A wear-resistant and weather-resistant nano coating and preparation method thereof

Through the design of nanocoating with two-layer structure, the use of polyurethane modified epoxy resin and polyamide grafting additives and other materials, the problem of insufficient wear resistance of existing nanocoatings is solved, and high adhesion, impact resistance and weather resistance are achieved. Nanocoating is suitable for building protection in water conservancy projects.

CN118580750BActive Publication Date: 2024-11-05ZIBO YINGQIANG CHEM TECH
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411048127.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-05
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The wear resistance of existing nanocoatings is poor and cannot meet the needs of buildings in high-speed sand-sanding water flow erosion and thrust impact and grinding in water conservancy projects.

Method used

Wear-resistant and weather-resistant nanocoating with two-layer structure, coating A is composed of polyurethane-modified epoxy resin and polyepoxy propyl alcohol grafted nanosilicon dioxide, coating B is composed of polyamide grafted wear-resistant additives, The polymer modified aluminum hydroxide nanosheets and aminopropyl triethoxysilane are composed of which cross-link Coating A and Coating B through composite to enhance adhesion and impact resistance.

Benefits of technology

It significantly improves the adhesion, impact resistance, wear resistance and weather resistance of the coating, can effectively prevent the penetration of aging media and extend the service life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of coating preparation, and in particular to a wear-resistant and weather-resistant nano coating and a preparation method thereof. The nano coating comprises a coating A and a coating B, wherein the coating A is coated on a sample surface and dried; the coating B is coated on the surface of the coating A and dried. In the invention, the coating A and the coating B are compounded and used, so that the nano coating has strong adhesion to the sample, so that it is not easy to fall off after long-term use. At the same time, the coating B can be cross-linked with the active ingredients in the coating A, so that the nano coating has strong impact resistance and wear resistance, and the coating B located on the surface can effectively block the aging medium to prevent it from penetrating into the material, thereby increasing the corrosion resistance and weather resistance of the coating, and thus has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating preparation, and in particular to a wear-resistant and weather-resistant nano coating and a preparation method thereof. Background Art

[0002] Nano coatings are a kind of protective material widely used in modern industrial industries. They have achieved good applications in many aspects such as concrete facility base protection, metal material surface treatment protection, and construction equipment protection. Using the small size effect, surface and interface effect, and quantum size effect of nanoparticles, applying nanotechnology to the coating synthesis process, and preparing nano functional coatings has become an important development direction of modern coating research. Adding nano phases to high hardness wear-resistant coatings can further improve the hardness and wear resistance of the coating, while maintaining high toughness.

[0003] Patent technology document CN1556162A nano transparent wear-resistant composite coating introduces a two-component wear-resistant composite coating and a single-component wear-resistant composite coating, which can be applied to resin, metal and wood surfaces. Since the resin used is a saturated hydroxy polyester resin, hydroxy acrylic resin, epoxy resin, and alkyd resin, the hardness of the coating used is limited. In addition, the wear resistance of nanoparticles and film-forming resins is solely relied on, and the improvement of wear resistance is relatively limited; Patent technology document CN1821325A discloses a method for preparing a wear-resistant and corrosion-resistant nano composite epoxy asphalt repair coating. The invention adds one or two nano-scale functional powder materials to the epoxy asphalt anti-corrosion coating. The obtained coating has significantly improved friction resistance compared with the original epoxy asphalt anti-corrosion coating. However, relying solely on the wear resistance of nanoparticles cannot meet the needs of buildings in water conservancy projects being eroded by high-speed sand-containing water flow and impact and abrasion of bedload.

[0004] Therefore, according to the above-mentioned related technologies, it is urgent to develop a wear-resistant and weather-resistant nano coating and a preparation method thereof. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a wear-resistant and weather-resistant nano coating and a preparation method thereof, so as to solve the problem of poor wear resistance of nano coatings in the prior art.

[0006] Based on the above purpose, the present invention provides a wear-resistant and weather-resistant nano coating and a preparation method thereof.

[0007] A wear-resistant and weather-resistant nano coating, the nano coating comprising a coating A and a coating B, wherein the thickness ratio of the coating A to the coating B is 15.6-15.8:24.4-26.6;

[0008] The coating A is obtained by coating the coating A on the surface of the sample and drying it;

[0009] The coating B is obtained by coating the coating B on the surface of the coating A and drying it;

[0010] The coating A comprises the following raw materials in parts by weight: 23-25 ​​parts of polyurethane modified epoxy resin, 15-18 parts of polyoxypropylene grafted nano-silicon dioxide, and 5.7-6.45 parts of butyl glycidyl ether;

[0011] The coating B comprises the following raw materials in parts by weight: 6-9 parts of polyamide grafted wear-resistant additive, 18-21 parts of polymer-modified aluminum hydroxide nanosheets, 3.6-4.5 parts of butyl glycidyl ether, and 14-18 parts of aminopropyl triethoxy silane.

