A TOPCon battery back nickel-copper slurry and preparation method thereof
By preparing nickel-copper slurry on the back of the TOPCon battery, which combines nickel-copper powder with micron silver powder, nano silver powder and low-melting point glass powder, the problems of high cost and insufficient conductivity of silver powder are solved, and efficient and low-cost conductive effect is achieved, improving the efficiency and low-cost conductive effect. The conversion efficiency and wear resistance of photovoltaic cells are achieved.
Patent Information
- Application Number
- CN202411036896.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The existing TOPCon battery conductive paste has a large amount of silver powder and high cost. The nickel-covered copper substitution has a great impact on conductivity, which limits the application and efficiency of photovoltaic cells.
Nickel-covered copper powder is prepared by ultrasonic oscillation and diamine reduction method, combining micron silver powder, nano silver powder and low melting point glass powder to form a high-efficiency conductive TOPCon battery The nickel-copper slurry on the back is used to form a cluster-shaped chelating agent with a multi-phosphorus-nitrogen structure and an interlaced cluster structure through electroless nickel plating, which improves conductivity and reduces costs.
It has achieved efficient replacement of traditional silver powder, reduced slurry cost, improved battery conversion efficiency, and significantly improved the conductivity and wear resistance of nickel-clad copper powder, and has good stability, which is suitable for photovoltaic cell applications.
Smart Images

Figure CN118571525B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photovoltaic cells, and in particular, relates to a nickel-copper slurry for the back side of a TOPCon cell and a preparation method thereof. Background Art
[0002] Energy, which is becoming increasingly scarce, has always been an important foundation for promoting economic and social development. Currently, the use of renewable energy to replace over-exploited non-renewable energy has become a common direction of international efforts in resource research. In the face of the development of renewable energy, its economic and environmental advantages have become increasingly prominent. The international community is paying more and more attention to ensuring the safety of the energy system and effectively responding to environmental issues. International energy needs to achieve a transition from a fossil energy structure to a low-carbon energy structure. In the future, it will enter a sustainable energy era dominated by renewable energy. The photovoltaic industry is one of the key driving forces for promoting energy transformation and implementing a revolution in energy production and consumption.
[0003] As the efficiency of existing P-type PERC cells gradually approaches the theoretical limit, N-type TOPCon cells will become an important technical route for future industrialization. TOPCon is a tunneling oxide passivation contact solar cell technology based on the principle of selective carriers. Its cell structure is an N-type silicon substrate cell. An ultra-thin layer of silicon oxide is prepared on the back of the cell, and then a thin layer of doped silicon is deposited. The two together form a passivation contact structure, which effectively reduces surface recombination and metal contact recombination, and has a higher theoretical efficiency.
[0004] Conductive paste is the conductive material of the back electrode of N-type TOPCon solar cells. It is mainly composed of conductive functional phase, inorganic binder phase and organic carrier. It plays a key role in the current extraction of the cell. The existing conductive functional phase is mostly silver powder, which has a large amount and high cost, seriously restricting the application of photovoltaic cells. In the existing technology, nickel-coated copper is used to replace silver powder, which can reduce the paste cost to a certain extent, but it has a greater impact on the conductivity of the paste. Summary of the invention
[0005] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a nickel-copper slurry for the back side of a TOPCon battery and a preparation method thereof.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A nickel-copper slurry for the back of a TOPCon battery, comprising the following components by weight percentage:
[0008] Micron silver powder 40-75wt%, nano silver powder 5-15wt%, silver nanowire 3-6wt%, nickel-coated copper powder 5-25wt% and low-melting point glass powder 2.5-4.5wt%, and the balance is organic carrier.
[0009] Furthermore, the average particle size of the nano silver powder is 50-100 nm, and the diameter of the silver nanowire is 20-40 nm.
[0010] Furthermore, the melting point of the low-melting-point glass powder is not higher than 800° C., and the fineness is not lower than 5000 mesh.
