyl stearate, isotridecyl stearate, and polyoxyethylene oleate;
[0015] The polyol fatty acid ester is at least one of sorbitan fatty acid ester and polyoxyethylene sorbitan fatty acid ester.
[0016] Furthermore, the polyol / castor oil and ethylene oxide condensate is at least one of isomeric tridecanol polyoxyethylene ether, polyoxyethylene ether castor oil, and polyoxyethylene hydrogenated castor oil.
[0017] Furthermore, the polyol ether phosphate potassium salt is at least one of isomeric tridecanol polyoxyethylene ether phosphate potassium salt and C12-13 alcohol polyoxyethylene ether phosphate potassium salt.
[0018] Furthermore, the coupling agent is waterborne polyurethane; and the epoxy resin is waterborne epoxy resin.
[0019] Furthermore, the weight ratio of the coupling agent to the epoxy resin is (1-2):1; the weight ratio of the polyol / castor oil and ethylene oxide condensate to the polyol ether phosphate potassium salt is (1-5):1; the weight ratio of the polyol / castor oil and ethylene oxide condensate to the epoxy resin is (1.5-3.5):1.
[0020] The invention also discloses a method for preparing a para-aramid spinning aid, which comprises the following steps: adding polybasic fatty acid ester, polyol fatty acid ester, polyol / castor oil and ethylene oxide condensate, polyol ether phosphate potassium salt, epoxy resin and coupling agent to a stirring kettle in sequence, heating and then homogenizing and mixing with a homogenizer; then adding deionized water, stirring and mixing, and filtering to obtain the para-aramid spinning aid.
[0021] The invention also discloses an application of a para-aramid spinning aid, wherein the spinning aid is applied in the oiling operation of the para-aramid, and the oiling rate of the para-aramid is 1.4-1.6%.
[0022] The beneficial effects of the present invention are:
[0023] The para-aramid spinning aid of the present invention can not only meet the requirements of bundling, wear resistance, antistatic and the like required for para-aramid production, but also can modify the fiber surface and introduce active epoxy groups. It can be used to prepare aramid / epoxy resin composite materials without downstream water washing treatment, and improve the interface shear strength between aramid fiber and resin. The para-aramid spinning aid of the present invention can enhance the wetting effect of the resin matrix on the fiber surface, and can introduce a large number of active groups to enhance the chemical linking effect between the fiber and the resin, effectively enhancing the shear strength between the para-aramid fiber and the resin.
[0024] The para-aramid spinning aid of the present invention can improve the resin wettability of the surface of the para-aramid fiber, so that when the resin matrix is coated in the next step, the resin can wet the fiber surface faster and have a better wettability. The para-aramid spinning aid of the present invention is used in para-aramid spinning, which can reduce the process of modifying the surface of the para-aramid fiber, that is, it is not necessary to perform multiple surface treatment processes, which can improve the bonding effect between the coating resin and the aramid fiber, and reduce the multiple damages to the fiber caused by the numerous processes.
[0025] The para-aramid spinning aid of the present invention is applied to para-aramid fibers, can reduce the degree of friction damage between the fibers and metal guide rollers, reduce static electricity effects, play a role in lubrication and protection, and can also effectively improve the interlaminar shear strength of the composite material and improve the impact resistance.
[0026] The components of the para-aramid spinning aid of the present invention are highly compatible with each other, the para-aramid spinning aid is in a uniform transparent emulsion state, will not be delaminated after being placed for a long time, has good stability, and is easy to store; the para-aramid spinning aid is used in the para-aramid spinning process, the para-aramid oiling rate is 1.4-1.6%; the tensile strength is greater than 20.0 cN / dtex; when the para-aramid fiber and the resin are used to prepare a composite material, the para-aramid fiber does not need to be cleaned with water or other reagents for the oil agent, and does not need to be subjected to other fiber surface active treatments, and the interlaminar shear strength of the aramid / epoxy resin composite material is greater than 40.0 MPa.
[0027] The para-aramid spinning aid of the present invention has a simple preparation process, a simple workshop use process, and an excellent modification effect, which is conducive to the further industrialization and expansion of para-aramid fibers in the field of composite materials. DETAILED DESCRIPTION
[0028] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0030] A para-aramid spinning aid, wherein the components and mass percentages of the spinning aid are:
[0031] Spinning oil: 15.0-20.0 wt%;
[0032] Activity enhancer: 1.0-5.0 wt%;
[0033] Deionized water: 75.0-84.0 wt%; the total weight of each component is 100%;
[0034] The spinning oil comprises polyhydric fatty acid ester, polyhydric alcohol fatty acid ester, polyhydric alcohol / castor oil and ethylene oxide condensate, and polyhydric alcohol ether phosphate potassium salt;
[0035] The activity enhancer includes a coupling agent and an epoxy resin.
[0036] Specifically, the mass percentages of the various components of the spinning oil in the spinning aid are: 10-12 wt% of polybasic fatty acid ester, 2-4 wt% of polyol fatty acid ester, 1-5 wt% of polyol / castor oil and ethylene oxide condensate, and 1-2 wt% of polyol ether phosphate potassium salt.
[0037] Specifically, the mass percentages of the components of the active enhancer in the spinning aid are: coupling agent 0.5-3 wt %, epoxy resin 0.5-2 wt %.
[0038] Specifically, the polybasic fatty acid ester is at least one of isooctyl stearate, isotridecyl stearate, and polyoxyethylene oleate;
[0039] The polyol fatty acid ester is at least one of sorbitan fatty acid ester and polyoxyethylene sorbitan fatty acid ester.
