A phase-change ultra-slip drag-reducing multilayer composite material and its preparation method and application
By constructing a multi-level microstructure phase-change polymer layer and a slow-release layer on the surface of the ship, combined with a hydrophilic charged interpenetrating cross-linked layer, the problem of liquid escape during high-speed operation of the existing ultra-slippery liquid perfusion materials is solved, achieving Stable drag reduction effect and long life of the material.
Patent Information
- Application Number
- CN202411062199.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing ultra-slippery liquid-infused porous surface easily escapes when running at high speed, causing material failure and failing to effectively reduce the frictional resistance of waterborne and underwater ships.
A steam-heat-induced phase separation method is used to construct a phase change polymer layer with a multi-level microstructure, and a wrinkled polyamide sustained-release layer is generated through the interfacial polymerization reaction of acid chloride monomers and amine monomers, combined with hydrophilic charged interactions. Through the cross-linked layer, a stable phase-change super-slip drag-reducing multi-layer composite material is formed.
It achieves a stable phase change super-slip drag reduction effect, reduces the frictional resistance of water and underwater ships, increases the speed and extends the service life of the material.
Smart Images

Figure CN118577466B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a drag reduction material, in particular to a phase-change ultra-slip drag reduction multilayer composite material and a preparation method and application thereof, belonging to the technical field of marine drag reduction materials. Background Art
[0002] During the operation of ships and underwater vessels, the friction resistance reduces the speed and increases the energy consumption. Slippery liquid-infused porous surfaces (SLIPS) are a drag reduction technology that has attracted wide attention. SLIPS uses a lubricating liquid that is immiscible with water instead of airbags to fill the gaps in the rough structure to prevent the pinning effect of water droplets, making the surface smooth and having hydrophobic drag reduction properties. However, when running at high speeds, the infused liquid easily escapes and the material fails. Summary of the invention
[0003] The main purpose of the present invention is to provide a phase-change ultra-slip drag-reducing multilayer composite material and a preparation method thereof, so as to overcome the deficiencies in the prior art.
[0004] Another object of the present invention is to provide an application of the phase-change ultra-slippery drag-reducing multilayer composite material.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0006] The embodiment of the present invention provides a method for preparing a phase-change ultra-slip drag-reducing multilayer composite material, which comprises:
[0007] (1) coating a polymer solution on a substrate, exposing it to a water vapor bath, and constructing a phase change polymer layer with a multi-level microstructure by using a steam-thermal induced phase separation method;
[0008] (2) immersing the substrate / phase change polymer layer composite structure having a multi-level microstructure prepared in step (1) in an oil phase acyl chloride monomer solution, and then immersing it in a first mixed aqueous solution containing an amine monomer and cellulose, and heat treating it, thereby forming a wrinkled polyamide sustained-release layer on the phase change polymer layer;
[0009] (3) Coating a second mixed aqueous solution comprising a hydrophilic negatively charged polymer, a hydrophilic positively charged polymer, a hydrophilic homopolymer, a hydrophilic monomer and an ultraviolet light initiator on the surface of the substrate / phase change polymer layer with a multi-level microstructure / corrugated polyamide sustained-release layer composite structure prepared in step (2), and irradiating it with ultraviolet light to obtain a hydrophilic charged interpenetrating cross-linked layer, thereby obtaining a phase change ultra-slip drag-reducing multilayer composite material.
[0010] In some embodiments, step (1) of the preparation method specifically includes: applying the polymer solution on the surface of the substrate, exposing it to a water vapor bath with a relative humidity of 60-100% and a temperature of 0-60°C for 5s-1h to obtain the phase change polymer layer with a multi-level microstructure.
[0011] In some embodiments, step (2) of the preparation method specifically includes: immersing the substrate / phase change polymer layer composite structure having a multi-level microstructure in an oil-phase acyl chloride monomer solution for 30 seconds to 10 minutes, then immersing it in the first mixed aqueous solution for 30 seconds to 10 minutes, and heat treating it at 30 to 100° C. for 1 to 30 minutes to obtain the wrinkled polyamide sustained-release layer.
[0012] The embodiment of the present invention also provides a phase-change ultra-slip drag-reducing multi-layer composite material prepared by the aforementioned method.
[0013] In some embodiments, the phase-change ultra-slip drag-reducing multilayer composite material includes a phase-change polymer layer with a multi-level microstructure, a wrinkled polyamide sustained-release layer, and a hydrophilic charged interpenetrating cross-linked layer which are sequentially stacked in the thickness direction of the substrate.
[0014] The embodiment of the present invention also provides the application of the aforementioned phase-change ultra-lubricous drag-reducing multi-layer composite material in the field of drag reduction and speed increase.
[0015] Compared with the prior art, the beneficial effects of the present invention include:
[0016] The present invention reduces frictional resistance by strengthening the swinging and twisting of polymer chains through the synergistic phase change characteristics of the polymer layer and the anchoring effect of the multi-level microstructure, the sustained release characteristics of the wrinkled polyamide layer, and the swelling effect of the phase change material of the hydrophilic charged interpenetrating cross-linked layer. The advantages of the multiple layers are complementary and the multi-functional coupling is achieved to obtain a stable phase change ultra-slip drag reduction multi-layer composite material, which can achieve drag reduction and speed increase for water vessels, underwater ships, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 It is a schematic structural diagram of a phase-changing ultra-slip drag-reducing multilayer composite material in a typical embodiment of the present invention;
[0019] Figure 2 This is a surface SEM image of a substrate / phase change polymer layer having a multi-level microstructure prepared in Example 5 of the present invention;
[0020] Figure 3 This is a surface SEM image of the substrate / phase change polymer layer with a multi-level microstructure / corrugated polyamide sustained-release layer prepared in Example 5 of the present invention;
[0021] Figure 4 This is a surface SEM image of the substrate / phase change polymer layer with multi-level microstructure / corrugated polyamide sustained-release layer / hydrophilic charged interpenetrating cross-linked layer prepared in Example 5 of the present invention.
