Tire tread composition with low rolling resistance and low VOCs emission, preparation method, and tire

By using high content of white carbon black and new silane coupling agents in tires, the VOCs emission and rolling resistance problems in the tire industry are solved, the goal of low rolling resistance green tires is achieved, and the workshop emissions and heat generation performance are significantly reduced.

CN118580580BActive Publication Date: 2024-11-19DOUBLE COIN GRP JIANGSU TIRE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411034482.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

There are high VOCs emissions and rolling resistance problems in the existing tire products industry, especially when using white carbon black silane coupling agent, which leads to an increase in environmental pressure and is difficult to meet the requirements of low rolling resistance green tires.

Method used

High content of white carbon black combined with new silane coupling agent is used to adjust the rubber formula and vulcanization process to reduce VOCs emissions and heat generation performance, and improve the rolling resistance performance of the tire.

Benefits of technology

It has achieved an 80% reduction in VOCs emissions, meets the use requirements of low-roll resistance green tires, and improves the physical and mechanical properties of the tires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to a tire tread composition with low rolling resistance and low VOCs emission, a preparation method, and a tire. The tire tread composition includes the following components in parts by weight: 100 parts of natural rubber, 5-20 parts of carbon black, 20-50 parts of white carbon black, 2-5 parts of coupling agent, 3-5 parts of zinc oxide, 1-3 parts of stearic acid, 2-5 parts of antioxidant, 1-2 parts of sulfur, 1-4 parts of accelerator, and 0.1-0.5 parts of anti-scorch agent; the coupling agent includes 3-mercaptopropylethoxybis(propyl-hexapropoxy)siloxane. Compared with the prior art, the present invention uses high-content white carbon black and a new silane coupling agent at the same time, so that the mechanical properties of the rubber meet the requirements for tire use, the heat generation performance decreases, and the VOCs emission in the workshop can be reduced by about 80%, which can meet the use requirements of low rolling resistance green tires.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tire preparation, and in particular to a tire tread composition with low rolling resistance and low VOCs emission, a preparation method and a tire. Background Art

[0002] For the tire product industry, the formal implementation of the "Emission Standards for Pollutants from Rubber Products Industry" requires that the emission concentration limit of waste gas from rubber refining and vulcanization equipment of tire and other product enterprises be 10mg / m 3 , the environmental protection pressure on the rubber industry has increased sharply, and environmental protection issues have become a "bottleneck" for the survival and development of many tire companies.

[0003] On the other hand, with the development of new energy vehicles, the requirements for low rolling resistance green tires are getting higher and higher. The combined use of white carbon black silane coupling agent is beyond the reach of other fillers in solving rolling resistance. Therefore, the amount of white carbon black silane coupling agent is gradually increasing. Most of the silane coupling agents currently used in the market are Si69. Si69 first undergoes hydrolysis to remove ethanol gas, and then forms a chemical bond with the surface of white carbon black. Therefore, a large amount of ethanol gas is discharged during the production process, resulting in excessive VOCs. Therefore, seeking a coupling agent with low gas emissions has become the focus of source control. At the same time, it can further reduce the heat generation of the rubber compound. Improving the rolling resistance of the tire is also a key technology to improve product quality, increase product market share and brand capabilities. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a tire tread composition, preparation method and tire with low rolling resistance and low VOCs emissions. The present invention uses a high content of white carbon black and a new silane coupling agent at the same time. The mechanical properties of the rubber meet the requirements for tire use, the heat generation performance is reduced, and the VOCs emissions in the workshop can be reduced by about 80%, which can meet the use requirements of low rolling resistance green tires.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] The first aspect of the present invention provides a tire tread composition with low rolling resistance and low VOCs emission, comprising the following components in parts by weight:

[0007] Natural rubber 100

[0008] Carbon black 5-20

[0009] White carbon black 20-50

[0010] Coupling agent 2-5

[0011] Zinc oxide 3-5

[0012] Stearic acid 1-3

[0013] Antioxidant 2-5

[0014] Sulfur 1-2

[0015] Accelerator 1-4

[0016] Anti-scorch agent 0.1-0.5;

[0017] The coupling agent includes 3-mercaptopropylethoxybis(propyl-hexapropoxy)siloxane.

[0018] Furthermore, the tire tread composition with low rolling resistance and low VOCs emission comprises the following components in parts by weight:

[0019] Natural rubber 100

[0020] Carbon black 5-20

[0021] White carbon black 20-50

[0022] Coupling agent 3-4.2

[0023] Zinc Oxide 4

[0024] Stearic acid 2

[0025] Antioxidant 4.5

[0026] Sulfur 1-1.2

[0027] Accelerator 2.4-2.8

[0028] Anti-scorch agent 0.3;

[0029] Further preferably, carbon black is preferably 20 parts;

[0030] Further preferably, the coupling agent is preferably 3 parts by weight of 3-mercaptopropylethoxybis(propyl-hexapropoxy)siloxane, or 3 parts by weight of 3-mercaptopropylethoxybis(propyl-hexapropoxy)siloxane + 1.2 parts by weight of bis-(γ-triethoxysilylpropyl)tetrasulfide.