[0040] Specifically, the polyol / castor oil and ethylene oxide condensate is at least one of isomeric tridecanol polyoxyethylene ether, polyoxyethylene ether castor oil, and polyoxyethylene hydrogenated castor oil.
[0041] Specifically, the polyol ether phosphate potassium salt is at least one of isomeric tridecanol polyoxyethylene ether phosphate potassium salt and C12-13 alcohol polyoxyethylene ether phosphate potassium salt.
[0042] Specifically, the coupling agent is waterborne polyurethane; and the epoxy resin is waterborne epoxy resin.
[0043] Isooctyl stearate, isotridecyl stearate, polyoxyethylene oleate, isomeric tridecanol polyoxyethylene ether, and polyoxyethylene oleate used in the embodiments of the present invention are industrial grade products purchased from Wuhan Chengtian Fine Chemical Co., Ltd.;
[0044] The polyoxyethylene ether castor oil used in the embodiments of the present invention is EL-40, which is purchased from Haian Sensheng Chemical Co., Ltd.;
[0045] The polyoxyethylene hydrogenated castor oil used in the embodiments of the present invention is HEL-40, which is purchased from Haian Sensheng Chemical Co., Ltd.;
[0046] The sorbitan fatty acid ester used in the embodiment of the present invention is Span-20, which was purchased from Nantong Renda Chemical Co., Ltd.
[0047] The polyoxyethylene sorbitan fatty acid ester used in the embodiment of the present invention is Tween-20, purchased from Nantong Renda Chemical Co., Ltd.;
[0048] The isomeric tridecanol polyoxyethylene ether phosphate potassium salt and C12-13 alcohol polyoxyethylene ether phosphate potassium salt used in the embodiments of the present invention are Haishihua brand and purchased from Nantong Jiuze Chemical Co., Ltd.;
[0049] The waterborne epoxy resin used in the embodiment of the present invention is F0707, purchased from Shenzhen Yoshida Chemical Co., Ltd.;
[0050] The waterborne polyurethane used in the embodiment of the present invention is homemade, and the specific preparation method is: under stirring conditions, diphenylmethane diisocyanate and polyethylene glycol (M2000) are mixed and reacted at 120°C for 6 hours to obtain a polyurethane prepolymer, and the temperature is lowered to 100°C, caprolactam is added, and the reaction is carried out at 100°C for 2 hours to obtain a waterborne polyurethane. The molar ratio of the hydroxyl group in the polyethylene glycol to the isocyanate group in the diphenylmethane diisocyanate is 1:2, and the molar ratio of the caprolactam to the isocyanate group in the diphenylmethane diisocyanate is 1:1.
[0051] Specifically, the weight ratio of the coupling agent to the epoxy resin is (1-2):1; the weight ratio of the polyol / castor oil and ethylene oxide condensate to the polyol ether phosphate potassium salt is (1-5):1; the weight ratio of the polyol / castor oil and ethylene oxide condensate to the epoxy resin is (1.5-3.5):1.
[0052] A method for preparing a para-aramid spinning aid comprises the following steps: adding polybasic fatty acid ester, polyol fatty acid ester, polyol / castor oil and ethylene oxide condensate, polyol ether phosphate potassium salt, epoxy resin and coupling agent to a stirring kettle in sequence, heating and then homogenizing and mixing with a homogenizer; then adding deionized water, stirring and mixing, and filtering to obtain the para-aramid spinning aid.
[0053] Specifically, the heating temperature is 60-80° C., the homogenizing speed is 2400-2800 r / min, the homogenizing time is 10-15 min, and the stirring time is 1-2 h; the stirrer used for stirring is a homogenizing emulsifier.
[0054] The para-aramid spinning aid is in a uniform transparent emulsion state, with good compatibility between the components, and will not stratify after long-term storage (no stratification will occur after 48 hours in the experiment), which is convenient for storage. The para-aramid spinning aid has an effective ingredient content of 15-25% by mass, a pH value of 7±1, and a kinematic viscosity (25°C) of <3.5 mm 2 / s.
[0055] An application of a para-aramid spinning auxiliary agent: using the para-aramid spinning oil agent to impregnate the para-aramid fiber that has not been surface treated, and after drying, obtaining the para-aramid fiber with the surface impregnated with the oil agent, and the oiling rate is controlled to be 1.4-1.6%;
[0056] Furthermore, the para-aramid fiber with the surface impregnated oil is coated with epoxy resin, pressurized in a pressurized mold, and heated to a pre-curing temperature, and then heated to a curing temperature to obtain a para-aramid / epoxy resin composite sample.
[0057] In the above process, the para-aramid fiber does not need to be cleaned with water or other reagents, nor does it need other fiber surface active treatments; the interlaminar shear strength of the aramid / epoxy resin composite material is >40.0 Mpa.
[0058] More specifically, the para-aramid fiber used in the embodiment of the present invention is Tepron 1500D-529S filament, and the epoxy resin used is bisphenol A epoxy resin, specifically AM-8927A / B coating resin.
[0059] Example 1
[0060] A para-aramid spinning aid, the components and mass percentages of which are:
[0061] 15.0 wt% spinning oil (8.0 wt% of isooctyl stearate, 2.0 wt% of polyoxyethylene oleate, 1.0 wt% of sorbitan fatty acid ester, 2.0 wt% of polyoxyethylene sorbitan fatty acid ester, 1.0 wt% of isomeric tridecanol polyoxyethylene ether, 1.0 wt% of C12-C13 alcohol polyoxyethylene ether potassium phosphate);
[0062] 1.0 wt% active enhancer (0.5 wt% waterborne polyurethane, 0.5 wt% waterborne epoxy resin);
[0063] 84 wt% deionized water.