[0022] Figure numerals: 1-substrate, 2-phase change polymer layer with multi-level microstructure, 3-pleated polyamide sustained-release layer, 4-hydrophilic charged interpenetrating cross-linked layer. DETAILED DESCRIPTION
[0023] In view of the problems existing in the above-mentioned prior art, after long-term research and a large number of experiments, the inventors of this case proposed this technical solution, which mainly involves coating a polymer solution on the surface of a substrate, constructing a phase change polymer layer with a multi-level microstructure using a steam-thermal induced phase separation method; generating a wrinkled polyamide sustained-release layer through an interfacial polymerization reaction between acyl chloride monomers and amine monomers; and fully contacting and cross-linking with the composite aqueous solution to generate a hydrophilic charged interpenetrating cross-linked layer.
[0024] The technical solution, its implementation process and principle will be further explained as follows.
[0025] As one aspect of the technical solution of the present invention, it involves a method for preparing a phase-change ultra-slip drag-reducing multilayer composite material, comprising:
[0026] (1) coating a polymer solution on a substrate, exposing it to a water vapor bath, and constructing a phase change polymer layer with a multi-level microstructure by using a steam-thermal induced phase separation method;
[0027] (2) immersing the substrate / phase change polymer layer composite structure having a multi-level microstructure prepared in step (1) in an oil phase acyl chloride monomer solution, and then immersing it in a first mixed aqueous solution containing an amine monomer and cellulose, and heat treating it, thereby forming a wrinkled polyamide sustained-release layer on the phase change polymer layer;
[0028] (3) Coating a second mixed aqueous solution comprising a hydrophilic negatively charged polymer, a hydrophilic positively charged polymer, a hydrophilic homopolymer, a hydrophilic monomer and an ultraviolet light initiator on the surface of the substrate / phase change polymer layer with a multi-level microstructure / corrugated polyamide sustained-release layer composite structure prepared in step (2), and irradiating it with ultraviolet light to obtain a hydrophilic charged interpenetrating cross-linked layer, thereby obtaining a phase change ultra-slip drag-reducing multilayer composite material.
[0029] In some embodiments, step (1) specifically includes: adding the polymer into a mixed solvent and stirring to dissolve the polymer to form the polymer solution.
[0030] Furthermore, the stirring and dissolving is carried out at a temperature of 60 to 160° C. and for a time of 0.5 to 24 hours.
[0031] Furthermore, the concentration of the polymer in the polymer solution is 4-30wt%.
[0032] In some embodiments, step (1) specifically includes: applying the polymer solution on the surface of the substrate, exposing it to a water vapor bath with a relative humidity of 60-100% and a temperature of 0-60°C for 5s-1h, and using a steam-thermal induced phase separation method to obtain the phase change polymer layer with a multi-level microstructure. In this step, the temperature of the polymer solution is 60-160°C, and the temperature during the steam-induced phase separation is 0-60°C. There is a temperature gradient, which makes the polymer crystallization rate faster, that is, solid-solid phase separation occurs preferentially before liquid-liquid phase separation, thereby spontaneously forming a multi-level microstructure. Among them, a nanosphere structure with a diameter of 1-20nm is embedded on the surface of a microsphere structure with a diameter of 100-800µm to form a multi-level microstructure.
[0033] In some embodiments, step (2) specifically includes: immersing the substrate / phase change polymer layer composite structure having a multi-level microstructure in an oil phase acyl chloride monomer solution for 30 seconds to 10 minutes, then immersing it in the first mixed aqueous solution for 30 seconds to 10 minutes, and heat-treating it at 30 to 100° C. for 1 to 30 minutes to obtain the wrinkled polyamide sustained-release layer. The heat treatment can increase the cross-linking degree of the polyamide.
[0034] In some embodiments, in step (2), the first mixed aqueous solution includes 0.5-5 wt % of amine monomer and 0.01-2 wt % of cellulose.
[0035] Furthermore, the concentration of the acyl chloride monomer in the oil phase acyl chloride monomer solution is 0.1-5 wt %.
[0036] In some embodiments, in step (3), the second mixed aqueous solution includes 0.5-10 wt % of a hydrophilic negatively charged polymer, 0.5-10 wt % of a hydrophilic positively charged polymer, 0.5-10 wt % of a hydrophilic homopolymer, 0.5-10 wt % of a hydrophilic monomer and 0.1-2 wt % of an ultraviolet light initiator.
[0037] In some embodiments, step (3) specifically includes: brushing the second mixed aqueous solution on the surface of the composite structure of the substrate / phase change polymer layer with multi-level microstructure / corrugated polyamide sustained-release layer, and irradiating with an ultraviolet high-pressure mercury lamp with a wavelength of 185-365nm and a power of 100-1000W for 1s-60min to obtain the hydrophilic charged interpenetrating crosslinked layer. In this step, the double bonds of the hydrophilic monomers undergo free radical polymerization to generate a crosslinked polymer network, and form hydrogen bonds with the hydrophilic negatively charged polymer or the hydrophilic positively charged polymer or the hydrophilic homopolymer to generate a stable crosslinked polymer network.