[0011] The nickel-coated copper powder is prepared by the following method:
[0012] Step A1: triethylenetetramine, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature of the reaction system is adjusted to 0-10°C in an ice-water bath, 25-33kHz ultrasonic oscillation is applied, phenylphosphonothioate dichloride is slowly added to react for 1.5-2h, tetrahydrofuran is removed by rotary evaporation after the reaction is completed, the substrate is washed with water, the aqueous phase is removed and vacuum dried to obtain a cluster chelating agent;
[0013] Furthermore, the dosage ratio of phenylthiophosphonyl dichloride, triethylenetetramine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 55-62 mmol: 10-15 mL: 45-60 mL, triethylamine is an acid binding agent, and under low-temperature ultrasound, triethylenetetramine and phenylthiophosphonyl dichloride undergo a substitution reaction of active phosphoryl chloride to form a clustered compound, and the multi-nitrogen-phosphorus structure forms a coordination effect with chelating properties.
[0014] Step A2: pickling the copper powder in concentrated hydrochloric acid, then soaking it in an acidic stannous chloride solution for sensitization treatment for 15-20 minutes, then soaking it in a hydrazine solution, and draining it to obtain activated copper powder;
[0015] Furthermore, the particle size of the copper powder is not higher than 10 μm, the pH value of the acidic stannous chloride solution is 2-3, and the mass fraction of stannous chloride is 0.6-0.8%.
[0016] Step A3: Mix the activated copper powder, clustered chelating agent, thiourea and ethanol solution, add nickel sulfate solution and mix, adjust the pH value to 10 with ammonia water, add hydrazine solution under ultrasonic oscillation to react for 10-15 minutes, then water bath at 60-70° C. for 1.2-1.6 hours, filter, wash and dry to obtain a precursor powder;
[0017] Furthermore, the dosage ratio of activated copper powder, nickel sulfate, clustered chelating agent, thiourea, hydrazine solution and ethanol solution is 50g:12-16g:3.5-4.2g:10-15mg:65-80mL:500mL, the mass fraction of hydrazine solution is 40%, and the mass fraction of ethanol solution is 50%; the clustered chelating agent preferentially chelates and complexes with the surface of activated copper powder to form a large number of clustered chelating sites on the surface, which capture the added nickel ions and fill them between the cluster structures, and then are reduced by hydrazine to form a nickel coating layer with interlaced cluster structures.
[0018] Step A4: Place the precursor powder in a calcination furnace, and calcine at 650±10°C for 1.5-2h under a nitrogen atmosphere, then continue to heat to 900±10°C and calcine for 30-50min, then cool to 200°C with the furnace, air cool and break up to obtain nickel-coated copper powder.
[0019] Furthermore, the roasting heating rate is not higher than 10°C / min, and the furnace cooling rate is not higher than 30°C / min.
[0020] A method for preparing nickel-copper slurry on the back of a TOPCon battery comprises the following specific operations: premixing micron silver powder, nano silver powder, silver nanowire, nickel-coated copper powder and low-melting point glass powder by a high-speed mixer, adding an organic carrier, grinding and mixing, and obtaining the nickel-copper slurry on the back of the TOPCon battery.
[0021] Beneficial effects of the present invention:
[0022] The invention adopts independently developed nickel-coated copper micropowder to replace part of the silver powder in the conventional TOPCon battery conductive paste. Compared with the conventional nickel-coated copper compound silver paste, the invention has less influence on the resistivity of the paste after sintering and forming, has higher conversion efficiency of the battery, realizes effective substitution of nickel-coated copper, and can greatly reduce the paste cost. The nickel-coated copper micropowder takes ultrafine copper powder as a matrix, forms a nickel coating layer on the surface by chemical nickel plating, and prepares a clustered chelating agent with a multi-element phosphorus-nitrogen structure by substitution reaction of triethylenetetramine and active phosphoryl chloride of phenylthiophosphonyl dichloride. In the process of chemical nickel plating, the clustered chelating agent preferentially chelates and compounds with the surface of the activated copper powder, and forms a large number of clustered chelating sites on the surface. points, which capture the added nickel ions and fill them between the cluster structures. After being reduced by hydrazine, a nickel coating layer with interlaced cluster structures is formed. Then, under high-temperature roasting, the cluster structure is decomposed and carbonized, and a small amount of phosphorus and nitrogen doping is introduced into the surface nickel layer to improve the conductivity of the nickel coating layer. At the same time, the decomposition of the cluster structure forms a large number of nickel compound protrusions on the surface. These protrusions have a flat conical structure, and the doping improves the wear resistance of the nickel compound. The stability of the protrusion structure can be maintained during the grinding and blending process. The stable nickel compound protrusions increase the specific surface area, form a snap-in contact with the silver nanowires and nano-silver powder, increase the conduction path between the particles, and improve the conductivity of the slurry, which is beneficial to the conversion efficiency of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0024] Figure 1 This is an electron microscope image of the nickel-clad copper powder prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1, preparation of nickel-copper slurry on the back of TOPCon battery, the specific implementation process is as follows:
[0027] (1) Preparation of nickel-coated copper powder
[0028] Step A1: triethylenetetramine, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature of the reaction system is regulated to 10°C in an ice-water bath, 33kHz ultrasonic oscillation is applied, phenylthiophosphonic dichloride is slowly added over 30 minutes, and the reaction is continued at a constant temperature after the addition is complete. The total reaction time of phenylthiophosphonic dichloride is controlled to be 1.5 hours, wherein the amount ratio of phenylthiophosphonic dichloride, triethylenetetramine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 62 mmol: 10 mL: 60 mL. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water, the aqueous phase is removed and the solution is dried in vacuo to obtain a clustered chelating agent.
