A kind of friction-reducing and anti-wear high-temperature lubricating oil and preparation method thereof
By performing two modification treatments on MoS2 and using additives, the problem of poor agglomeration and dispersion of MoS2 in high-temperature lubricating oil is solved, which significantly improves the high-temperature tribological performance and stability of lubricating oil, and achieves wear and moisture resistance. .
Patent Information
- Application Number
- CN202410482742.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-04-22
AI Technical Summary
After the existing high-temperature lubricant is placed for a long time, MoS2 agglomerates and settles, resulting in a decrease in tribological properties, and the perfluoropolyether is incompatible with the dispersant, resulting in a delamination of the lubricant and a significant reduction in tribological properties.
MoS2 was modified twice: firstly, polydopamine and calcination formed carbide polydopamine-modified MoS2, increasing the surface wrinkle and reaction sites, and then further modification was performed using perfluoroalkylthiol or fluoro-containing silane. , improve the dispersion and tribological properties of MoS2 in perfluoropolyethers, and add additives such as oleamine and SPAN 80 to the lubricating oil to improve stability.
The dispersion of MoS2 in perfluoropolyether and the high-temperature tribological properties of lubricating oil are significantly improved, the friction coefficient is reduced, and the wear and moisture resistance is achieved.
Smart Images

Figure CN118580901B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a friction-reducing and anti-wear high-temperature lubricating oil and a preparation method thereof, belonging to the technical field of lubrication. Background Art
[0002] Tribology is a discipline about friction, wear and lubrication, and has always been an important research direction that has attracted much attention in materials science and engineering. Especially in high-temperature friction environments under extreme conditions, the lubrication effect and tribological properties of materials are particularly important, which directly affects the reliable operation of equipment in the fields of aerospace, energy, and industrial manufacturing. In this challenging context, materials scientists and engineers urgently need to have a deeper understanding of the microscopic mechanisms of tribological phenomena and optimize the performance of lubricating materials through innovative methods.
[0003] Perfluoropolyether, as an excellent polymer matrix, has attracted much attention due to its excellent thermal stability and corrosion resistance in high-temperature environments. The introduction of nanomaterials provides a new strategy for regulating the tribological properties of perfluoropolyether. MoS2, as a nanomaterial widely used in the field of tribology, is favored for its layered structure and excellent high-temperature lubrication properties. The structure, shape and dispersibility of molybdenum disulfide nanomaterials in lubricating oil determine its tribological properties.
[0004] In the prior art, MoS2 is generally mixed with perfluoropolyether, stirred and ultrasonically treated to obtain a high-temperature lubricating oil. However, after the high-temperature lubricating oil is left for a long time, MoS2 agglomerates and settles, causing the lubricating oil to degenerate and the tribological performance to be greatly reduced. The prior art also adopts the following scheme: perfluoropolyether is mixed with dispersant T154B (boronated polyisobutylene succinimide), then stirred and mixed with MoS2 and ultrasonically treated to obtain a high-temperature lubricating oil. However, perfluoropolyether is incompatible with T154B due to its low surface energy and high chemical inertness, and this lubricating oil is quickly stratified, causing the lubricating oil to degenerate and the tribological performance to be greatly reduced.
[0005] Therefore, how to improve the tribological properties of perfluoropolyether lubricants at high temperatures remains one of the urgent problems to be solved in this field. Summary of the invention
[0006] In order to solve the above technical problems, the object of the present invention is to provide a friction-reducing and anti-wear high-temperature lubricating oil and a preparation method thereof. The present invention can improve the dispersibility of MoS2 in perfluoropolyether, and can improve the ability of perfluoropolyether lubricating oil to reduce friction, resist wear and lubricate at high temperature.
[0007] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a friction-reducing and anti-wear high-temperature lubricating oil, which comprises the following steps:
[0008] (1)Modification of MoS2:
[0009] The MoS2 powder is dispersed in a first solvent and subjected to ultrasonic treatment for a period of time; polydopamine is then added and reacted under stirring for a period of time; a solid product is obtained after separation, washing and drying; and the solid product is calcined in a protective gas environment to obtain a first modified MoS2;
[0010] The first modified MoS2 is dispersed in a second solvent and subjected to ultrasonic treatment for a period of time; then perfluoroalkylthiol or the first fluorine-containing silane is added and reacted under stirring for a period of time; then separated, washed and dried to obtain the second modified MoS2;
[0011] (2) Preparation of lubricating oil:
[0012] The secondary modified MoS2, perfluoropolyether and second fluorinated silane obtained in step (1) are mixed, stirred for a period of time, and then ultrasonically treated for a period of time to obtain the friction-reducing and anti-wear high-temperature lubricating oil.