[0064] A method for preparing a para-aramid spinning aid comprises the following steps: adding polyhydric fatty acid esters, polyol fatty acid esters, polyol / castor oil and ethylene oxide condensates, polyol ether phosphate potassium salts, epoxy resins and coupling agents to a stirring kettle in sequence, heating and then homogenizing and mixing using a homogenizer; then adding deionized water, stirring and mixing, and filtering to obtain the para-aramid spinning aid.
[0065] The heating temperature is 70° C., the homogenizing speed is 2500 r / min, the homogenizing time is 15 min, and the stirring time is 1.5 h; the stirrer used for stirring is a homogenizing emulsifier.
[0066] The para-aramid spinning aid is a blue-white transparent emulsion, which is uniform and stable for 48 hours without stratification, has an effective ingredient of 16.0wt%, and a viscosity of 2.3 mm 2 / s, pH value of para-aramid spinning aid: 7.5, conductivity of para-aramid spinning aid: 710.7 μS / cm.
[0067] The para-aramid fiber is oiled by using the para-aramid spinning aid, and no obvious broken ends or hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0068] Example 2
[0069] A para-aramid spinning aid, the components and mass percentages of which are:
[0070] 20.0 wt% spinning oil (8.0 wt% isotridecyl stearate, 4.0 wt% isooctyl stearate, 2.0 wt% isotridecyl alcohol polyoxyethylene ether, 2.0 wt% polyoxyethylene castor oil, 2.0 wt% polyoxyethylene sorbitan fatty acid ester, 2.0 wt% isotridecyl alcohol polyoxyethylene ether potassium salt);
[0071] 5.0 wt% active enhancer (3.0 wt% waterborne polyurethane, 2.0 wt% waterborne epoxy resin)
[0072] 75.0 wt% deionized water.
[0073] A method for preparing a para-aramid spinning aid comprises the following steps: adding polyhydric fatty acid esters, polyol fatty acid esters, polyol / castor oil and ethylene oxide condensates, polyol ether phosphate potassium salts, epoxy resins and coupling agents to a stirring kettle in sequence, heating and then homogenizing and mixing using a homogenizer; then adding deionized water, stirring and mixing, and filtering to obtain the para-aramid spinning aid.
[0074] The heating temperature is 60° C., the homogenizing speed is 2800 r / min, the homogenizing time is 10 min, and the stirring time is 2 h; the stirrer used for stirring is a homogenizing emulsifier.
[0075] The para-aramid spinning aid is a blue-white transparent emulsion, which is uniform, stable and non-stratified for 48 hours, has an effective ingredient of 25.0wt%, a viscosity of 2.7 mm2 / s, a pH value of 7.8, and an electrical conductivity of 720.4 μS / cm.
[0076] The para-aramid fiber is oiled by using the para-aramid spinning aid, and no obvious broken ends or hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0077] Example 3
[0078] A para-aramid spinning aid, the components and mass percentages of which are:
[0079] 18.0 wt% of basic spinning oil (6.0 wt% of isooctyl stearate, 2.0 wt% of isotridecyl stearate, 3.0 wt% of polyoxyethylene oleate, 3.0 wt% of polyoxyethylene hydrogenated castor oil, 1.0 wt% of sorbitan fatty acid ester, 2.0 wt% of polyoxyethylene sorbitan fatty acid ester, 0.5 wt% of isotridecyl alcohol polyoxyethylene ether phosphate potassium salt, 0.5 wt% of C12-C13 alcohol polyoxyethylene ether phosphate potassium salt);
[0080] 3.0 wt% active enhancer (2.0 wt% waterborne polyurethane, 1.0 wt% waterborne epoxy resin);
[0081] 79.0wt% deionized water.
[0082] A method for preparing a para-aramid spinning aid comprises the following steps: adding polyhydric fatty acid esters, polyol fatty acid esters, polyol / castor oil and ethylene oxide condensates, polyol ether phosphate potassium salts, epoxy resins and coupling agents to a stirring kettle in sequence, heating and then homogenizing and mixing using a homogenizer; then adding deionized water, stirring and mixing, and filtering to obtain the para-aramid spinning aid.
[0083] The heating temperature is 70° C., the homogenizing speed is 2500 r / min, the homogenizing time is 15 min, and the stirring time is 1.5 h; the stirrer used for stirring is a homogenizing emulsifier.
[0084] The para-aramid spinning aid is a blue-white transparent emulsion, which is uniform and stable for 48 hours without stratification, has an effective ingredient of 21.0wt%, and a viscosity of 2.6 mm 2 / s, pH value of para-aramid spinning aid: 7.8, conductivity of para-aramid spinning aid: 784.3 μS / cm.
[0085] The para-aramid fiber is oiled by using the para-aramid spinning aid, and no obvious broken ends or hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0086] Example 4
[0087] A para-aramid spinning aid, the components and mass percentages of which are:
[0088] 18.0 wt% basic spinning oil (8.0 wt% isotridecyl stearate, 2.0 wt% polyoxyethylene oleate, 2.0 wt% isotridecyl alcohol polyoxyethylene ether, 1.0 wt% polyoxyethylene castor oil, 1.0 wt% sorbitan fatty acid ester, 2.0 wt% polyoxyethylene sorbitan fatty acid ester, 2.0 wt% C12-C13 alcohol polyoxyethylene ether potassium phosphate);
[0089] 2.0 wt% active enhancer (1.0 wt% waterborne polyurethane, 1.0 wt% waterborne epoxy resin);
[0090] 80.0wt% deionized water.