[0031] Furthermore, the natural rubber is full latex or smoked sheet rubber or standard natural rubber.

[0032] Furthermore, the carbon black is selected from one or a mixture of two of the carbon blacks with models N220 or N234.

[0033] Furthermore, the white carbon black is precipitated white carbon black or highly dispersed white carbon black.

[0034] Furthermore, the antioxidant is selected from one or more of antioxidant 4020, antioxidant RD, and protective wax.

[0035] Furthermore, the accelerator is selected from a mixture of one or more of accelerator TBBS, accelerator DPG, and accelerator TBzTD.

[0036] Furthermore, after using the new coupling agent, the vulcanization speed is reduced, and the use of accelerator needs to be increased (2.4-2.8 parts) to increase the vulcanization speed.

[0037] Furthermore, the anti-scorching agent is selected from a mixture of one or more of N-chloroformylthio-4-propylene-dicarboximide, alkyl dithiophosphate zinc salt, N-cyclohexylthiophthalimide, N-cyclohexylthiophthalimide, and N-nitrosodiphenylamine.

[0038] A second aspect of the present invention provides a method for preparing a tire tread material with low rolling resistance and low VOCs emissions, comprising the following steps:

[0039] S1: preparing materials, preparing raw materials according to the tire tread composition described above;

[0040] S2: Masterbatch mixing: natural rubber, carbon black, white carbon black, coupling agent, stearic acid, zinc oxide, antioxidant, etc. are added into an internal mixer for plasticization to obtain a masterbatch;

[0041] S3: re-refining: adding the masterbatch obtained in S2 into an internal mixer and re-refining to obtain a second-stage masterbatch;

[0042] S4: Final refining: Add the masterbatch obtained in S3, sulfur, accelerator and anti-scorch agent into an internal mixer for final refining to obtain a tire tread material with low rolling resistance and low VOCs emission.

[0043] Furthermore, in S2, when mixing the masterbatch, the preset filling factor is maintained at 67%-75%, the mixing time is 2.5-3.5min, and the pressure is 6kg / cm 2 , debinding at 150-156℃;

[0044] In S3, during re-refining, the filling factor is maintained at 67%-75%, the mixing time is 1.5-2.5min, and the pressure is 6kg / cm 2 , debinding at 140-145℃;

[0045] In S4, at the final refining, the filling factor is maintained at 67%-75%, the refining time is 2.0-3.0min, and the pressure is 6kg / cm 2 , debinding at 110℃-118℃.

[0046] A third aspect of the present invention provides a low rolling resistance tire, comprising a tire tread material obtained by the above preparation method.

[0047] Compared with the prior art, the present invention has the following technical advantages:

[0048] By using high-content white carbon black and a new silane coupling agent, the mechanical properties of the rubber meet the requirements for tire use, the heat generation performance is reduced, and the VOCs emission in the workshop can be reduced by about 80%, which can meet the requirements for the use of low rolling resistance green tires. DETAILED DESCRIPTION

[0049] The present invention is described in detail below in conjunction with specific embodiments. Any features such as preparation means, materials, structures or composition ratios not clearly described in this technical solution are regarded as common technical features disclosed in the prior art.

[0050] Comparative Example 1

[0051] 100 parts by weight of natural rubber, 20 parts by weight of carbon black, 33 parts by weight of white carbon black, 3 parts by weight of bis-(γ-triethoxysilylpropyl) tetrasulfide, 2 parts by weight of stearic acid, 4 parts by weight of zinc oxide, 4.5 parts by weight of antioxidant, 1 part by weight of sulfur, 1.6 parts by weight of accelerator and 0.3 parts by weight of scorch retarder were fully mixed according to the above process, sampled, vulcanized and tested for performance. The results are shown in Table 2. Example 1

[0052] 3-mercaptopropylethoxybis(propyl-hexapropoxy)siloxane was used to replace bis-(γ-triethoxysilylpropyl)tetrasulfide, and the accelerator was increased by 0.8 parts by weight. The other components and process conditions were the same as those of the comparative example. The obtained sample was tested, and the physical properties were shown in Table 2. VOCs decreased from 2834ppm to 578ppm, and the decrease in VOCs was 79.6%. Compared with comparative example 1, the 300% elongation of the rubber compound of embodiment 1 decreased by 1.3MPa, the elongation increased by 9%, and the compression heat generation decreased by 12%. For low rolling resistance tires, the lower the heat generation, the better. Example 2

[0053] The weight fractions of sulfur and accelerator were increased by 0.1 and 0.1 respectively, and the other components and processes were the same as those in Example 1. The obtained samples were tested, and the physical properties were shown in Table 2. Compared with Comparative Example 1, the tearing property of the rubber compound in Example 2 was improved by 16%, and the compression heat generation was reduced by 18%. The VOCs decreased by more than 70% compared with Comparative Example 1. Example 3