[0013] In the above preparation method, preferably, in step (1), the first solvent comprises an ethanol aqueous solution with a volume concentration of 30-60%.
[0014] In the above-mentioned preparation method, preferably, in step (1), the volume mass ratio of the first solvent to the MoS2 powder is 100-500mL:1g.
[0015] In the above preparation method, preferably, in step (1), the time for dispersing MoS2 powder in the first solvent and subjecting it to ultrasonic treatment is 2-16 hours. Specifically, the power of the ultrasonic treatment can be 100-600w, and the frequency can be 20-25kHz.
[0016] In the above-mentioned preparation method, preferably, in step (1), the mass ratio of the MoS2 powder to the polydopamine is 1-5:1.
[0017] In the above preparation method, preferably, in step (1), the reaction time after adding polydopamine under stirring conditions is 10-48 hours.
[0018] In the above preparation method, preferably, in step (1), the solid product is calcined in a protective gas environment at a temperature of 200-350° C. for 2-12 hours, wherein the protective gas includes but is not limited to nitrogen.
[0019] In the above preparation method, preferably, in step (1), the second solvent comprises an ethanol aqueous solution with a volume concentration of 30-60%.
[0020] In the above-mentioned preparation method, preferably, in step (1), the volume mass ratio of the second solvent to the once-modified MoS2 is 100-500 mL:1 g.
[0021] In the above preparation method, preferably, in step (1), the time for dispersing the once modified MoS2 in the second solvent and subjecting it to ultrasonic treatment is 2-16 hours. Specifically, the power of the ultrasonic treatment can be 100-600w, and the frequency can be 20-25kHz.
[0022] In the above-mentioned preparation method, preferably, in step (1), the mass ratio of the once-modified MoS2 and the perfluoroalkylthiol or the first fluorine-containing silane is 1-5:1.
[0023] In the above preparation method, preferably, in step (1), the perfluoroalkylthiol includes 1H,1H,2H,2H-perfluorooctanethiol and / or 1H,1H,2H,2H-perfluorododecanethiol and the like.
[0024] In the above preparation method, preferably, in step (1), the first fluorine-containing silane includes one or a combination of trichloro(1H,1H,2H,2H-tridecafluorooctyl)silane, perfluorodecyltriethoxysilane and trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane, etc. More preferably, the first fluorine-containing silane is trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane.
[0025] In the above preparation method, preferably, in step (1), the reaction time after adding the perfluoroalkylthiol or the first fluorine-containing silane under stirring is 10-48 hours.
[0026] In step (1) of the above preparation method, the separation, washing and drying can all be carried out by conventional techniques in the art, for example, separation can be carried out by filtration, washing can be carried out by washing with deionized water for 2-5 times, and drying can be carried out by freeze drying. The freeze drying temperature can be -50°C to -20°C, the vacuum degree can be -0.01kPa to -0.1kPa, and the time can be 10-48h.
[0027] In step (1) of the preparation method of the present invention, MoS2 is modified to improve the performance of MoS2, thereby improving the performance of the lubricating oil. In the modification method of the present invention, MoS2 is first modified by polydopamine, and after calcination, carbonized polydopamine-modified MoS2, i.e., primary modified MoS2, is obtained; a large amount of residual carbon remains on the surface of the carbonized polydopamine-modified MoS2, which increases the wrinkle degree of the modified MoS2 surface, increases its specific surface area, and increases the reaction sites with subsequent perfluoroalkyl mercaptan or the first fluorinated silane. Afterwards, the carbonized polydopamine-modified MoS2 is further modified by perfluoroalkyl mercaptan or the first fluorinated silane, and the S atoms of the perfluoroalkyl mercaptan supplement the S vacancies of MoS2, thereby improving the tribological properties of the secondary modified MoS2 in a humid environment, and at the same time, due to the presence of fluorine groups in the perfluoroalkyl mercaptan and the first fluorinated silane, the dispersibility of the secondary modified MoS2 in perfluoropolyether is improved. Therefore, the lubricating oil prepared by using the secondary modified MoS2 of the present invention not only has improved high-temperature tribological properties, but also has good moisture resistance.
[0028] In the above-mentioned preparation method, preferably, in step (2), the mixing mass ratio of the secondary modified MoS2, the perfluoropolyether and the second fluorinated silane is 0.1:(5-10):(0.01-0.2).
[0029] In the above preparation method, preferably, in step (2), the second fluorine-containing silane includes one or a combination of trichloro(1H,1H,2H,2H-tridecafluorooctyl)silane, perfluorodecyltriethoxysilane and trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane, etc. More preferably, the second fluorine-containing silane is trichloro(1H,1H,2H,2H-tridecafluorooctyl)silane.