[0091] A method for preparing a para-aramid spinning aid comprises the following steps: adding polyhydric fatty acid esters, polyol fatty acid esters, polyol / castor oil and ethylene oxide condensates, polyol ether phosphate potassium salts, epoxy resins and coupling agents to a stirring kettle in sequence, heating and then homogenizing and mixing using a homogenizer; then adding deionized water, stirring and mixing, and filtering to obtain the para-aramid spinning aid.
[0092] The heating temperature is 70° C., the homogenizing speed is 2500 r / min, the homogenizing time is 15 min, and the stirring time is 1.5 h; the stirrer used for stirring is a homogenizing emulsifier.
[0093] The para-aramid spinning aid is a blue-white transparent emulsion, which is uniform and stable for 48 hours without stratification, has an effective ingredient of 20.0wt%, and a viscosity of 2.2 mm 2 / s, pH value of para-aramid spinning aid: 7.6; conductivity of para-aramid spinning aid: 765.4 μS / cm.
[0094] The para-aramid fiber is oiled by using the para-aramid spinning aid, and no obvious broken ends or hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0095] Example 5
[0096] A para-aramid spinning aid, the components and mass percentages of which are:
[0097] 18.0 wt% basic spinning oil (6.0 wt% polyoxyethylene oleate, 4.0 wt% isooctyl stearate, 3.0 wt% isotridecyl alcohol polyoxyethylene ether, 2.0 wt% polyoxyethylene hydrogenated castor oil, 2.0 wt% sorbitan fatty acid ester, 1.0 wt% isotridecyl alcohol polyoxyethylene ether potassium salt);
[0098] 2.0 wt% active enhancer (1.5 wt% waterborne polyurethane, 0.5 wt% waterborne epoxy resin);
[0099] 80.0 wt% deionized water.
[0100] A method for preparing a para-aramid spinning aid comprises the following steps: adding polyhydric fatty acid esters, polyol fatty acid esters, polyol / castor oil and ethylene oxide condensates, polyol ether phosphate potassium salts, epoxy resins and coupling agents to a stirring kettle in sequence, heating and then homogenizing and mixing using a homogenizer; then adding deionized water, stirring and mixing, and filtering to obtain the para-aramid spinning aid.
[0101] The heating temperature is 70° C., the homogenizing speed is 2500 r / min, the homogenizing time is 15 min, and the stirring time is 1.5 h; the stirrer used for stirring is a homogenizing emulsifier.
[0102] The para-aramid spinning aid is a blue-white transparent emulsion, which is uniform and stable for 48 hours without stratification, has an effective ingredient of 20.0wt%, and a viscosity of 2.3 mm 2 / s, pH value of para-aramid spinning aid: 7.3; conductivity of para-aramid spinning aid: 644.6 μS / cm.
[0103] The para-aramid fiber is oiled by using the para-aramid spinning aid, and no obvious broken ends or hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0104] Example 6
[0105] A para-aramid spinning aid, the components and mass percentages of which are:
[0106] 20.0 wt% basic spinning oil (12.0 wt% isooctyl stearate, 2.0 wt% sorbitan fatty acid ester, 2.0 wt% polyoxyethylene sorbitan fatty acid ester, 3.0 wt% polyoxyethylene castor oil, 1.0 wt% C12-C13 alcohol polyoxyethylene ether phosphate potassium salt);
[0107] 5.0 wt% active enhancer (3.0 wt% waterborne polyurethane, 2.0 wt% waterborne epoxy resin);
[0108] 75.0 wt% deionized water.
[0109] A method for preparing a para-aramid spinning aid comprises the following steps: adding polyhydric fatty acid esters, polyol fatty acid esters, polyol / castor oil and ethylene oxide condensates, polyol ether phosphate potassium salts, epoxy resins and coupling agents to a stirring kettle in sequence, heating and then homogenizing and mixing using a homogenizer; then adding deionized water, stirring and mixing, and filtering to obtain the para-aramid spinning aid.
[0110] The heating temperature is 70° C., the homogenizing speed is 2500 r / min, the homogenizing time is 15 min, and the stirring time is 1.5 h; the stirrer used for stirring is a homogenizing emulsifier.
[0111] The para-aramid spinning aid is a blue-white transparent emulsion, which is uniform and stable for 48 hours without stratification, has an effective ingredient of 25.0wt%, and a viscosity of 2.4 mm 2 / s, pH value of para-aramid spinning aid: 7.8; conductivity of para-aramid spinning aid: 614.3 μS / cm.
[0112] The para-aramid fiber is oiled by using the para-aramid spinning aid, and no obvious broken ends or hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0113] Comparative Example 1
[0114] The para-aramid spinning aid was prepared by the same method as in Example 1, except that no water-based epoxy resin was added to the formulation. The formulation of this comparative example 1 was as follows:
[0115] 15.0 wt% spinning oil (8.0 wt% of isooctyl stearate, 2.0 wt% of polyoxyethylene oleate, 1.0 wt% of sorbitan fatty acid ester, 2.0 wt% of polyoxyethylene sorbitan fatty acid ester, 1.0 wt% of isomeric tridecanol polyoxyethylene ether, 1.0 wt% of C12-C13 alcohol polyoxyethylene ether potassium phosphate);
[0116] 0.5 wt% active enhancer (0.5 wt% waterborne polyurethane);
[0117] 84.5 wt% deionized water.
[0118] The para-aramid spinning aid prepared in this comparative example 1 is a bluish-white transparent liquid, which is uniform and stable without stratification for 48 hours, has an effective ingredient of 15.5 wt%, and a viscosity of 2.3 mm 2 / s, pH value of para-aramid spinning aid: 7.4, conductivity of para-aramid spinning aid: 690.4 μS / cm.