[0038] As one of the more specific embodiments, the method for preparing the phase-change ultra-slip drag-reducing multilayer composite material may include the following steps:
[0039] (1) Add 4-30 wt% polymer to a mixed solvent, stir and dissolve at 60-160 °C for 0.5-24 h, quickly apply it on the surface of the substrate, expose it to a water vapor bath with a relative humidity of 60-100% and a temperature of 0-60 °C for 5 s-1 h, and construct a phase change polymer layer with a multi-level microstructure by using a steam-thermal induced phase separation method;
[0040] (2) immersing the substrate / phase change polymer layer having a multi-level microstructure prepared in step (1) in a 0.1-5 wt% oil phase acyl chloride monomer solution for 30 seconds to 10 minutes, removing the surface oil solution, and then immersing it in a first mixed aqueous solution consisting of 0.5-5 wt% amine monomer and 0.01-2 wt% cellulose for 30 seconds to 10 minutes, and heat treating at 30-100° C. for 1-30 minutes to form a wrinkled polyamide sustained-release layer on the phase change polymer layer;
[0041] (3) The surface of the substrate / phase change polymer layer with multi-level microstructure / pleated polyamide sustained-release layer composite material prepared in step (2) is coated with a second mixed aqueous solution consisting of 0.5-10wt% of a hydrophilic negatively charged polymer, 0.5-10wt% of a hydrophilic positively charged polymer, 0.5-10wt% of a hydrophilic homopolymer, 0.5-10wt% of a hydrophilic monomer and 0.1-2wt% of an ultraviolet light initiator, and irradiated with an ultraviolet high-pressure mercury lamp with a wavelength of 185-365nm and a power of 100-1000W for 1s-60min to obtain a hydrophilic charged interpenetrating cross-linked layer, thereby obtaining the phase change ultra-slip drag-reducing multilayer composite material.
[0042] In some embodiments, in step (1), the polymer may include any one or more combinations of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylonitrile, polyethersulfone, etc., but is not limited thereto.
[0043] In some embodiments, in step (1), the mixed solvent includes a combination of at least one of dimethyl sulfoxide, N-methylpyrrolidone, ethanol, and N,N'-dimethylformamide and a phase change material. The mixed solvent used in the present invention must contain a phase change material (dimethyl sulfone or diphenyl sulfone). The phase change material is compounded with other polar solvents to form a mixed solvent, and the melting point will be reduced, changing from a solid phase to a liquid phase. The phase change process will change the surface properties of the composite material, thereby affecting the drag reduction performance.
[0044] Furthermore, the content of the phase change material in the mixed solvent is 30-99wt%.
[0045] Furthermore, the phase change material may be at least one of dimethyl sulfone and diphenyl sulfone, but is not limited thereto.
[0046] In some embodiments, in step (1), the substrate may include at least any one of glass, plastic, metal plate, etc., but is not limited thereto.
[0047] In some embodiments, in step (2), the oil phase acyl chloride monomer solution includes acyl chloride monomers and an oil phase solvent, and the acyl chloride monomers include any one or more combinations of trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride and phthaloyl chloride, but are not limited thereto.
[0048] Furthermore, the oil phase solvent may include any one or more combinations of n-hexane, cyclohexane, toluene, etc., but is not limited thereto.
[0049] In some embodiments, in step (2), the cellulose may include any one or more combinations of carboxyl cellulose, hydroxy cellulose, sulfonate cellulose, and phosphate cellulose, but is not limited thereto.
[0050] In some embodiments, in step (2), the amine monomer may include any one or more combinations of m-phenylenediamine, p-phenylenediamine, and dopamine, but is not limited thereto.
[0051] In some embodiments, in step (3), the hydrophilic negatively charged polymer may include any one or more combinations of polyacrylic acid, sodium polybenzene sulfonate, and polyglutamic acid, but is not limited thereto.
[0052] In some embodiments, in step (3), the hydrophilic positively charged polymer may include any one or more combinations of polyethyleneimine, polyacrylamide, and polymethacryloyloxyethyltrimethylammonium chloride, but is not limited thereto.
[0053] In some embodiments, in step (3), the hydrophilic homopolymer may include any one or more combinations of polyethylene oxide, polyvinyl pyrrolidone and polyvinyl alcohol, but is not limited thereto.
[0054] In some embodiments, in step (3), the hydrophilic monomer may include any one or more combinations of polyethylene glycol diacrylate and polytetraethylene glycol diacrylate, etc., but is not limited thereto.
[0055] In some embodiments, in step (3), the ultraviolet light initiator may include any one or more combinations of benzophenone, 2-hydroxy-2-methyl-1-phenylpropanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, etc., but is not limited thereto.
[0056] As another aspect of the technical solution of the present invention, it also relates to a phase-change ultra-slip drag-reducing multi-layer composite material prepared by the aforementioned method.
[0057] See also Figure 1 As shown, in some preferred embodiments, the phase-change ultra-slip drag-reducing multilayer composite material includes three layers stacked in sequence from bottom to top in the thickness direction of the substrate 1, namely: a phase-change polymer layer 2 with a multi-level microstructure, a wrinkled polyamide sustained-release layer 3, and a hydrophilic charged interpenetrating cross-linked layer 4.