[0029] Step A2: Take copper powder and soak it in concentrated hydrochloric acid with a mass fraction of 37% for 5 minutes, prepare a stannous chloride aqueous solution, acidify it with hydrochloric acid to a pH value of 2, and the mass fraction of stannous chloride is 0.8%. Then, soak the pickled copper powder in the acidic stannous chloride solution for sensitization treatment for 15 minutes, and then soak it in a hydrazine solution with a mass fraction of 40% twice, and obtain activated copper powder after draining.
[0030] Step A3: Mix activated copper powder, clustered chelating agent, thiourea and ethanol solution, add nickel sulfate solution and mix, adjust the pH value to 10 with ammonia water, add hydrazine solution under 28kHz ultrasonic oscillation for 10 minutes, and then water bath at 70°C for 1.2 hours, wherein the amount ratio of activated copper powder, nickel sulfate, clustered chelating agent, thiourea, hydrazine solution and ethanol solution is 50g:16g:4.2g:10mg:80mL:500mL, the mass fraction of hydrazine solution is 40%, the mass fraction of ethanol solution is 50%, and the nickel sulfate solution is a saturated aqueous solution at room temperature. After the reaction, filter and wash the filter cake with water and dry it to obtain a precursor powder.
[0031] Step A4: Place the precursor powder in a calcination furnace, and roast it at 650±10℃ for 1.5h under a nitrogen atmosphere, then continue to heat it to 900±10℃ and roast it for 30min, controlling the heating rate during the heating process to be no higher than 10℃ / min, then cool it to 200℃ with the furnace, and control the cooling rate during the cooling process to be no higher than 30℃ / min, air-cool the material and break it up to obtain nickel-coated copper powder.
[0032] (2) Configure nickel-copper paste on the back of TOPCon cells
[0033] Ingredients: Prepare materials according to weight percentage, micron silver powder 40wt%, Brofos-Ag-W05 type micron silver powder of Bohuas Nano Technology (Ningbo) Co., Ltd. is used in the implementation process; nano silver powder 15wt%, Brofos-Ag-100 type nano silver powder of Bohuas Nano Technology (Ningbo) Co., Ltd. is used in the implementation process, and the average particle size is 100nm; silver nanowire 6wt%, Brofos-Ag-X040 type silver nanowire of Bohuas Nano Technology (Ningbo) Co., Ltd. is used in the implementation process, and the diameter is about 40nm; nickel-coated copper powder 25wt%, which is homemade in this embodiment; low-melting point glass powder 4.5wt%, FD76A type raw material of Anmi Micro-Nano New Materials (Guangzhou) Co., Ltd. is used in the implementation process, with a fineness of about 6000 mesh and a melting point of about 750°C; organic carrier 9.5wt%, dibutyl phthalate, tributyl citrate, xylene and pinene alcohol are premixed in a mass ratio of 1:1:1:0.5 during the implementation process.
[0034] Mixing: Add micron silver powder, nano silver powder, silver nanowire, nickel-coated copper powder and low-melting point glass powder into a mixer, premix at 1200 rpm for 5 minutes, add an organic carrier and mix, transfer to a three-roll grinder for grinding and mixing to obtain nickel-copper slurry for the back of the TOPCon battery.