[0119] The para-aramid fiber is oiled by using the para-aramid spinning aid, and no obvious broken ends or hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0120] Comparative Example 2
[0121] The para-aramid spinning aid was prepared by the same method as in Example 1, except that no waterborne polyurethane was added to the formulation. The formulation of this comparative example 2 was as follows:
[0122] 15.0 wt% spinning oil (8.0 wt% of isooctyl stearate, 2.0 wt% of polyoxyethylene oleate, 1.0 wt% of sorbitan fatty acid ester, 2.0 wt% of polyoxyethylene sorbitan fatty acid ester, 1.0 wt% of isomeric tridecanol polyoxyethylene ether, 1.0 wt% of C12-C13 alcohol polyoxyethylene ether potassium phosphate);
[0123] 0.5 wt% active enhancer (0.5 wt% waterborne epoxy resin);
[0124] 84.5 wt% deionized water.
[0125] The para-aramid spinning aid prepared in this comparative example 2 is a bluish-white transparent liquid, which is uniform and stable without stratification for 48 hours, has an effective ingredient of 15.5 wt%, and a viscosity of 2.4 mm 2 / s, pH value of para-aramid spinning aid: 7.4, conductivity of para-aramid spinning aid: 702.5 μS / cm.
[0126] The para-aramid fiber is oiled by using the para-aramid spinning aid, and no obvious broken ends or hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0127] Comparative Example 3
[0128] The para-aramid spinning aid was prepared by the same method as in Example 1, except that the amount of the waterborne epoxy resin was increased. The formulation of this comparative example 3 was as follows:
[0129] 15.0 wt% spinning oil (8.0 wt% of isooctyl stearate, 2.0 wt% of polyoxyethylene oleate, 1.0 wt% of sorbitan fatty acid ester, 2.0 wt% of polyoxyethylene sorbitan fatty acid ester, 1.0 wt% of isomeric tridecanol polyoxyethylene ether, 1.0 wt% of C12-C13 alcohol polyoxyethylene ether potassium phosphate);
[0130] 4.5 wt% active enhancer (0.5 wt% waterborne polyurethane, 4 wt% waterborne epoxy resin);
[0131] 80.5 wt% deionized water.
[0132] The para-aramid spinning aid prepared in this comparative example 3 is a blue-white transparent liquid, which shows stratification after 48 hours, with an effective ingredient of 19.5 wt % and a viscosity of 2.5 mm 2 / s, pH value of para-aramid spinning aid: 7.5, conductivity of para-aramid spinning aid: 711.4 μS / cm.
[0133] The para-aramid fiber is oiled by using the para-aramid spinning aid, and obvious broken ends and hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0134] Comparative Example 4
[0135] The para-aramid spinning aid was prepared by the same method as in Example 1, except that the waterborne polyurethane was replaced with other conventional coupling agent 3-aminopropyltriethoxysilane. The formulation of this comparative example 4 was as follows:
[0136] 15.0 wt% spinning oil (8.0 wt% of isooctyl stearate, 2.0 wt% of polyoxyethylene oleate, 1.0 wt% of sorbitan fatty acid ester, 2.0 wt% of polyoxyethylene sorbitan fatty acid ester, 1.0 wt% of isomeric tridecanol polyoxyethylene ether, 1.0 wt% of C12-C13 alcohol polyoxyethylene ether potassium phosphate);
[0137] 1.0 wt% of active enhancer (0.5 wt% of 3-aminopropyltriethoxysilane, 0.5 wt% of waterborne epoxy resin);
[0138] 84 wt% deionized water.
[0139] The para-aramid spinning aid prepared in this comparative example 4 is a bluish-white transparent liquid, which is uniform and stable without stratification for 48 hours, has an effective ingredient of 16 wt%, and a viscosity of 2.5 mm 2 / s, pH value of para-aramid spinning aid: 7.5, conductivity of para-aramid spinning aid: 611.4 μS / cm.
[0140] The para-aramid fiber is oiled by using the para-aramid spinning aid, and no obvious broken ends or hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0141] Comparative Example 5
[0142] The para-aramid spinning aid was prepared by the same method as in Example 1, except that the isomeric tridecanol polyoxyethylene ether was not added, and the total amount of the spinning oil was made the same as that in Example 1 by increasing the amount of polyoxyethylene sorbitan fatty acid ester. The formulation of this comparative example 5 was as follows:
[0143] 15.0 wt% spinning oil (8.0 wt% isooctyl stearate, 2.0 wt% polyoxyethylene oleate, 1.0 wt% sorbitan fatty acid ester, 3.0 wt% polyoxyethylene sorbitan fatty acid ester, 1.0 wt% C12-C13 alcohol polyoxyethylene ether phosphate potassium salt);
[0144] 1.0 wt% of active enhancer (0.5 wt% of 3-aminopropyltriethoxysilane, 0.5 wt% of waterborne epoxy resin);
[0145] 84 wt% deionized water.
[0146] The para-aramid spinning aid prepared in this comparative example 5 is a blue-white transparent liquid, which shows stratification after 48 hours, has an effective ingredient of 16 wt%, and a viscosity of 2.3 mm 2 / s, pH value of para-aramid spinning aid: 7.2, conductivity of para-aramid spinning aid: 688.2μS / cm.