[0058] Furthermore, the multi-level microstructure in the phase-change polymer layer with a multi-level microstructure includes a micron ball structure and a nano ball structure embedded on the surface of the micron ball structure; the diameter of the micron ball structure is 100-800µm, and the diameter of the nano ball structure is 1-20nm. The polymer layer with a multi-level microstructure of the present invention contains a large amount of phase change material, which dissolves at high temperature and solidifies at room temperature, has good water solubility, and can dissolve highly polar polymers. After contacting with water, the solid phase dimethyl sulfone gradually dissolves and diffuses from the multi-level micropores to the wrinkled polyamide layer, and is slowly released to the hydrophilic charged interpenetrating cross-linked layer, so that the cross-linked layer swells moderately to form a micro liquid surface. Furthermore, the micro liquid surface and the various polymer chains of the hydrophilic charged interpenetrating cross-linked layer form an ultra-slippery surface, which reduces the friction resistance between water molecules and the surface, thereby playing a stable drag reduction role.
[0059] The phase-change polymer layer with a multi-level microstructure of the present invention is mainly used to store phase-change materials, and its multi-level microstructure is mainly used to anchor the wrinkled polyamide layer and the hydrophilic charged interpenetrating cross-linking layer.
[0060] Furthermore, the corrugated polyamide sustained-release layer has a corrugated structure. The corrugated polyamide sustained-release layer of the present invention mainly plays a sustained-release role and inhibits the loss of the phase change material, and its corrugated structure mainly regulates the dissolution and diffusion characteristics of the phase change material.
[0061] Furthermore, the hydrophilic charged interpenetrating crosslinked layer has a flat surface on the side away from the wrinkled polyamide sustained-release layer. The hydrophilic charged interpenetrating crosslinked layer of the present invention strengthens the swing and twisting of the polymer chain through the swelling action of the phase change material to reduce the friction resistance, and its charged interpenetrating property maintains the mechanical stability and long life of the hydrophilic crosslinked layer.
[0062] Furthermore, the drag reduction rate of the phase-change ultra-lubricant drag reduction multi-layer composite material is 18.1% to 28.4%.
[0063] In summary, the phase change characteristics of the synergistic polymer layer of the present invention, the anchoring effect of the multi-level microstructure, the sustained release characteristics of the wrinkled polyamide layer, and the swelling effect of the hydrophilic charged interpenetrating cross-linked layer through the phase change material strengthen the swinging and twisting of the polymer chains to reduce frictional resistance, thereby obtaining a stable phase change ultra-slip drag-reducing multilayer composite material, which can achieve drag reduction and speed increase for water vessels, underwater ships, etc.
[0064] Another aspect of the embodiments of the present invention further provides an application of the aforementioned phase-change ultra-lubricous drag-reducing multilayer composite material. Specifically, the multilayer composite material can be used to achieve drag reduction and speed increase of water vessels, underwater ships, etc.
[0065] The whole process is described in detail below through several embodiments and drawings, but the scope of the claims of the present invention is not limited by these embodiments. At the same time, the embodiments only provide some conditions for achieving this purpose, but it does not mean that these conditions must be met to achieve this purpose. All variations associated with or derived from the contents disclosed in the present invention are considered to be within the scope of protection of the present invention.
[0066] Example 1
[0067] (1) 4 wt% of a polymer was added to a mixed solvent, stirred and dissolved at 60°C for 0.5 h, and quickly coated on the surface of a substrate. The polymer was polyvinylidene fluoride, the mixed solvent was 30 wt% of dimethyl sulfone and 70 wt% of N-methylpyrrolidone, and the substrate was a glass sheet. The polymer was polyvinylidene fluoride, the mixed solvent was 30 wt% of dimethyl sulfone and 70 wt% of N-methylpyrrolidone, and the substrate was a glass sheet.
[0068] (2) immersing the substrate / phase change polymer layer composite material with a multi-level microstructure prepared in step (1) in a 5wt% oil-phase acyl chloride monomer solution for 10 minutes, removing the surface oil solution and then immersing it in a first mixed aqueous solution consisting of 0.5wt% amine substance and 0.01wt% cellulose for 30 seconds, and heat treating at 30°C for 30 minutes to form a wrinkled polyamide sustained-release layer on the phase change polymer layer with a multi-level microstructure; the cellulose is carboxycellulose, the amine monomer is m-phenylenediamine, the acyl chloride monomer is trimesoyl chloride, and the oil-phase solvent is n-hexane;
[0069] (3) The surface of the substrate / phase change polymer layer with multi-level microstructure / corrugated polyamide sustained-release layer composite material prepared in step (2) is coated with a second mixed aqueous solution consisting of 0.5wt% of a hydrophilic negatively charged polymer, 10wt% of a hydrophilic positively charged polymer, 0.5wt% of a hydrophilic homopolymer, 10wt% of a hydrophilic monomer and 2wt% of an ultraviolet light initiator, and irradiated with an ultraviolet high-pressure mercury lamp with a wavelength of 365nm and a power of 1000W for 1s to obtain a hydrophilic charged interpenetrating cross-linked layer, thereby obtaining a phase change ultra-slip drag-reducing multilayer composite material; the hydrophilic negatively charged polymer is polyacrylic acid, the hydrophilic positively charged polymer is polyethyleneimine, the hydrophilic homopolymer is polyethylene oxide, the hydrophilic monomer is polyethylene glycol diacrylate, and the ultraviolet light initiator is benzophenone.
[0070] After a 24-hour water tunnel test, the drag reduction rate of the phase-change ultra-lubricous drag-reducing multilayer composite material prepared in this embodiment is 18.1%.