[0035] Example 2, preparation of nickel-copper slurry on the back of TOPCon battery, the specific implementation process is as follows:
[0036] (1) Preparation of nickel-coated copper powder
[0037] Step A1: triethylenetetramine, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature of the reaction system is adjusted to 0°C in an ice-water bath, 25kHz ultrasonic oscillation is applied, phenylthiophosphonic dichloride is slowly added over 50 minutes, and the reaction is continued at a constant temperature after the addition is complete. The total reaction time of phenylthiophosphonic dichloride is controlled to be 2 hours, wherein the amount ratio of phenylthiophosphonic dichloride, triethylenetetramine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 55 mmol: 15 mL: 45 mL. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water, the aqueous phase is removed and vacuum dried to obtain a cluster chelating agent.
[0038] Step A2: Take the copper powder and soak it in 37% concentrated hydrochloric acid for 5 minutes, prepare a stannous chloride aqueous solution, acidify it with hydrochloric acid to a pH value of 3, and the mass fraction of stannous chloride is 0.6%. Then, soak the pickled copper powder in the acidic stannous chloride solution for 20 minutes, and then soak it in a 40% hydrazine solution twice, and then drain it to obtain the activated copper powder.
[0039] Step A3: Mix activated copper powder, clustered chelating agent, thiourea and ethanol solution, add nickel sulfate solution, adjust the pH value to 10 with ammonia water, add hydrazine solution under 28kHz ultrasonic oscillation for 15 minutes, and then water bath at 60°C for 1.6 hours, wherein the amount ratio of activated copper powder, nickel sulfate, clustered chelating agent, thiourea, hydrazine solution and ethanol solution is 50g:12g:3.5g:15mg:65mL:500mL, the mass fraction of hydrazine solution is 40%, the mass fraction of ethanol solution is 50%, and the nickel sulfate solution is a saturated aqueous solution at room temperature. After the reaction, filter and wash the filter cake with water and dry it to obtain a precursor powder.
[0040] Step A4: Place the precursor powder in a calcination furnace, and roast it at 650±10℃ for 2h under a nitrogen atmosphere. Then continue to heat it to 900±10℃ and roast it for 30min. Control the heating rate during the heating process to be no higher than 10℃ / min. Then cool it to 200℃ with the furnace. Control the cooling rate during the cooling process to be no higher than 30℃ / min. Air cool the material and break it up to obtain nickel-coated copper powder.
[0041] (2) Configure nickel-copper paste on the back of TOPCon cells
[0042] Ingredients: Prepare materials according to weight percentage, micron silver powder 75wt%, Brofos-Ag-W05 micron silver powder of Bohuas Nano Technology (Ningbo) Co., Ltd. is used in the implementation process; nano silver powder 5wt%, Brofos-Ag-80 nano silver powder of Bohuas Nano Technology (Ningbo) Co., Ltd. is used in the implementation process, and the average particle size is 80nm; silver nanowire 3wt%, Brofos-Ag-X030 silver nanowire of Bohuas Nano Technology (Ningbo) Co., Ltd. is used in the implementation process, and the diameter is about 30nm; nickel-coated copper powder 5wt%, which is homemade in this embodiment; low-melting point glass powder 2.5wt%, FD76A raw material of Anmi Micro-Nano New Materials (Guangzhou) Co., Ltd. is used in the implementation process, with a fineness of about 6000 mesh and a melting point of about 750°C; organic carrier 9.5wt%, dibutyl phthalate, tributyl citrate, xylene and pinene alcohol are premixed in a mass ratio of 1:1:1:0.5 during the implementation process.
[0043] Mixing: Add micron silver powder, nano silver powder, silver nanowire, nickel-coated copper powder and low-melting point glass powder into a mixer, premix at 1200 rpm for 5 minutes, add an organic carrier and mix, transfer to a three-roll grinder for grinding and mixing to obtain nickel-copper slurry for the back of the TOPCon battery.
[0044] Example 3, preparation of nickel-copper slurry on the back of TOPCon battery, the specific implementation process is as follows:
[0045] (1) Preparation of nickel-coated copper powder
[0046] Step A1: triethylenetetramine, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature of the reaction system is adjusted to 0°C in an ice-water bath, 33kHz ultrasonic oscillation is applied, phenylthiophosphonic dichloride is slowly added over 40 minutes, and the reaction is continued at a constant temperature after the addition is complete. The total reaction time of phenylthiophosphonic dichloride is controlled to be 1.8 hours, wherein the amount ratio of phenylthiophosphonic dichloride, triethylenetetramine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 58 mmol: 12 mL: 55 mL. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water, the aqueous phase is removed and vacuum dried to obtain a cluster chelating agent.