[0147] The para-aramid fiber is oiled by using the para-aramid spinning aid, and obvious broken ends and hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0148] Comparative Example 6
[0149] The para-aramid spinning aid was prepared by the same method as in Example 3, except that the ratio of the coupling agent to the epoxy resin was adjusted. In this comparative example 6, the weight ratio of the waterborne polyurethane to the waterborne epoxy resin was 1:2 (not within the ratio range defined in the present invention). The formula composition of this comparative example 6 is as follows:
[0150] 18.0 wt% of basic spinning oil (6.0 wt% of isooctyl stearate, 2.0 wt% of isotridecyl stearate, 3.0 wt% of polyoxyethylene oleate, 3.0 wt% of polyoxyethylene hydrogenated castor oil, 1.0 wt% of sorbitan fatty acid ester, 2.0 wt% of polyoxyethylene sorbitan fatty acid ester, 0.5 wt% of isotridecyl alcohol polyoxyethylene ether phosphate potassium salt, 0.5 wt% of C12-C13 alcohol polyoxyethylene ether phosphate potassium salt);
[0151] 3.0 wt% of modified active agent (1.0 wt% of waterborne polyurethane, 2.0 wt% of waterborne epoxy resin);
[0152] 79.0wt% deionized water.
[0153] The para-aramid spinning aid prepared in Comparative Example 6 was a bluish-white transparent liquid, which showed stratification after 48 hours, with an effective ingredient of 21 wt % and a viscosity of 2.4 mm 2 / s, pH value of para-aramid spinning aid: 7.3, conductivity of para-aramid spinning aid: 738.2μS / cm.
[0154] The para-aramid fiber is oiled by using the para-aramid spinning aid, and obvious broken ends and hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0155] Comparative Example 7
[0156] The para-aramid spinning aid was prepared by the same method as in Example 1, except that the ratio of the polyol / castor oil to the ethylene oxide condensate and the polyol ether phosphate potassium salt was adjusted. In this comparative example 7, the weight ratio of the isomeric tridecanol polyoxyethylene ether to the C12-C13 alcohol polyoxyethylene ether phosphate potassium salt was 1:3 (not within the ratio range defined in the present invention). The formula composition of this comparative example 7 is as follows:
[0157] 15.0 wt% spinning oil (8.0 wt% of isooctyl stearate, 2.0 wt% of polyoxyethylene oleate, 1.0 wt% of sorbitan fatty acid ester, 2.0 wt% of polyoxyethylene sorbitan fatty acid ester, 0.5 wt% of isomeric tridecanol polyoxyethylene ether, 1.5 wt% of C12-C13 alcohol polyoxyethylene ether potassium phosphate);
[0158] 1.0 wt% active enhancer (0.5 wt% waterborne polyurethane, 0.5 wt% waterborne epoxy resin);
[0159] 84 wt% deionized water.
[0160] The para-aramid spinning aid prepared in this comparative example 7 is a blue-white transparent liquid, which shows stratification after 48 hours, has an effective ingredient of 16 wt%, and a viscosity of 2.3 mm 2 / s, pH value of para-aramid spinning aid: 7.3, conductivity of para-aramid spinning aid: 778.2μS / cm.
[0161] The para-aramid fiber is oiled by using the para-aramid spinning aid, and obvious broken ends and hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0162] Comparative Example 8
[0163] The para-aramid spinning aid was prepared by the same method as in Example 3, except that the amount of the water-based epoxy resin was adjusted so that the weight ratio of the polyol / castor oil to the ethylene oxide condensate to the epoxy resin was 1:1 (not within the ratio range defined in the present invention). The formulation of this comparative example 8 was as follows:
[0164] 18.0 wt% of basic spinning oil (6.0 wt% of isooctyl stearate, 2.0 wt% of isotridecyl stearate, 3.0 wt% of polyoxyethylene oleate, 3.0 wt% of polyoxyethylene hydrogenated castor oil, 1.0 wt% of sorbitan fatty acid ester, 2.0 wt% of polyoxyethylene sorbitan fatty acid ester, 0.5 wt% of isotridecyl alcohol polyoxyethylene ether phosphate potassium salt, 0.5 wt% of C12-C13 alcohol polyoxyethylene ether phosphate potassium salt);
[0165] 4.0 wt% active enhancer (2.0 wt% waterborne polyurethane, 2.0 wt% waterborne epoxy resin);
[0166] 78.0wt% deionized water.
[0167] The para-aramid spinning aid prepared in this comparative example 7 is a blue-white transparent liquid, which shows stratification after 48 hours, with an effective ingredient of 22 wt % and a viscosity of 2.3 mm 2 / s, pH value of para-aramid spinning aid: 7.3, conductivity of para-aramid spinning aid: 578.2μS / cm.
[0168] The para-aramid fiber is oiled by using the para-aramid spinning aid, and obvious broken ends and hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0169] Comparative Example 9
[0170] The para-aramid spinning aid was prepared by the same method as in Example 4, except that no active enhancer was added in this comparative example 9. The specific formula composition is as follows:
[0171] 18.0 wt% basic spinning oil (8.0 wt% isotridecyl stearate, 2.0 wt% polyoxyethylene oleate, 2.0 wt% isotridecyl alcohol polyoxyethylene ether, 1.0 wt% polyoxyethylene castor oil, 1.0 wt% sorbitan fatty acid ester, 2.0 wt% polyoxyethylene sorbitan fatty acid ester, 2.0 wt% C12-C13 alcohol polyoxyethylene ether potassium phosphate);
[0172] 82.0wt% deionized water.
[0173] The para-aramid spinning aid is a blue-white transparent emulsion, which is uniform and stable for 48 hours without stratification, has an effective ingredient of 18.0wt%, and a viscosity of 2.4 mm 2 / s, pH value of para-aramid spinning aid: 7.6; conductivity of para-aramid spinning aid: 748.3 μS / cm.