[0071] Example 2
[0072] (1) 30 wt% of a polymer was added to a mixed solvent, stirred and dissolved at 160°C for 24 h, quickly coated on the surface of a substrate, exposed to a water vapor bath at a relative humidity of 100% and a temperature of 60°C for 1 h, and a phase change polymer layer with a multi-level microstructure was constructed by a steam-thermal induced phase separation method; the polymer was polyvinylidene fluoride-hexafluoropropylene copolymer, the mixed solvent was 99 wt% dimethyl sulfone and 1 wt% ethanol, and the substrate was a plastic plate;
[0073] (2) immersing the substrate / phase change polymer layer composite material with a multi-level microstructure prepared in step (1) in a 0.1wt% oil-phase acyl chloride monomer solution for 30 seconds, removing the surface oil solution, and then immersing it in a first mixed aqueous solution consisting of 5wt% amine substance and 2wt% cellulose for 10 minutes, and heat treating it at 100°C for 1 minute to generate a wrinkled polyamide sustained-release layer on the phase change polymer layer with a multi-level microstructure; the cellulose is hydroxy cellulose, the amine monomer is p-phenylenediamine, the acyl chloride monomer is terephthaloyl chloride, and the oil phase solvent is cyclohexane;
[0074] (3) A second mixed aqueous solution consisting of 10 wt % of a hydrophilic negatively charged polymer, 0.5 wt % of a hydrophilic positively charged polymer, 10 wt % of a hydrophilic homopolymer, 0.5 wt % of a hydrophilic monomer and 0.1 wt % of an ultraviolet light initiator is applied to the surface of the substrate / phase change polymer layer with a multi-level microstructure / corrugated polyamide sustained-release layer composite material prepared in step (2), and irradiated with an ultraviolet high-pressure mercury lamp with a wavelength of 365 nm and a power of 100 W for 60 min to obtain a hydrophilic charged interpenetrating cross-linked layer, thereby obtaining a phase change ultra-slip drag-reducing multilayer composite material; the hydrophilic negatively charged polymer is sodium polybenzene sulfonate, the hydrophilic positively charged polymer is polyacrylamide, the hydrophilic homopolymer is polyvinyl pyrrolidone, the hydrophilic monomer is polyethylene glycol diacrylate, and the ultraviolet light initiator is 2-hydroxy-2-methyl-1-phenylacetone.
[0075] After a 24-hour water tunnel test, the drag reduction rate of the phase-change ultra-lubricous drag-reducing multilayer composite material prepared in this embodiment is 21.2%.
[0076] Example 3
[0077] (1) 20 wt% of a polymer was added to a mixed solvent, stirred and dissolved at 110°C for 2 h, quickly coated on the surface of a substrate, and exposed to a water vapor bath at a relative humidity of 80% and a temperature of 10°C for 5 min, and a phase change polymer layer with a multi-level microstructure was constructed by a steam-thermal induced phase separation method; the polymer was polyacrylonitrile, the mixed solvent was 90 wt% of dimethyl sulfone and 10 wt% of dimethyl sulfoxide, and the substrate was a steel plate;
[0078] (2) immersing the substrate / phase change polymer layer composite material with a multi-level microstructure prepared in step (1) in a 3 wt % oil phase acyl chloride monomer solution for 3 min, removing the surface oil solution and then immersing it in a first mixed aqueous solution consisting of 1 wt % amine substance and 0.1 wt % cellulose for 2 min, and heat treating at 80° C. for 10 min to form a wrinkled polyamide sustained-release layer on the phase change polymer layer with a multi-level microstructure; the cellulose is sulfonate cellulose, the amine monomer is dopamine, the acyl chloride monomer is isophthaloyl chloride, and the oil phase solvent is toluene;
[0079] (3) A second mixed aqueous solution consisting of 3 wt % of a hydrophilic negatively charged polymer, 4 wt % of a hydrophilic positively charged polymer, 1 wt % of a hydrophilic homopolymer, 5 wt % of a hydrophilic monomer and 1 wt % of an ultraviolet light initiator is applied to the surface of the substrate / phase change polymer layer with a multi-level microstructure / corrugated polyamide sustained-release layer composite material prepared in step (2), and irradiated with an ultraviolet high-pressure mercury lamp with a wavelength of 365 nm and a power of 800 W for 2 min to obtain a hydrophilic charged interpenetrating cross-linked layer, thereby obtaining a phase change ultra-slip drag-reducing multilayer composite material; the hydrophilic negatively charged polymer is polyglutamic acid, the hydrophilic positively charged polymer is polymethacryloyloxyethyltrimethylammonium chloride, the hydrophilic homopolymer is polyvinyl alcohol, the hydrophilic monomer is polyethylene glycol diacrylate, and the ultraviolet light initiator is 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone.
[0080] After a 24-hour water tunnel test, the drag reduction rate of the phase-change ultra-lubricous drag-reducing multilayer composite material prepared in this embodiment is 19.4%.