[0047] Step A2: Take copper powder and soak it in concentrated hydrochloric acid with a mass fraction of 37% for 5 minutes, prepare a stannous chloride aqueous solution, acidify it with hydrochloric acid to a pH value of 2, and the mass fraction of stannous chloride is 0.7%. Then, soak the pickled copper powder in the acidic stannous chloride solution for sensitization treatment for 18 minutes, and then soak it in a hydrazine solution with a mass fraction of 40% twice, and obtain activated copper powder after draining.
[0048] Step A3: Mix activated copper powder, clustered chelating agent, thiourea and ethanol solution, add nickel sulfate solution and mix, adjust the pH value to 10 with ammonia water, add hydrazine solution under 28kHz ultrasonic oscillation for 12 minutes, and then bathe in 65°C water for 1.4 hours, wherein the amount ratio of activated copper powder, nickel sulfate, clustered chelating agent, thiourea, hydrazine solution and ethanol solution is 50g:14g:4g:12mg:75mL:500mL, the mass fraction of hydrazine solution is 40%, the mass fraction of ethanol solution is 50%, the nickel sulfate solution is a saturated aqueous solution at room temperature, filter after the reaction, wash the filter cake with water and dry it to obtain a precursor powder.
[0049] Step A4: Place the precursor powder in a calcination furnace, and roast it at 650±10℃ for 1.7h under a nitrogen atmosphere. Then continue to heat it to 900±10℃ and roast it for 40min. Control the heating rate during the heating process to be no higher than 10℃ / min. Then cool it to 200℃ with the furnace. Control the cooling rate during the cooling process to be no higher than 30℃ / min. Air cool the material and break it up to obtain nickel-coated copper powder.
[0050] (2) Configure nickel-copper paste on the back of TOPCon cells
[0051] Ingredients: Prepare materials according to weight percentage, micron silver powder 55wt%, Brofos-Ag-W05 micron silver powder of Bohuas Nano Technology (Ningbo) Co., Ltd. is used in the implementation process; nano silver powder 10wt%, Brofos-Ag-50 nano silver powder of Bohuas Nano Technology (Ningbo) Co., Ltd. is used in the implementation process, and the average particle size is 50nm; silver nanowire 4wt%, Brofos-Ag-X020 silver nanowire of Bohuas Nano Technology (Ningbo) Co., Ltd. is used in the implementation process, and the diameter is about 20nm; nickel-coated copper powder 18wt%, which is homemade in this embodiment; low-melting point glass powder 3.5wt%, FD76A raw material of Anmi Micro-Nano New Materials (Guangzhou) Co., Ltd. is used in the implementation process, with a fineness of about 6000 mesh and a melting point of about 750°C; organic carrier 9.5wt%, dibutyl phthalate, tributyl citrate, xylene and pinene alcohol are premixed in a mass ratio of 1:1:1:0.5 during the implementation process.
[0052] Mixing: Add nano silver powder, silver nanowires, nickel-coated copper powder and low-melting point glass powder into a mixer, premix at 1200 rpm for 5 minutes, add an organic carrier and mix, transfer to a three-roll grinder for grinding and mixing to obtain nickel-copper slurry for the back of the TOPCon battery.
[0053] Comparative Example
[0054] This comparative example is a control example of Example 2, except that the homemade nickel-coated copper powder is replaced with W-5 nickel-coated copper powder provided by Huizhou Tenghui Technology Co., Ltd., with an average particle size of about 5 μm, and the rest of the implementation process is exactly the same.
[0055] The above back nickel-copper paste was screen-printed on the N-TOPCon cell silicon wafer by Baccini screen printing, sintered at 900°C, and the resistivity was tested by SZT-B four-probe tester, and the conversion efficiency was tested by PSS10-HEBerger tester. The specific test results are shown in the following table. At the same time, the nickel-coated copper powder in Example 2 was observed by electron microscope. Figure 1 As shown:
[0056]
[0057] It can be seen from the test results in the above table that the back nickel-copper slurry prepared in the embodiment has a lower resistivity after sintering, and the conversion efficiency reaches 26.02-26.95%, which greatly reduces the slurry cost.