[0054] 3-Mercaptopropylethoxybis(propyl-hexapropoxy)siloxane was compounded with bis-(γ-triethoxysilylpropyl)tetrasulfide (Si-69), and the remaining components and processes were the same as those in Example 1. The obtained samples were tested, and the physical properties are shown in Table 2. Compared with the comparative example, the elongation and strength of the rubber compound in Example 3 increased slightly, the elongation and tearing decreased slightly, and the compression heat generation decreased by 18%. The reduction of VOCs compared with Comparative Example 1 exceeded 70%. Example 4

[0055] The weight fractions of sulfur and accelerator were increased by 0.2 and 0.2 respectively, and the other components and processes were the same as those in Example 3. The obtained samples were tested, and the physical properties were shown in Table 2. Compared with Comparative Example 1, the mechanical properties of the rubber material in Example 4 and the performance of the comparative example were basically within 5%, and the compression heat generation was reduced by 14%. The reduction of VOCs compared with Comparative Example 1 was more than 70%. Example 5

[0056] The weight portion of TBzTD was increased by 0.2 parts, and the other components and processes were the same as those in Example 4. The obtained samples were tested, and the physical properties are shown in Table 2. Compared with Comparative Example 1, the tearing of Example 5 decreased by 20%, and the compression heat generation decreased by 25%. The VOCs decreased by more than 70% compared with Comparative Example 1.

[0057] Table 1 Summary of Comparative Examples and Implementation Formulas

[0058]

[0059] According to the above-mentioned rubber compound formula and preparation process, the specific test data of the rubber compound is shown in Table 2.

[0060] The physical and mechanical properties test data according to national standards are as follows:

[0061] Table 2 Physical properties of rubber

[0062]

[0063] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A tire tread composition with low rolling resistance and low VOCs emission, characterized in that: The composition comprises the following components in parts by weight: Natural rubber 100 Carbon Black 20 White carbon black 20-50 Coupling agent 3-5 Zinc oxide 3-5 Stearic acid 1-3 Antioxidant 2-5 Sulfur 1-2 Accelerator 1-4 Anti-scorch agent 0.1-0.5; The coupling agent includes 3-mercaptopropylethoxybis(propyl-hexapropoxy)siloxane; The coupling agent contains 3 parts by weight of 3-mercaptopropylethoxybis(propyl-hexapropoxy)siloxane, or 3 parts by weight of 3-mercaptopropylethoxybis(propyl-hexapropoxy)siloxane and 1.2 parts by weight of bis-(γ-triethoxysilylpropyl)tetrasulfide.

2. The tire tread composition with low rolling resistance and low VOCs emission according to claim 1, characterized in that: The natural rubber is full latex, smoked rubber or standard natural rubber.

3. The tire tread composition with low rolling resistance and low VOCs emission according to claim 1, characterized in that: The carbon black is selected from one of the carbon blacks of type N220 or N234 or a mixture of two of the two.

4. The tire tread composition with low rolling resistance and low VOCs emission according to claim 1, characterized in that: The white carbon black is precipitated white carbon black or highly dispersed white carbon black.

5. The tire tread composition with low rolling resistance and low VOCs emission according to claim 1, characterized in that: The antioxidant is selected from one or more of antioxidant 4020, antioxidant RD, and protective wax.

6. The tire tread composition with low rolling resistance and low VOCs emission according to claim 1, characterized in that: The accelerator is selected from a mixture of one or more of accelerator TBBS, accelerator DPG, and accelerator TBzTD.

7. The tire tread composition with low rolling resistance and low VOCs emission according to claim 1, characterized in that: The anti-scorch agent is selected from a mixture of one or more of N-chloroformylthio-4-propylene-dicarboximide, alkyl dithiophosphate zinc salt, N-cyclohexylthiophthalimide, N-cyclohexylthiophthalimide, and N-nitrosodiphenylamine.

8. A method for preparing a tire tread material with low rolling resistance and low VOCs emission, characterized in that: The following steps are involved: S1: preparing materials, preparing raw materials according to the tire tread composition according to any one of claims 1 to 7; S2: Masterbatch mixing: natural rubber, carbon black, white carbon black, coupling agent, stearic acid, zinc oxide and antioxidant are added into an internal mixer for plasticizing to obtain a masterbatch; S3: re-refining: adding the masterbatch obtained in S2 into an internal mixer and re-refining to obtain a second-stage masterbatch; S4: Final refining: Add the masterbatch obtained in S3, sulfur, accelerator and anti-scorch agent into an internal mixer for final refining to obtain a tire tread material with low rolling resistance and low VOCs emission.

9. The method for preparing a tire tread material with low rolling resistance and low VOCs emission according to claim 8, characterized in that: In S2, when mixing the masterbatch, keep the preset filling factor at 67%-75%, mixing time at 2.5-3.5min, and pressure at 6kg / cm 2 , debinding at 150-156℃; In S3, during re-refining, the filling factor is maintained at 67%-75%, the mixing time is 1.5-2.5min, and the pressure is 6kg / cm 2 , debinding at 140-145℃; In S4, at the final refining, the filling factor is maintained at 67%-75%, the refining time is 2.0-3.0min, and the pressure is 6kg / cm 2 , debinding at 110℃-118℃.

10. A low rolling resistance tire, characterized in that: The tire tread material comprises the tire tread material obtained by the preparation method as claimed in claim 8.