[0081] Example 4
[0082] (1) 15 wt% of a polymer was added to a mixed solvent, stirred and dissolved at 150°C for 6 h, quickly coated on the surface of a substrate, exposed to a water vapor bath at a relative humidity of 70% and a temperature of 30°C for 10 min, and a phase change polymer layer with a multi-level microstructure was constructed by a steam-thermal induced phase separation method; the polymer was polyethersulfone, the mixed solvent was 80 wt% of dimethylsulfone and 20 wt% of N,N'-dimethylformamide, and the substrate was a steel plate;
[0083] (2) immersing the substrate / phase change polymer layer composite material with a multi-level microstructure prepared in step (1) in a 3.5wt% oil-phase acyl chloride monomer solution for 8 minutes, removing the surface oil solution, and then immersing it in a first mixed aqueous solution consisting of 3wt% amine substance and 0.05wt% cellulose for 6 minutes, and heat treating at 90°C for 15 minutes to form a wrinkled polyamide sustained-release layer on the phase change polymer layer with a multi-level microstructure; the cellulose is phosphate cellulose, the amine monomer is m-phenylenediamine, the acyl chloride monomer is phthaloyl chloride, and the oil phase solvent is 50wt% n-hexane and 50wt% toluene;
[0084] (3) A second mixed aqueous solution consisting of 5 wt% of a hydrophilic negatively charged polymer, 1 wt% of a hydrophilic positively charged polymer, 1 wt% of a hydrophilic homopolymer, 3 wt% of a hydrophilic monomer and 0.5 wt% of an ultraviolet light initiator is applied to the surface of the substrate / phase change polymer layer with a multi-level microstructure / corrugated polyamide sustained-release layer composite material prepared in step (2), and irradiated with an ultraviolet high-pressure mercury lamp with a wavelength of 365 nm and a power of 300 W for 10 min to obtain a hydrophilic charged interpenetrating cross-linked layer, thereby obtaining a phase change ultra-slip drag-reducing multilayer composite material; the hydrophilic negatively charged polymer is polyacrylic acid, the hydrophilic positively charged polymer is polyethyleneimine, the hydrophilic homopolymer is polyethylene oxide, the hydrophilic monomer is polyethylene glycol diacrylate, and the ultraviolet light initiator is benzophenone.
[0085] After a 24-hour water tunnel test, the drag reduction rate of the phase-change ultra-lubricous drag-reducing multilayer composite material prepared in this embodiment is 23.2%.
[0086] Example 5
[0087] (1) 8 wt% of polymer was added to a mixed solvent, stirred and dissolved at 100°C for 8 h, quickly coated on the surface of a substrate, exposed in a water vapor bath at a relative humidity of 90% and a temperature of 15°C for 15 min, and a phase change polymer layer with a multi-level microstructure was constructed by a steam-thermal induced phase separation method; the polymer was polyvinylidene fluoride, the mixed solvent was 70 wt% dimethyl sulfone and 30 wt% dimethyl sulfoxide, and the substrate was a steel plate; the surface SEM image of the substrate / phase change polymer layer with a multi-level microstructure prepared in this step is shown in FIG. Figure 2 As shown, the multi-level microstructure includes a micron ball structure and a nano ball structure embedded on the surface of the micron ball structure;
[0088] (2) The substrate / phase change polymer layer composite material with a multi-level microstructure prepared in step (1) is immersed in a 2.5wt% oil-phase acyl chloride monomer solution for 8 minutes, and after removing the surface oil solution, it is immersed in a first mixed aqueous solution consisting of 2wt% amine substance and 0.06wt% cellulose for 7 minutes, and heat-treated at 70°C for 12 minutes to generate a wrinkled polyamide sustained-release layer on the phase change polymer layer with a multi-level microstructure; the cellulose is carboxyl cellulose, the amine monomer is 60wt% m-phenylenediamine and 40wt% dopamine, the acyl chloride monomer is trimesoyl chloride, and the oil phase solvent is n-hexane; the surface SEM image of the substrate / phase change polymer layer with a multi-level microstructure / wrinkled polyamide sustained-release layer prepared in this step is as shown in FIG. Figure 3 As shown;
[0089] (3) A second mixed aqueous solution consisting of 4 wt % of a hydrophilic negatively charged polymer, 2 wt % of a hydrophilic positively charged polymer, 2 wt % of a hydrophilic homopolymer, 4 wt % of a hydrophilic monomer and 1 wt % of an ultraviolet light initiator is applied to the surface of the substrate / phase change polymer layer with a multi-level microstructure / corrugated polyamide sustained-release layer composite material prepared in step (2), and irradiated with an ultraviolet high-pressure mercury lamp at a wavelength of 365 nm and a power of 400 W for 8 min to obtain a hydrophilic charged interpenetrating cross-linked layer, thereby obtaining a phase change ultra-slip drag-reducing multilayer composite material; the hydrophilic negatively charged polymer is polyacrylic acid, the hydrophilic positively charged polymer is polyethyleneimine, the hydrophilic homopolymer is polyvinyl pyrrolidone, the hydrophilic monomer is polyethylene glycol diacrylate, and the ultraviolet light initiator is 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone. The surface SEM image of the phase-change ultra-slip drag-reducing multilayer composite material prepared in this embodiment, namely the substrate / phase-change polymer layer with multi-level microstructure / corrugated polyamide sustained-release layer / hydrophilic charged interpenetrating cross-linked layer is shown in FIG. Figure 4 shown.
[0090] After a 24-hour water tunnel test, the drag reduction rate of the phase-change ultra-lubricous drag-reducing multilayer composite material prepared in this embodiment is 28.4%.