[0058] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0059] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A nickel-copper paste for the back of a TOPCon battery. It is characterized in that The composition is composed of the following components according to weight percentage: 40-75wt% of micron silver powder, 5-15wt% of nano silver powder, 3-6wt% of silver nanowire, 5-25wt% of nickel-coated copper powder and 2.5-4.5wt% of low-melting-point glass powder, and the balance is an organic carrier; The nickel-coated copper powder is prepared by the following method: step A1: triethylenetetramine, triethylamine and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature of the reaction system is adjusted to 0-10°C in an ice-water bath, 25-33kHz ultrasonic oscillation is applied, phenylthiophosphonyl dichloride is slowly added to react for 1.5-2h, tetrahydrofuran is removed by rotary evaporation after the reaction is completed, the substrate is washed with water and separated, the water phase is removed and vacuum dried to obtain a cluster chelating agent; step A2: the copper powder is pickled in concentrated hydrochloric acid, then immersed in an acidic stannous chloride solution for sensitization treatment for 15-20min, then immersed in a hydrazine solution, and the activated copper is obtained after draining. Powder; Step A3: Mix the activated copper powder, clustered chelating agent, thiourea and ethanol solution, then add nickel sulfate solution to mix, adjust the pH value to 10 with ammonia water, add hydrazine solution under ultrasonic oscillation to react for 10-15 minutes, then water bath at 60-70°C for 1.2-1.6 hours, filter, wash and dry to obtain a precursor powder; Step A4: Place the precursor powder in a roasting furnace, roast at 650±10°C for 1.5-2 hours under a nitrogen atmosphere, then continue to heat to 900±10°C and roast for 30-50 minutes, then cool to 200°C with the furnace, air cool and break up the material to obtain nickel-coated copper micropowder.
2. A TOPCon battery back nickel-copper slurry according to claim 1, It is characterized in that The usage ratio of phenylphosphonothioic acid dichloride, triethylenetetramine, triethylamine and anhydrous tetrahydrofuran is 0.1 mol: 55-62 mmol: 10-15 mL: 45-60 mL.
3. A TOPCon battery back nickel-copper slurry according to claim 2, It is characterized in that The particle size of the copper powder is not higher than 10 μm, the pH value of the acidic stannous chloride solution is 2-3, and the mass fraction of stannous chloride is 0.6-0.8%.
4. A nickel-copper paste for the back side of a TOPCon battery according to claim 3, It is characterized in that In step A3, the amount ratio of activated copper powder, nickel sulfate, clustered chelating agent, thiourea, hydrazine solution and ethanol solution is 50g:12-16g:3.5-4.2g:10-15mg:65-80mL:500mL, the mass fraction of hydrazine solution is 40%, and the mass fraction of ethanol solution is 50%.
5. A TOPCon battery back nickel-copper paste according to claim 1, It is characterized in that The roasting heating rate is not higher than 10℃ / min, and the furnace cooling rate is not higher than 30℃ / min.
6. A TOPCon battery back nickel-copper paste according to claim 1, It is characterized in that The average particle size of the nano silver powder is 50-100 nm, and the diameter of the silver nanowire is 20-40 nm.
7. A TOPCon battery back nickel-copper paste according to claim 1, It is characterized in that The melting point of the low-melting-point glass powder is not higher than 800°C, and the fineness is not lower than 5000 mesh.
8. A method for preparing the nickel-copper slurry for the back side of a TOPCon battery according to any one of claims 1 to 7, It is characterized in that The specific operation is: pre-mix micron silver powder, nano silver powder, silver nanowire, nickel-coated copper powder and low-melting point glass powder in a high-speed mixer, add an organic carrier and grind and mix to obtain nickel-copper slurry on the back of the TOPCon battery.
Citation Information
Patent Citations
Sonochemistry preparation method allowing surface of copper powder to be coated with nickel and phosphorus alloy layer
CN103611932A
Nickel-coated copper clad metal powder and preparation method and application thereof
CN104801709A
Solar cell electrode slurry, preparation method, cell electrode and solar cell
CN105280265A
High-temperature-resistant silver-coated and nickel-coated copper conductive powder of core-shell structure and preparation method thereof
CN105598467A
Nickel-coated copper fine particle, manufacturing method of the same, conductive paste, and manufacturing method of conductive film
JP2007115497A