[0174] The para-aramid fiber is oiled by using the para-aramid spinning aid, and no obvious broken ends or hairy fibers are produced. The fiber does not disperse after being placed for a long time, and has good bundling property.
[0175] Comparative Example 10
[0176] An imported oil currently sold on the market has a light yellow transparent oily liquid appearance. According to the ratio of oil: deionized water = 1:4, the finished product is a blue-white transparent emulsion after stirring. It is uniform and stable without stratification for 48 hours. The effective ingredient is 20.0 wt%, and the emulsion viscosity is 2.3 mm 2 / s; emulsion pH: 7.5; emulsion conductivity: 737.9 μS / cm;
[0177] The para-aramid fiber was oiled with the oil agent, and no obvious broken ends or hairs were produced. The fiber did not disperse after being placed for a long time, and the bundling property was good.
[0178] Comparative Example 11
[0179] A domestic oil currently sold on the market has a light yellow turbid oily liquid appearance. According to the ratio of oil: deionized water = 1:4, the finished product is a white emulsion after stirring. It is uniform and stable without stratification for 48 hours. The effective ingredient is 20.0 wt% and the emulsion viscosity is 2.5 mm 2 / s, emulsion pH: 7.4; emulsion conductivity: 360.3 μS / cm;
[0180] The para-aramid fiber was oiled with the oil agent, and no obvious broken ends or hairs were produced. The fiber did not disperse after being placed for a long time, and the bundling property was good.
[0181] The para-aramid fibers after oiling in the above embodiments and comparative examples were tested to compare the bundling effect, number of filaments, oiling rate, elongation at break, breaking strength and other indicators of the textile auxiliaries (the test results are shown in Table 1 below); the specific test methods are: GB / T 6504-2017 "Test method for oil content of chemical fibers", FZT 50035-2016 "Test method for resistance of synthetic fiber filaments", TCSTM 00522-2022 "Test method for friction coefficient of chemical fibers", GB / T 14344-2022 "Test method for tensile properties of chemical fiber filaments".
[0182] The evaluation method for the bundling effect is as follows: the para-aramid fiber is cut open after winding. If the filament bundles are hugged together after cutting, the bundling effect is considered "excellent"; if the filament bundles are partially unfolded after cutting, the bundling effect is considered "good"; if the filament bundles are completely unfolded after cutting, the bundling effect is considered "poor".
[0183] In addition, the evaluation method for the number of hairy fibers is as follows: a fiber hairiness tester is used to test the number of hairy fibers of a sample per unit length. If the number of hairy fibers detected is ≤4 pieces / km, the number of hairy fibers generated in the subsequent processing is considered to be "small", and it can be considered that the requirements of the subsequent processing procedures can be met; if the number of hairy fibers detected is >4 pieces / km, the number of hairy fibers generated in the subsequent processing is considered to be "large", and it can be considered that the requirements of the subsequent processing procedures cannot be met.
[0184] Table 1 Test results of para-aramid fiber properties after oiling
[0185]
[0186] The para-aramid fibers treated with oil in the above implementation and comparative examples were compounded with resin to prepare prepregs, and standard strips were prepared, and the strip dimensions were: length × width × height = 20 mm × 6 mm × 2 mm;
[0187] Standard sample preparation method: epoxy resin is coated on the oiled para-aramid fiber, and the temperature is raised to 80°C for pre-curing for 1 h under a curing pressure of 0.2 MPa, and then the temperature is raised to 120°C for curing for 1 h to obtain the standard sample;
[0188] The epoxy resin is a bisphenol A epoxy resin, specifically AM-8927A / B coating resin;
[0189] The interlaminar shear strength test of the standard specimens was carried out in accordance with the GB / T30969-2014 standard. The specific test results are shown in Table 2 below.
[0190] Table 2 Interlaminar shear strength test results
[0191]
[0192] From the data in Table 1 and Table 2, it can be seen that the para-aramid spinning aids prepared by the formula composition of the present invention in Examples 1 to 6 can control the oiling rate of the para-aramid fiber through the cooperation of the active enhancer and the spinning oil, and the para-aramid fiber has excellent bundling effect, less hairiness, and when the fiber surface is oiled, it will not damage the original mechanical properties of the para-aramid fiber and will not affect downstream applications. Under the premise of not requiring downstream water washing treatment, it can be used to prepare aramid / epoxy resin composite materials to improve the interface shear strength between aramid fiber and resin; compared with the existing oil (Comparative Examples 10-11), the increase ratio of interlaminar shear strength is more than 20%.
[0193] From the data comparison between Comparative Example 1 and Example 1, it can be seen that if water-based epoxy resin is not added to the formula composition, the improvement in the interfacial shear strength between the aramid fiber and the resin will be reduced. This is because although the water-based polyurethane forms active groups on the fiber surface, the lack of epoxy resin access cannot effectively enhance the wetting effect of the epoxy resin on the fiber surface during subsequent processing, so the improvement effect is not obvious.
[0194] From the data comparison between Comparative Example 2 and Example 1, it can be seen that if water-based polyurethane is not added to the formula composition, more active groups will not be generated on the fiber surface. Although the addition of epoxy resin improves the wetting effect of the fiber surface, the surface activity of the fiber is not enhanced, so the bonding ability between the resin and the fiber is not significantly improved. Therefore, water-based polyurethane and water-based epoxy resin are used together in the spinning aid to make the para-aramid spinning aid have better application performance.