[0091] Comparative Example 1
[0092] This control example is basically the same as Example 5, except that a phase change polymer layer with a multi-level microstructure is not constructed. Due to the lack of a phase change polymer layer, there is no diffusion and sustained release of the phase change material to the wrinkled polyamide layer and the hydrophilic charged interpenetrating cross-linked layer, that is, it is impossible to use the micro-liquid surface and the polymer chain to form an ultra-slip drag reduction surface. Lacking the anchoring effect of the phase change polymer layer with a multi-level microstructure, the wrinkled polyamide layer and the hydrophilic charged interpenetrating cross-linked layer are easily damaged and fall off, and have a short service life. After 12 hours of water tunnel testing, the drag reduction rate of the composite material obtained in this control example was -7.6%, that is, the drag increase rate was 7.6%; after 24 hours of water tunnel testing, the wrinkled polyamide layer and the hydrophilic charged interpenetrating cross-linked layer had completely fallen off, and the material failed.
[0093] Comparative Example 2
[0094] This control example is basically the same as Example 5, except that: in step (1), the exposure in the water vapor bath is reduced from 15 min to 0 min, and the prepared phase change polymer layer does not have a multi-level microstructure. Lacking the anchoring effect of the multi-level microstructure, the wrinkled polyamide layer and the hydrophilic charged interpenetrating cross-linked layer are easily damaged and fall off, and the phase change material directly dissolves in water to form macropores, thereby increasing the resistance. After 24 hours of water tunnel testing, the drag reduction rate of the composite material obtained in this control example was -10.5%, that is, the drag increase rate was 10.5%. The wrinkled polyamide layer and the hydrophilic charged interpenetrating cross-linked layer had completely fallen off, and the material failed.
[0095] Comparative Example 3
[0096] This control example is basically the same as Example 5, except that no wrinkled polyamide sustained-release layer is constructed. The phase change material in the phase change polymer layer with a multi-level microstructure diffuses rapidly into the hydrophilic charged interpenetrating cross-linked layer, which can temporarily improve the drag reduction effect, but the phase change material is lost quickly and has a short service life. After a 0.5h water tunnel test, the drag reduction rate of the composite material obtained in this control example was 14.1%; after a 24h water tunnel test, the drag reduction rate of the composite material was -7.8%, that is, the drag increase rate was 7.8%.
[0097] Comparative Example 4
[0098] This control example is basically the same as Example 5, except that: in step (2), the cellulose concentration is reduced from 0.06wt% cellulose to 0wt%, and the prepared polyamide sustained-release layer does not have a wrinkled structure. The smooth polyamide layer has a higher density, which hinders the diffusion and sustained release of the phase change material and inhibits the formation of an ultra-slip drag-reducing surface. After a 24-hour water tunnel test, the drag reduction rate of the composite material obtained in this control example is -3.1%, that is, the drag increase rate is 3.1%.
[0099] Comparative Example 5
[0100] This control example is basically the same as Example 5, except that: no hydrophilic charged interpenetrating cross-linking layer is constructed. The hydrophilic charged interpenetrating cross-linking layer can adapt to the external flow field pressure through the swing and twist of the polymer chain, effectively suppress the pressure pulsation, and absorb the kinetic energy of the external flow field acting on the coating, so that the friction resistance is reduced. Therefore, when the hydrophilic charged interpenetrating cross-linking layer is missing, after 24 hours of water tunnel testing, the drag reduction rate of the composite material obtained in this control example is -9.2%, that is, the drag increase rate is 9.2%.
[0101] Comparative Example 6
[0102] This control example is basically the same as Example 5, except that the hydrophilic cross-linked layer does not have the property of charge interpenetration, that is, it only contains hydrophilic positively charged polymers or hydrophilic negatively charged polymers. There is a strong electrostatic interaction between the positively charged polymer and the negatively charged polymer, which maintains the mechanical stability and long life of the hydrophilic cross-linked layer. After 0.5h of water tunnel testing, the drag reduction rate of the composite material obtained in this control example is 5.2%; after 24h of water tunnel testing, the drag reduction rate of the composite material is -8.4%, that is, the drag increase rate is 8.4%.
[0103] In addition, the inventors of this case also conducted experiments with other raw materials and conditions listed in this specification with reference to the methods of Examples 1 to 5, and also produced a stable phase-change ultra-slip drag-reducing multilayer composite material.
[0104] It should be understood that the above are only specific application examples of the present invention and do not constitute any limitation on the protection scope of the present invention. Any technical solution formed by equivalent transformation or equivalent replacement falls within the protection scope of the present invention.
Claims
1. A method for preparing a phase-change ultra-slip drag-reducing multilayer composite material, characterized in that: include: (1) adding a polymer to a mixed solvent and stirring to dissolve the polymer solution, wherein the mixed solvent is a combination of at least one of dimethyl sulfoxide, N-methylpyrrolidone, ethanol, and N,N'-dimethylformamide and a phase change material, wherein the content of the phase change material in the mixed solvent is 30-99 wt %; and the phase change material is at least one of dimethyl sulfone and diphenyl sulfone; coating the polymer solution on a substrate, exposing the substrate to a water vapor bath, and constructing a phase change polymer layer with a multi-level microstructure by a steam-thermal induced phase separation method; (2) immersing the substrate / phase change polymer layer composite structure having a multi-level microstructure prepared in step (1) in an oil phase acyl chloride monomer solution, and then immersing it in a first mixed aqueous solution containing an amine monomer and cellulose, and heat treating it, thereby forming a wrinkled polyamide sustained-release layer on the phase change polymer layer; (3) A second mixed aqueous solution comprising a hydrophilic negatively charged polymer, a hydrophilic positively charged polymer, a hydrophilic homopolymer, a hydrophilic monomer and an ultraviolet light initiator is applied to the surface of the substrate / phase change polymer layer with a multi-level microstructure / corrugated polyamide sustained-release layer composite structure prepared in step (2), and irradiated with ultraviolet light to obtain a hydrophilic charged interpenetrating cross-linked layer, thereby obtaining a phase change ultra-slip drag reduction multilayer composite material, wherein the hydrophilic negatively charged polymer is selected from any one or more of a combination of polyacrylic acid, sodium polybenzene sulfonate and polyglutamic acid, the hydrophilic positively charged polymer is selected from any one or more of a combination of polyethyleneimine, polyacrylamide and polymethacryloyloxyethyltrimethylammonium chloride, the hydrophilic homopolymer is selected from any one or more of a combination of polyethylene oxide, polyvinyl pyrrolidone and polyvinyl alcohol, and the hydrophilic monomer is selected from any one or a combination of two of polyethylene glycol diacrylate and polytetraethylene glycol diacrylate.