[0012] Preferably, the preparation method of the polyurethane modified epoxy resin is as follows:

[0013] Step A1. Add half of the total amount of polytetrahydrofuran diol to 4,4'-diphenyl diisocyanate, heat the reaction to 70-75°C for 1-1.5h, then cool to 58-60°C, add the remaining polytetrahydrofuran diol, heat to 72-75°C for 80-90min, and generate an isocyanate-terminated polyurethane prepolymer;

[0014] Step A2. Mix the terminal isocyanate polyurethane prepolymer and glycidol in an anhydrous dichloromethane solvent at a molar ratio of 1:2, and react at 38-42° C. for 3.5-4 hours under a nitrogen atmosphere to obtain a polyurethane-modified epoxy resin.

[0015] Preferably, the mass ratio of 4,4'-diphenyl diisocyanate to polytetrahydrofuran diol in step A1 is 480-520:100-120.

[0016] Preferably, the preparation method of the poly(propylene oxide)-grafted nano-silica is as follows:

[0017] Step B1. Anhydrous ethanol, distilled water and ammonia water are mixed, stirred at room temperature at a stirring speed of 500 r / min, and then tetraethyl orthosilicate and the second portion of anhydrous ethanol are added, and stirring is continued for 2.5-3h, and excess solvent is removed by high-speed centrifugation, washed with distilled water 3-5 times, and then vacuum dried to obtain nano-silicon dioxide;

[0018] Step B2. In a nitrogen atmosphere, disperse the nano-silica in a sodium methoxide solution, ultrasonically shake for 8-12 minutes, continue the reaction for 50-60 minutes, stop the reaction, wash twice with 20 mL of anhydrous methanol, and then dry and grind to obtain pretreated nano-silica;

[0019] Step B3. Mix the pretreated nano-silica and glycidol evenly, control the stirring speed to 400r / min, the temperature to 100-110°C, react for 40-45min under nitrogen protection, then centrifuge and wash 3-5 times with 30mL of a mixed solution of ethanol and water, and dry to obtain poly(glycidyl alcohol)-grafted nano-silica.

[0020] Preferably, the usage ratio of anhydrous ethanol, distilled water, ammonia water, tetraethyl orthosilicate and the second portion of anhydrous ethanol in step B1 is 800-900 mL: 70-72 g: 24-27 g: 122-126 g: 90-100 mL;

[0021] In step B2, the dosage ratio of the nano-silicon dioxide to the sodium methoxide solution is 5-5.2 g: 90-100 mL, and the concentration of the sodium methoxide solution is 0.3-0.4 mol / L;

[0022] The mass ratio of the pretreated nano-silica to glycidol in step B3 is 4.6-5.2:10-12, and the mixed solution of ethanol and water is obtained by mixing ethanol and water in a volume ratio of 1:1.

[0023] Preferably, the preparation method of the polyamide grafted wear-resistant additive is as follows:

[0024] Plasma treatment is performed on the wear-resistant additive, and any one of compressed air, nitrogen, oxygen and argon is used as plasma. The treated wear-resistant additive is added to polyamide, and reacted at a temperature of 90-100° C. and a stirring speed of 100-120 r / min for 6-8 hours to obtain a polyamide-grafted wear-resistant additive;

[0025] The mass ratio of the wear-resistant additive to polyamide is 40-43:8-11, and the wear-resistant additive is one or more of nano-tungsten carbide, zirconium oxide, aluminum oxide and silicon carbide mixed in any proportion.

[0026] Preferably, the preparation method of the polymer-modified aluminum hydroxide nanosheets is as follows:

[0027] Step C1. dissolving aluminum sec-butoxide and aluminum isopropoxide in water, adding 12-(2-bromoisobutyrylamino) dodecanoic acid, heating to 60-70° C., reacting for 2-3 hours to obtain a reaction solution, precipitating and purifying the reaction solution 3-5 times to obtain aluminum bromide hydroxide nanosheets;

[0028] Step C2. dissolving aluminum hydroxide bromide nanosheets in N,N-dimethylformamide, adding acrylonitrile, copper bromide and 2,2'-bipyridine, deoxygenating with nitrogen, freezing into a solid with liquid nitrogen, adding cuprous bromide, heating to 58-60°C and polymerizing for 8-9h to obtain polymer-modified aluminum hydroxide nanosheets;

[0029] The mass ratio of aluminum sec-butoxide, aluminum isopropoxide, water and 12-(2-bromoisobutyrylamino)dodecanoic acid in step C1 is 4.8-5.1:4.8-5.1:90-100:0.4-0.5;

[0030] The dosage ratio of the aluminum hydroxide bromide nanosheets, N,N-dimethylformamide, acrylonitrile, copper bromide, 2,2'-bipyridine and cuprous bromide in step C2 is 0.08-0.12 g: 10-12 mL: 80-100 mL: 0.08-0.1 g: 0.08-0.1 g: 0.02-0.04 g.

[0031] A method for preparing a wear-resistant and weather-resistant nano coating comprises the following steps:

[0032] Step S1. polyurethane modified epoxy resin, polypropylene oxide grafted nano-silica and butyl glycidyl ether are mixed evenly to obtain coating A, coating A is evenly applied on the surface of the sample and dried to obtain sample 1 with coating A on the surface;

[0033] Step S2. Mix the polyamide grafted wear-resistant additive, polymer-modified aluminum hydroxide nanosheets, butyl glycidyl ether and aminopropyl triethoxysilane evenly to obtain coating B, and evenly apply coating B on the surface of sample 1 with coating A and dry it to obtain sample 2 with coating A and coating B on the surface, that is, to obtain wear-resistant and weather-resistant nano coating.