[0195] From the comparison of the data of Comparative Example 3 and Example 1, it can be seen that if the amount of waterborne epoxy resin is increased, the friction coefficient of the fiber will increase significantly, and the wear during the processing will be more obvious, because increasing the amount will cause the oil agent to be stratified, and during the oiling process, the distribution of the oil agent on the fiber surface becomes uneven, resulting in increased hairiness, decreased mechanical properties, etc. Therefore, the use of the waterborne epoxy resin amount defined in the present invention is more conducive to protecting the fiber molding process, reducing the friction coefficient, and reducing the amount of hairiness.
[0196] From the data comparison between Comparative Example 4 and Example 1, it can be seen that if the coupling agent is replaced with other conventional coupling agents, the improvement in fiber surface activity will be weaker and the improvement in interface bonding effect will also be lower. Because the surface activity of para-aramid fiber is low, the inert groups and steric hindrance effects are more obvious, the effect of conventional coupling agents on its surface treatment is not obvious.
[0197] From the comparison of the data of Comparative Example 5 and Example 1, it can be seen that if the polyol / castor oil and ethylene oxide condensate are not added, the oil emulsion will be unevenly emulsified and more friction will occur during the processing. This is because if the polyol / castor oil and ethylene oxide condensate are added in too little or too much proportion, the overall emulsification effect of the oil will be affected, which will in turn affect the extension effect on the fiber surface, resulting in inconsistent fiber oiling rate distribution and a larger friction coefficient during fiber molding or downstream processing.
[0198] From the data comparison between Comparative Example 6 and Example 3, it can be seen that if the ratio of the coupling agent to the epoxy resin is changed (the ratio of the epoxy resin is increased), the subsequent curing of the epoxy resin will be difficult, and the increase in the ratio of the epoxy resin will not effectively improve the performance, because the coupling agent has a certain effect on the treatment of the fiber, and simply increasing the epoxy resin will make the extension of the oil agent and the subsequent infiltration of the epoxy resin more difficult.
[0199] From the comparison of the data of Comparative Example 7 and Example 1, it can be seen that if the ratio of polyol / castor oil to ethylene oxide condensate and polyol ether phosphate potassium salt is changed (the ratio of polyol / castor oil to ethylene oxide condensate is reduced), the fiber friction coefficient will increase, the hairiness generated will increase significantly, and the interlayer shear will also decrease. This is because the change in ratio will affect the emulsification effect of the oil agent, resulting in uneven oiling, and the hairiness generated by friction will also appear to stick together, affecting the infiltration of the epoxy resin on the fiber surface, resulting in poor local infiltration and affecting the overall effect.
[0200] From the comparison of the data of Comparative Example 8 and Example 3, it can be seen that if the ratio of polyol / castor oil to ethylene oxide condensate and the epoxy resin is changed, the oil agent will be obviously stratified and the components will be unevenly distributed. Because the addition ratio of the emulsifier is crucial to the uniformity and stability of the oil agent, changes in the ratio will affect its stability and further affect whether its spreading on the fiber surface is consistent.
[0201] From the data comparison between Comparative Example 9 and Example 1, it can be seen that if no active enhancer is added to the spinning aid, the interlaminar shear effect of the oil agent will not be significantly improved, and may even be reduced, because the pure oil agent has a side effect on the composite effect of the fiber, which will affect the wetting of the resin system on the fiber surface and hinder the binding of the remaining fiber active groups.
[0202] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0203] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A para-aramid spinning aid, characterized in that: The components and mass percentages of the spinning aid are as follows: Spinning oil: 15.0-20.0 wt%; Activity enhancer: 1.0-5.0 wt%; Deionized water: 75.0-84.0 wt%; the total weight of each component is 100%; The spinning oil is composed of polyhydric fatty acid ester, polyhydric alcohol fatty acid ester, polyhydric alcohol / castor oil and ethylene oxide condensate, and polyhydric alcohol ether phosphate potassium salt; The activity enhancer is composed of a coupling agent and an epoxy resin; The coupling agent is waterborne polyurethane; the epoxy resin is waterborne epoxy resin; The weight ratio of the coupling agent to the epoxy resin is (1-2): 1; the weight ratio of the polyol / castor oil and ethylene oxide condensate to the epoxy resin is (1.5-3.5): 1; The mass percentages of the various components of the spinning oil in the spinning aid are: 10-12 wt% of polybasic fatty acid ester, 2-4 wt% of polyol fatty acid ester, 1-5 wt% of polyol / castor oil and ethylene oxide condensate, and 1-2 wt% of polyol ether phosphate potassium salt; The polybasic fatty acid ester is at least one of isooctyl stearate, isotridecyl stearate, and polyoxyethylene oleate; The polyol fatty acid ester is at least one of sorbitan fatty acid ester and polyoxyethylene sorbitan fatty acid ester.
2. The para-aramid spinning aid according to claim 1, characterized in that: The polyol / castor oil and ethylene oxide condensate is at least one of isomeric tridecanol polyoxyethylene ether, polyoxyethylene ether castor oil, and polyoxyethylene hydrogenated castor oil.
3. The para-aramid spinning aid according to claim 1, characterized in that: The polyol ether phosphate potassium salt is at least one of C12-13 alcohol polyoxyethylene ether phosphate potassium salts.
4. A method for preparing a para-aramid spinning aid according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: adding polyhydric fatty acid ester, polyol fatty acid ester, polyol / castor oil and ethylene oxide condensate, polyol ether phosphate potassium salt, epoxy resin and coupling agent into a stirring kettle in sequence, heating and then homogenizing and mixing with a homogenizer; then adding deionized water, stirring and mixing, and filtering to obtain a para-aramid spinning aid.
5. An application of a para-aramid spinning aid according to any one of claims 1 to 3, characterized in that: The spinning aid is used in the oiling operation of para-aramid, and the oiling rate of the para-aramid is 1.4-1.6%.