2. The preparation method according to claim 1, characterized in that: Step (1) specifically comprises: applying the polymer solution on the surface of the substrate, exposing it to a water vapor bath with a relative humidity of 60-100% and a temperature of 0-60° C. for 5 seconds to an hour, so as to obtain the phase change polymer layer with a multi-level microstructure.
3. The preparation method according to claim 2, characterized in that: In step (1), the polymer includes any one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylonitrile, and polyether sulfone; and / or, in step (1), the concentration of the polymer in the polymer solution is 4-30wt%; And / or, in step (1), the stirring and dissolving is performed at a temperature of 60 to 160° C. and for a time of 0.5 to 24 h; And / or, in step (1), the substrate includes at least any one of glass, plastic, and metal plate.
4. The preparation method according to claim 3, characterized in that: Step (2) specifically comprises: immersing the substrate / phase change polymer layer composite structure having a multi-level microstructure in an oil phase acyl chloride monomer solution for 30 seconds to 10 minutes, then immersing it in the first mixed aqueous solution for 30 seconds to 10 minutes, and heat treating it at 30 to 100° C. for 1 to 30 minutes to obtain the wrinkled polyamide sustained-release layer.
5. The preparation method according to claim 1 or 4, characterized in that: In step (2), the oil phase acyl chloride monomer solution comprises an acyl chloride monomer and an oil phase solvent, wherein the acyl chloride monomer comprises any one or more of trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride and phthaloyl chloride; and the oil phase solvent comprises any one or more of n-hexane, cyclohexane and toluene. and / or, in step (2), the concentration of the acyl chloride monomer in the oil phase acyl chloride monomer solution is 0.1-5 wt %; And / or, in step (2), the first mixed aqueous solution comprises 0.5-5 wt % of amine monomer and 0.01-2 wt % of cellulose; And / or, in step (2), the amine monomer includes any one or more combinations of m-phenylenediamine, p-phenylenediamine and dopamine; And / or, in step (2), the cellulose includes any one or more combinations of carboxyl cellulose, hydroxy cellulose, sulfonate cellulose and phosphate cellulose.
6. The preparation method according to claim 1, characterized in that: In step (3), the second mixed aqueous solution comprises 0.5-10 wt % of a hydrophilic negatively charged polymer, 0.5-10 wt % of a hydrophilic positively charged polymer, 0.5-10 wt % of a hydrophilic homopolymer, 0.5-10 wt % of a hydrophilic monomer and 0.1-2 wt % of an ultraviolet light initiator; And / or, in step (3), the ultraviolet light initiator includes any one or more combinations of benzophenone, 2-hydroxy-2-methyl-1-phenylpropanone, and 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone.
7. The preparation method according to claim 1, characterized in that: Step (3) specifically comprises: applying a second mixed aqueous solution on the surface of the composite structure of the substrate / phase change polymer layer with a multi-level microstructure / corrugated polyamide sustained-release layer, and irradiating the surface with an ultraviolet high-pressure mercury lamp with a wavelength of 185-365 nm and a power of 100-1000 W for 1 second to 60 minutes to obtain the hydrophilic charged interpenetrating cross-linked layer.
8. The phase-change ultra-slip drag-reducing multilayer composite material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The phase-change ultra-slip drag-reducing multi-layer composite material comprises a phase-change polymer layer with a multi-level microstructure, a wrinkled polyamide sustained-release layer, and a hydrophilic charged interpenetrating cross-linked layer which are sequentially stacked in the thickness direction of the substrate.
9. The phase-change ultra-slip drag-reducing multi-layer composite material according to claim 8, characterized in that: The multi-level microstructure in the phase-change polymer layer having a multi-level microstructure includes a micron ball structure and a nano ball structure embedded on the surface of the micron ball structure; the diameter of the micron ball structure is 100-800 μm, and the diameter of the nano ball structure is 1-20 nm; And / or, the corrugated polyamide sustained-release layer has a corrugated structure; And / or, the side of the hydrophilic charged interpenetrating cross-linked layer away from the wrinkled polyamide sustained-release layer has a flat surface; And / or, the drag reduction rate of the phase-change ultra-lubricous drag reduction multi-layer composite material is 18.1% to 28.4%.
10. Application of the phase-change ultra-lubricating drag-reducing multilayer composite material according to claim 8 or 9 in the field of drag reduction and speed increase.
Citation Information
Patent Citations
Copolymers and oil- and water-repellent compositions containing them
WO2001053366A1
Block copolymers grafted to porous polymeric substrate
WO2023248020A1