[0034] Beneficial effects of the present invention:

[0035] The coating A and coating B in the wear-resistant and weather-resistant nano coating provided by the present invention are compounded and used, so that the nano coating has strong adhesion to the sample, so that it is not easy to fall off after long-term use. At the same time, coating B will cross-link with the active ingredients inside coating A, so that the nano coating has strong impact resistance and wear resistance, and coating B located on the surface can effectively block the aging medium to prevent it from penetrating into the interior of the material, thereby increasing the corrosion resistance and weather resistance of the coating. Therefore, compared with the prior art, it has broad application prospects. DETAILED DESCRIPTION

[0036] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0037] The sources and properties of some raw materials in the present invention are as follows:

[0038] Polyamide was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. with a CAS number of 63428-84-2.

[0039] Embodiment 1: A method for preparing a wear-resistant and weather-resistant nano coating, comprising the following steps:

[0040] Step 1. Add 50g of polytetrahydrofuran diol to 480g of 4,4'-diphenyl diisocyanate, heat the reaction to 70°C for 1h, then cool to 58°C, add 50g of polytetrahydrofuran diol, heat to 72°C for 80min, and generate a terminal isocyanate polyurethane prepolymer;

[0041] Step 2. Mix the terminal isocyanate polyurethane prepolymer and glycidol in an anhydrous dichloromethane solvent at a molar ratio of 1:2, and react at 38° C. for 3.5 hours under a nitrogen atmosphere to obtain a polyurethane-modified epoxy resin;

[0042] Step 3. 800 mL of anhydrous ethanol, 70 g of distilled water, and 24 g of ammonia water were mixed, stirred at a stirring speed of 500 r / min at room temperature, and then 122 g of tetraethyl orthosilicate and 90 mL of the second portion of anhydrous ethanol were added, and stirring was continued for 2.5 h. The excess solvent was removed by high-speed centrifugation, and the mixture was washed with distilled water for 3 times, and then vacuum dried to obtain nano-silica;

[0043] Step 4. Under nitrogen atmosphere, 5 g of nano-silica was dispersed in 90 mL of 0.3 mol / L sodium methoxide solution, ultrasonically shaken for 8 min, and reacted for 50 min. The reaction was stopped and washed twice with 20 mL of anhydrous methanol, and then dried and ground to obtain pretreated nano-silica;

[0044] Step 5. 4.6 g of pretreated nano-silica and 10 g of glycidol were mixed evenly, the stirring speed was controlled to be 400 r / min, the temperature was 100° C., the mixture was reacted for 40 min under nitrogen protection, and then centrifuged and separated. The mixture was washed three times with a mixed solution of ethanol and water obtained by mixing 30 mL of ethanol and water in a volume ratio of 1:1, and dried to obtain nano-silica grafted with poly(glycidyl alcohol);

[0045] Step 6. Plasma-treat the nano-tungsten carbide, using any one of compressed air, nitrogen, oxygen, and argon as plasma, adding 40 g of the treated wear-resistant additive to 8 g of polyamide, reacting at a temperature of 90° C. and a stirring speed of 100 r / min for 6 hours to obtain a polyamide-grafted wear-resistant additive;

[0046] Step 7. Dissolve 4.8 g of aluminum sec-butoxide and 4.8 g of aluminum isopropoxide in 90 g of water, add 0.4 g of 12-(2-bromoisobutyrylamino) dodecanoic acid, heat to 60° C., react for 2 h to obtain a reaction solution, precipitate and purify the reaction solution three times to obtain aluminum bromide hydroxide nanosheets;

[0047] Step 8. Dissolve 0.08 g of aluminum hydroxide bromide nanosheets in 10 mL of N,N-dimethylformamide, add 80 mL of acrylonitrile, 0.08 g of copper bromide and 0.08 g of 2,2'-bipyridine, deoxygenate with nitrogen, freeze into a solid with liquid nitrogen, add 0.02 g of cuprous bromide, heat to 58°C and polymerize for 8 h to obtain polymer-modified aluminum hydroxide nanosheets;

[0048] Step 9. 23 g of polyurethane-modified epoxy resin, 15 g of nano-silica grafted with polypropylene oxide and 5.7 g of butyl glycidyl ether are mixed evenly to obtain coating A, and coating A is evenly applied on the surface of the sample and dried to obtain sample 1 with coating A on the surface;

[0049] Step 10. Mix 6 g of polyamide-grafted wear-resistant additive, 18 g of polymer-modified aluminum hydroxide nanosheets, 3.6 g of butyl glycidyl ether and 14 g of aminopropyl triethoxysilane to obtain coating B. Evenly apply coating B on the surface of sample 1 with coating A and dry it to obtain sample 2 with coating A and coating B on the surface, that is, a wear-resistant and weather-resistant nano coating, in which the thickness ratio of coating A to coating B is 15.6:24.4.

[0050] Embodiment 2: A method for preparing a wear-resistant and weather-resistant nano coating, comprising the following steps:

[0051] Step 1. Add 56g of polytetrahydrofuran diol to 490g of 4,4'-diphenyl diisocyanate, heat the reaction to 72°C for 1.3h, then cool to 59°C, add 54g of polytetrahydrofuran diol, heat to 73°C for 84min, and generate a terminal isocyanate polyurethane prepolymer;

[0052] Step 2. Mix the terminal isocyanate polyurethane prepolymer and glycidol in an anhydrous dichloromethane solvent at a molar ratio of 1:2, and react at 39° C. for 3.6 hours under a nitrogen atmosphere to obtain a polyurethane-modified epoxy resin;

[0053] Step 3. 840 mL of anhydrous ethanol, 71 g of distilled water, and 25 g of ammonia water were mixed, stirred at room temperature at a stirring speed of 500 r / min, and then 123 g of tetraethyl orthosilicate and 94 mL of the second portion of anhydrous ethanol were added, and stirring was continued for 2.6 h. Excess solvent was removed by high-speed centrifugation, and the mixture was washed with distilled water for 4 times, and then vacuum dried to obtain nano-silica;

[0054] Step 4. Under nitrogen atmosphere, 5.1 g of nano-silica was dispersed in 94 mL of 0.34 mol / L sodium methoxide solution, ultrasonically shaken for 9 min, and reacted for 54 min. The reaction was stopped and washed twice with 20 mL of anhydrous methanol, and then dried and ground to obtain pretreated nano-silica;

[0055] Step 5. 4.7 g of pretreated nano-silica and 11 g of glycidol were mixed evenly, the stirring speed was controlled to be 400 r / min, the temperature was 104°C, the reaction was carried out under nitrogen protection for 42 min, and then centrifuged and separated, and washed 4 times with a mixed solution of ethanol and water obtained by mixing 30 mL of ethanol and water in a volume ratio of 1:1, and dried to obtain nano-silica grafted with poly(glycidyl alcohol);

[0056] Step 6. Plasma-treat the zirconium oxide, using any one of compressed air, nitrogen, oxygen, and argon as plasma, adding 42 g of the treated wear-resistant additive to 9 g of polyamide, reacting at a temperature of 94° C. and a stirring speed of 105 r / min for 7 h to obtain a polyamide-grafted wear-resistant additive;

[0057] Step 7. Dissolve 4.9 g of aluminum sec-butoxide and 4.9 g of aluminum isopropoxide in 94 g of water, add 0.44 g of 12-(2-bromoisobutyrylamino) dodecanoic acid, heat to 64° C., react for 2.5 h to obtain a reaction solution, precipitate and purify the reaction solution 4 times to obtain aluminum hydroxide bromide nanosheets;

[0058] Step 8. Dissolve 0.09 g of aluminum hydroxide bromide nanosheets in 11 mL of N,N-dimethylformamide, add 86 mL of acrylonitrile, 0.09 g of copper bromide and 0.09 g of 2,2'-bipyridine, deoxygenate with nitrogen and freeze into a solid with liquid nitrogen, add 0.03 g of cuprous bromide, heat to 59 ° C and polymerize for 8.5 hours to obtain polymer-modified aluminum hydroxide nanosheets;

[0059] Step 9. 24 g of polyurethane-modified epoxy resin, 16 g of nano-silica grafted with polypropylene oxide and 5.95 g of butyl glycidyl ether are mixed evenly to obtain coating A, and coating A is evenly applied on the surface of the sample and dried to obtain sample 1 with coating A on the surface;

[0060] Step 10. Mix 7g of polyamide-grafted wear-resistant additive, 19g of polymer-modified aluminum hydroxide nanosheets, 3.9g of butyl glycidyl ether and 16g of aminopropyl triethoxysilane to obtain coating B. Evenly apply coating B on the surface of sample 1 with coating A and dry it to obtain sample 2 with coating A and coating B on the surface, that is, to obtain wear-resistant and weather-resistant nano coating, wherein the thickness ratio of coating A to coating B is 15.7:25.

[0061] Embodiment 3: A method for preparing a wear-resistant and weather-resistant nano coating, comprising the following steps:

[0062] Step 1. Add 58g of polytetrahydrofuran diol to 500g of 4,4'-diphenyl diisocyanate, heat the reaction to 74°C for 1.4h, then cool to 59°C, add 58g of polytetrahydrofuran diol, heat to 74°C for 88min, and generate an isocyanate-terminated polyurethane prepolymer;

[0063] Step 2. Mix the terminal isocyanate polyurethane prepolymer and glycidol in an anhydrous dichloromethane solvent at a molar ratio of 1:2, and react at 40° C. for 3.8 hours under a nitrogen atmosphere to obtain a polyurethane-modified epoxy resin;

[0064] Step 3. 880 mL of anhydrous ethanol, 71 g of distilled water, and 26 g of aqueous ammonia were mixed, stirred at room temperature at a stirring speed of 500 r / min, and then 125 g of tetraethyl orthosilicate and 98 mL of the second portion of anhydrous ethanol were added, and stirring was continued for 2.8 h. Excess solvent was removed by high-speed centrifugation, and the mixture was washed with distilled water for 4 times, and then vacuum dried to obtain nano-silica;

[0065] Step 4. Under nitrogen atmosphere, 5.1 g of nano-silica was dispersed in 98 mL of 0.38 mol / L sodium methoxide solution, ultrasonically shaken for 11 min, and reacted for 58 min. The reaction was stopped and washed twice with 20 mL of anhydrous methanol, and then dried and ground to obtain pretreated nano-silica;

[0066] Step 5. 5 g of pretreated nano-silica and 11 g of glycidol were mixed evenly, the stirring speed was controlled to be 400 r / min, the temperature was 108°C, the reaction was carried out under nitrogen protection for 44 min, and then centrifuged and separated, and washed 4 times with a mixed solution of ethanol and water obtained by mixing 30 mL of ethanol and water in a volume ratio of 1:1, and dried to obtain nano-silica grafted with poly(glycidyl alcohol);

[0067] Step 6. Plasma-treating the alumina, using any one of compressed air, nitrogen, oxygen, and argon as plasma, adding 42 g of the treated wear-resistant additive to 10 g of polyamide, reacting at a temperature of 98° C. and a stirring speed of 115 r / min for 7 h to obtain a polyamide-grafted wear-resistant additive;

[0068] Step 7. Dissolve 5 g of aluminum sec-butoxide and 5 g of aluminum isopropoxide in 98 g of water, add 0.48 g of 12-(2-bromoisobutyrylamino)dodecanoic acid, heat to 68° C., react for 2.5 h to obtain a reaction solution, precipitate and purify the reaction solution 4 times to obtain aluminum bromohydroxide nanosheets;

[0069] Step 8. Dissolve 0.1 g of aluminum hydroxide bromide nanosheets in 11 mL of N,N-dimethylformamide, add 95 mL of acrylonitrile, 0.09 g of copper bromide and 0.09 g of 2,2'-bipyridine, deoxygenate with nitrogen, freeze into a solid with liquid nitrogen, add 0.03 g of cuprous bromide, heat to 59° C. and polymerize for 8 h to obtain polymer-modified aluminum hydroxide nanosheets;

[0070] Step 9. 24 g of polyurethane-modified epoxy resin, 17 g of nano-silica grafted with polypropylene oxide and 6.2 g of butyl glycidyl ether are mixed evenly to obtain coating A, and coating A is evenly applied on the surface of the sample and dried to obtain sample 1 with coating A on the surface;

[0071] Step 10. Mix 8g of polyamide-grafted wear-resistant additive, 20g of polymer-modified aluminum hydroxide nanosheets, 4.2g of butyl glycidyl ether and 17g of aminopropyl triethoxysilane to obtain coating B. Evenly apply coating B on the surface of sample 1 with coating A and dry it to obtain sample 2 with coating A and coating B on the surface, that is, to obtain wear-resistant and weather-resistant nano coating, wherein the thickness ratio of coating A to coating B is 15.8:26.2.

[0072] Embodiment 4: A method for preparing a wear-resistant and weather-resistant nano coating, comprising the following steps:

[0073] Step 1. Add 60g of polytetrahydrofuran diol to 520g of 4,4'-diphenyl diisocyanate, heat the reaction to 75°C for 1.5h, then cool to 60°C, add 60g of polytetrahydrofuran diol, heat to 75°C for 90min, and generate a terminal isocyanate polyurethane prepolymer;

[0074] Step 2. Mix the terminal isocyanate polyurethane prepolymer and glycidol in an anhydrous dichloromethane solvent at a molar ratio of 1:2, and react at 42° C. for 4 hours under a nitrogen atmosphere to obtain a polyurethane-modified epoxy resin;

[0075] Step 3. 900 mL of anhydrous ethanol, 72 g of distilled water, and 27 g of ammonia water were mixed, stirred at room temperature at a stirring speed of 500 r / min, and then 126 g of tetraethyl orthosilicate and 100 mL of the second portion of anhydrous ethanol were added, and stirring was continued for 3 h. Excess solvent was removed by high-speed centrifugation, and the mixture was washed with distilled water for 5 times, and then vacuum dried to obtain nano-silicon dioxide;

[0076] Step 4. Under nitrogen atmosphere, 5.2 g of nano-silica was dispersed in 100 mL of 0.4 mol / L sodium methoxide solution, ultrasonically shaken for 12 min, and reacted for 60 min. The reaction was stopped and washed twice with 20 mL of anhydrous methanol, and then dried and ground to obtain pretreated nano-silica;

[0077] Step 5. 5.2 g of pretreated nano-silica and 12 g of glycidol were mixed evenly, the stirring speed was controlled to be 400 r / min, the temperature was 110° C., the mixture was reacted for 45 min under nitrogen protection, and then centrifuged and separated. The mixture was washed 5 times with a mixed solution of ethanol and water obtained by mixing 30 mL of ethanol and water in a volume ratio of 1:1, and dried to obtain nano-silica grafted with poly(glycidyl alcohol);

[0078] Step 6. Plasma-treating the nano-silicon carbide, using any one of compressed air, nitrogen, oxygen, and argon as plasma, adding 43 g of the treated wear-resistant additive to 11 g of polyamide, reacting at a temperature of 100° C. and a stirring speed of 120 r / min for 8 h to obtain a polyamide-grafted wear-resistant additive;

[0079] Step 7. Dissolve 5.1 g of aluminum sec-butoxide and 5.1 g of aluminum isopropoxide in 100 g of water, add 0.5 g of 12-(2-bromoisobutyrylamino) dodecanoic acid, heat to 70° C., react for 3 h to obtain a reaction solution, precipitate and purify the reaction solution 5 times to obtain aluminum bromohydroxide nanosheets;

[0080] Step 8. Dissolve 0.12 g of aluminum hydroxide bromide nanosheets in 12 mL of N,N-dimethylformamide, add 100 mL of acrylonitrile, 0.1 g of copper bromide and 0.1 g of 2,2'-bipyridine, deoxygenate with nitrogen, freeze into a solid with liquid nitrogen, add 0.04 g of cuprous bromide, heat to 60°C and polymerize for 9 hours to obtain polymer-modified aluminum hydroxide nanosheets;

[0081] Step 9. 25 g of polyurethane-modified epoxy resin, 18 g of nano-silica grafted with polypropylene oxide and 6.45 g of butyl glycidyl ether are mixed evenly to obtain coating A, and coating A is evenly applied on the surface of the sample and dried to obtain sample 1 with coating A on the surface;

[0082] Step 10. Mix 9g of polyamide grafted wear-resistant additive, 21g of polymer-modified aluminum hydroxide nanosheets, 4.2g of butyl glycidyl ether and 18g of aminopropyl triethoxysilane to obtain coating B. Evenly apply coating B on the surface of sample 1 with coating A and dry it to obtain sample 2 with coating A and coating B on the surface, that is, to obtain wear-resistant and weather-resistant nano coating, wherein the thickness of coating A and coating B is 15.8:26.6.

[0083] Comparative Example 1:

[0084] Compared with Example 1, this comparative example does not add coating A during the preparation of the weather-resistant and wear-resistant nano coating, and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally the weather-resistant and wear-resistant nano coating is obtained.

[0085] Comparative Example 2:

[0086] Compared with Example 1, this comparative example does not add coating B during the preparation of the weather-resistant and wear-resistant nano coating, and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally the weather-resistant and wear-resistant nano coating is obtained.

[0087] Comparative Example 3:

[0088] Compared with Example 1, this comparative example does not add polyoxypropylene alcohol grafted nano-silica during the preparation of the weather-resistant and wear-resistant nano-coating. The remaining steps and parameters are the same and will not be repeated in this comparative example. Finally, the weather-resistant and wear-resistant nano-coating is obtained.

[0089] Comparative Example 4:

[0090] Compared with Example 1, this comparative example does not add a polyamide-grafted wear-resistant additive during the preparation of the weather-resistant and wear-resistant nano coating. The remaining steps and parameters are the same and will not be repeated in this comparative example. Finally, a weather-resistant and wear-resistant nano coating is obtained.

[0091] Comparative Example 5:

[0092] Compared with Example 1, this comparative example only replaces the "polyamide grafted wear-resistant additive" with the "wear-resistant additive", and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally a weather-resistant and wear-resistant nano coating is obtained.

[0093] Comparative Example 6:

[0094] Compared with Example 1, this comparative example does not add polymer-modified aluminum hydroxide nanosheets during the preparation of the weather-resistant and wear-resistant nano-coating. The remaining steps and parameters are the same and will not be repeated in this comparative example. Finally, a weather-resistant and wear-resistant nano-coating is obtained.

[0095] Comparative Example 7:

[0096] Compared with Example 1, this comparative example only replaces the "polymer-modified aluminum hydroxide nanosheets" with "aluminum hydroxide", and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally a weather-resistant and wear-resistant nano-coating is obtained.

[0097] Comparative Example 8: Compared with Example 1, this comparative example only adjusts "wherein the ratio of the thickness of coating A and coating B is 15.6:24.4" to "wherein the ratio of the thickness of coating A and coating B is 24.4:15.6", and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally a weather-resistant and wear-resistant nano coating is obtained.

[0098] Performance test: The sample 2 test plate with coating A and coating B on the surface prepared in Examples 1 to 4 and Comparative Examples 1 to 8 was placed flat at 25° C. for 7 days and then the performance was tested;

[0099] Mechanical properties test: Adhesion: tested according to "GB5210-85 Paint film adhesion determination method (pull-off method)"; Impact resistance: tested according to "GB / T1732-93 Paint film impact resistance determination method", recording the impact resistance at room temperature and heated (40°C); Abrasion resistance: tested according to "GB / T1768-89 Paint film abrasion resistance determination method", load 500g, grinding number 500r; Hydrophobicity test: YJ-82-1 contact angle tester was used to test the water contact angle of the coating, and the mass of each water droplet was 4mg; Weathering performance test: Aging in a UV aging box for 7d, using WGG-60E4 gloss meter to measure the gloss of the coating before and after UV aging, and record the gloss retention rate (%), the UV aging box uses a straight tube high-pressure mercury lamp GGZ-500 as the UV light source, and the UV intensity is 20w / m 2 , test temperature 60℃; Anticorrosion performance test: The anticorrosion performance of the coating was tested by repeated immersion test in acidic salt water. Scratches were preformed on the surface of each group of samples. One test cycle was 24h, including 18h of immersion and 6h of baking, which was carried out continuously for a total of 240h. Environmental conditions: The solution was an acidic 5wt% NaCl solution, pH=3-4, T=40℃. During baking, the moisture on the surface of the specimen was dried within 10min, and the surface temperature of the specimen was below 60℃. The results are shown in Table 1:

[0100] Table 1 Summary of product performance test results in Examples 1-4 and Comparative Examples 1-8

[0101] project Adhesion / MPa Impact resistance / cm Wear mass loss / mg Water contact angle / ° Gloss retention rate / % Corrosion Example 1 12.2 52 1.4 78 90 1mm corrosion at the scratch Example 2 11.8 51 1.5 75 88 1mm corrosion at the scratch Example 3 12.0 53 1.2 76 90 1mm corrosion at the scratch Example 4 11.6 49 1.2 76 89 1mm corrosion at the scratch Comparative Example 1 8.2 38 2.7 71 76 3mm corrosion at the scratch Comparative Example 2 11.0 47 1.8 71 85 4mm corrosion at the scratch Comparative Example 3 10.4 44 2.1 73 83 3mm corrosion at the scratch Comparative Example 4 9.6 40 2.5 69 80 5mm corrosion at the scratch Comparative Example 5 10.0 41 2.4 70 81 5mm corrosion at the scratch Comparative Example 6 10.2 43 2.2 69 82 4mm corrosion at the scratch Comparative Example 7 10.6 45 1.9 70 84 4mm corrosion at the scratch Comparative Example 8 11.4 48 1.6 74 87 1mm corrosion at the scratch

[0102] Data Analysis:

[0103] It can be seen from Table 1 that the nano coating prepared by the present invention has higher adhesion, stronger impact resistance, higher wear resistance, higher weather resistance and corrosion resistance.

[0104] This may be because the polyurethane-modified epoxy resin and polypropylene oxide grafted nano-silica in the coating A provided by the present invention have good adhesion to the sample, so that the coating as a whole can fit firmly to the sample, and it also has certain flame retardancy; coating B can effectively isolate external corrosive media from penetrating into the material due to its own hydrophobicity, and the polyamide grafted wear-resistant additive and polymer-modified aluminum hydroxide nanosheets in coating B can be evenly dispersed in the matrix, increasing wear resistance and impact resistance, and can also cross-link with the active ingredients in coating A and coating B, further improving the mechanical properties and weather resistance and corrosion resistance of the coating.

[0105] Therefore, by compounding coating A and coating B, the nano coating has strong adhesion to the sample, so that it is not easy to fall off after long-term use, and the nano coating has strong impact resistance and wear resistance. However, when the thickness of coating A is increased and the thickness of coating B is reduced, it is found that the performance of the final nano coating is reduced.

[0106] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0107] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A wear-resistant and weather-resistant nano coating, characterized in that: The nano coating comprises a coating A and a coating B, wherein the thickness ratio of the coating A to the coating B is 15.6-15.8:24.4-26.6; The coating A is obtained by coating the coating A on the surface of the sample and drying it; The coating B is obtained by coating the coating B on the surface of the coating A and drying; The coating A comprises the following raw materials in parts by weight: 23-25 ​​parts of polyurethane modified epoxy resin, 15-18 parts of polyoxypropylene grafted nano-silicon dioxide, and 5.7-6.45 parts of butyl glycidyl ether; The coating B comprises the following raw materials in parts by weight: 6-9 parts of polyamide grafted wear-resistant additive, 18-21 parts of polymer-modified aluminum hydroxide nanosheets, 3.6-4.5 parts of butyl glycidyl ether, and 14-18 parts of aminopropyl triethoxysilane; The preparation method of the polyamide grafted wear-resistant additive is as follows: Plasma treatment is performed on the wear-resistant additive, and any one of compressed air, nitrogen, oxygen and argon is used as plasma. The treated wear-resistant additive is added to polyamide, and reacted at a temperature of 90-100° C. and a stirring speed of 100-120 r / min for 6-8 hours to obtain a polyamide-grafted wear-resistant additive; The mass ratio of the wear-resistant additive to the polyamide is 40-43:8-11, and the wear-resistant additive is one or more of nano-tungsten carbide, zirconium oxide, aluminum oxide and silicon carbide mixed in any proportion; The preparation method of the polymer-modified aluminum hydroxide nanosheets is as follows: Step C1. dissolving aluminum sec-butoxide and aluminum isopropoxide in water, adding 12-(2-bromoisobutyrylamino) dodecanoic acid, heating to 60-70° C., reacting for 2-3 hours to obtain a reaction solution, precipitating and purifying the reaction solution 3-5 times to obtain aluminum bromide hydroxide nanosheets; Step C2. dissolving aluminum hydroxide bromide nanosheets in N,N-dimethylformamide, adding acrylonitrile, copper bromide and 2,2'-bipyridine, deoxygenating with nitrogen, freezing into a solid with liquid nitrogen, adding cuprous bromide, heating to 58-60°C and polymerizing for 8-9h to obtain polymer-modified aluminum hydroxide nanosheets; The mass ratio of aluminum sec-butoxide, aluminum isopropoxide, water and 12-(2-bromoisobutyrylamino)dodecanoic acid in step C1 is 4.8-5.1:4.8-5.1:90-100:0.4-0.5; The dosage ratio of the aluminum hydroxide bromide nanosheets, N,N-dimethylformamide, acrylonitrile, copper bromide, 2,2'-bipyridine and cuprous bromide in step C2 is 0.08-0.12 g: 10-12 mL: 80-100 mL: 0.08-0.1 g: 0.08-0.1 g: 0.02-0.04 g.

2. The wear-resistant and weather-resistant nano coating according to claim 1, characterized in that: The preparation method of the polyurethane modified epoxy resin is as follows: Step A1. Add half of the total amount of polytetrahydrofuran diol to 4,4'-diphenyl diisocyanate, heat the reaction to 70-75°C for 1-1.5h, then cool to 58-60°C, add the remaining polytetrahydrofuran diol, heat to 72-75°C for 80-90min, and generate an isocyanate-terminated polyurethane prepolymer; Step A2. Mix the terminal isocyanate polyurethane prepolymer and glycidol in an anhydrous dichloromethane solvent at a molar ratio of 1:2, and react at 38-42° C. for 3.5-4 hours under a nitrogen atmosphere to obtain a polyurethane-modified epoxy resin.

3. The wear-resistant and weather-resistant nano coating according to claim 2, characterized in that: The mass ratio of 4,4'-diphenyl diisocyanate to polytetrahydrofuran diol in step A1 is 480-520:100-120.

4. The wear-resistant and weather-resistant nano coating according to claim 1, characterized in that: The preparation method of the poly(propylene oxide)-grafted nano-silicon dioxide is as follows: Step B1. Anhydrous ethanol, distilled water and ammonia water are mixed, stirred at room temperature at a stirring speed of 500 r / min, and then tetraethyl orthosilicate and the second portion of anhydrous ethanol are added, and stirring is continued for 2.5-3h, and excess solvent is removed by high-speed centrifugation, washed with distilled water 3-5 times, and then vacuum dried to obtain nano-silicon dioxide; Step B2. In a nitrogen atmosphere, disperse the nano-silica in a sodium methoxide solution, ultrasonically shake for 8-12 minutes, continue the reaction for 50-60 minutes, stop the reaction, wash twice with 20 mL of anhydrous methanol, and then dry and grind to obtain pretreated nano-silica; Step B3. Mix the pretreated nano-silica and glycidol evenly, control the stirring speed to 400r / min, the temperature to 100-110°C, react for 40-45min under nitrogen protection, then centrifuge and wash 3-5 times with 30mL of a mixed solution of ethanol and water, and dry to obtain poly(glycidyl alcohol)-grafted nano-silica.

5. The wear-resistant and weather-resistant nano coating according to claim 4, characterized in that: The usage ratio of anhydrous ethanol, distilled water, ammonia water, tetraethyl orthosilicate and the second portion of anhydrous ethanol in step B1 is 800-900 mL: 70-72 g: 24-27 g: 122-126 g: 90-100 mL.

6. The wear-resistant and weather-resistant nano coating according to claim 4, characterized in that: The usage ratio of the nano-silicon dioxide and the sodium methoxide solution in step B2 is 5-5.2 g: 90-100 mL, and the concentration of the sodium methoxide solution is 0.3-0.4 mol / L.

7. The wear-resistant and weather-resistant nano coating according to claim 4, characterized in that: The mass ratio of the pretreated nano-silica to glycidol in step B3 is 4.6-5.2:10-12, and the mixed solution of ethanol and water is obtained by mixing ethanol and water in a volume ratio of 1:

1.

8. A method for preparing the wear-resistant and weather-resistant nano coating according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step S1. polyurethane modified epoxy resin, polypropylene oxide grafted nano-silica and butyl glycidyl ether are mixed evenly to obtain coating A, coating A is evenly applied on the surface of the sample and dried to obtain sample 1 with coating A on the surface; Step S2. Mix the polyamide grafted wear-resistant additive, polymer-modified aluminum hydroxide nanosheets, butyl glycidyl ether and aminopropyl triethoxysilane evenly to obtain coating B, and evenly apply coating B on the surface of sample 1 with coating A and dry it to obtain sample 2 with coating A and coating B on the surface, that is, to obtain wear-resistant and weather-resistant nano coating.

Citation Information

Patent Citations

  • Method for preparing anti-wear, anti-corrosion nano composite epoxy asphalt repair paint

    CN1821325A

  • Mirror back protective coating based on priming-finishing paint coupling technology, manufacture method and construction method

    CN101613560A

  • Preparation method of highly transparent wear-resistant superhydrophobic composite coating

    CN107022279A

  • Environment-friendly high-strength sealant composition and preparation method thereof

    CN107057629A

  • Wear-resistant anticorrosive paint for polar ships and preparation method thereof

    CN110903734A