[0030] In step (2) of the preparation method of the present invention, a second fluorine-containing silane is mixed with the secondary modified MoS2 and perfluoropolyether, so that the unreacted hydroxyl groups on the surface of the secondary modified MoS2 react with the second fluorine-containing silane (the reaction is rapid) to form new chains, which helps to further stabilize the dispersion of the secondary modified MoS2 in the perfluoropolyether.
[0031] In the above-mentioned preparation method, preferably, step (2) comprises: mixing the secondary modified MoS2, perfluoropolyether and second fluorine-containing silane obtained in step (1), adding additives, stirring for a period of time, and then ultrasonically treating for a period of time to obtain the friction-reducing and anti-wear high-temperature lubricating oil.
[0032] In the above preparation method, preferably, in step (2), the additives include oleylamine, SPAN 80 and cetyltrimethylammonium bromide; based on 1 part by mass of the perfluoropolyether, the amount of oleylamine added is 0.01-0.1 part by mass, the amount of SPAN 80 added is 0.01-0.1 part by mass, and the amount of cetyltrimethylammonium bromide added is 0.01-0.1 part by mass.
[0033] In step (2) of the preparation method of the present invention, the above-mentioned additives are preferably further added to improve the dispersibility and suspension stability of the secondary modified MoS2 in perfluoropolyether and improve the storage stability of the lubricating oil.
[0034] In the above preparation method, preferably, in step (2), the stirring time is 5-30 min, and the ultrasonic treatment time is 2-15 h. Specifically, the power of the ultrasonic treatment can be 100-600 w, and the frequency can be 20-25 kHz.
[0035] The second aspect of the present invention provides a friction-reducing, anti-wear, and high-temperature lubricating oil, which is prepared by the above-mentioned method for preparing the friction-reducing, anti-wear, and high-temperature lubricating oil.
[0036] The present invention provides a friction-reducing and anti-wear high-temperature lubricating oil and a preparation method thereof. The present invention explores a method for regulating the interaction between MoS2 and perfluoropolyether, and also explores a method for regulating the surface chemistry and structure of MoS2, and creatively develops a method for modifying the MoS2 of the present invention. The secondary modified MoS2 of the present invention has improved dispersibility in perfluoropolyether, and may have improved tribological properties in a humid environment. The present invention uses fluorinated silane to mix with the secondary modified MoS2 and perfluoropolyether, and preferably further adds an additive selected by the present invention, which helps to further stably disperse the secondary modified MoS2 in the perfluoropolyether, and improve its dispersibility and suspension stability. Therefore, the friction-reducing and anti-wear high-temperature lubricating oil provided by the present invention has excellent friction reduction ability, wear resistance ability and lubrication performance at high temperatures, and may also have good moisture resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 These are the water contact angle test results of the secondary modified MoS2 prepared in Example 1 and the raw MoS2 powder. DETAILED DESCRIPTION
[0038] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0039] Example 1
[0040] (1)Modification of MoS2:
[0041] 4 g of MoS2 powder (average particle size of 800 nm) was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g of polydopamine was added and reacted for 24 h under stirring conditions; then filtered, washed with deionized water 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain a solid product; then the solid product was calcined at 300 ° C in a nitrogen environment for 4 h to obtain a first modified MoS2;
[0042] 4 g of the first modified MoS2 was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g of 1H,1H,2H,2H-perfluorododecanethiol was added dropwise and reacted for 24 h under stirring conditions; then filtered, washed with deionized water 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain the second modified MoS2;
[0043] (2) Preparation of lubricating oil:
[0044] 0.1 g of secondary modified MoS2 was added to 5 g of perfluoropolyether, and then 0.075 g of trichloro(1H,1H,2H,2H-tridecafluorooctyl)silane was added dropwise, stirred for 5 min, and then ultrasonically treated for 2 h (power of 300 W and frequency of 20 kHz) to obtain a friction-reducing and anti-wear high-temperature lubricating oil.
[0045] The water contact angle of the secondary modified MoS2 prepared in step (1) of this embodiment and the raw material MoS2 powder used are tested. The specific steps include: dropping a water drop on the surface of the secondary modified MoS2 or the raw material MoS2, adjusting the goniometer so that the contact line coincides with the goniometer, and then reading the angle on the dial to obtain the water contact angle. The water contact angles of the secondary modified MoS2 and the raw material MoS2 powder are as follows: Figure 1 As shown. Figure 1 It can be seen that compared with the unmodified MoS2, the water contact angle of the secondarily modified MoS2 in this embodiment is greatly improved.
[0046] Example 2
[0047] (1)Modification of MoS2:
[0048] 4 g of MoS2 powder (average particle size of 800 nm) was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g of polydopamine was added and reacted for 24 h under stirring conditions; then filtered, washed with deionized water 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain a solid product; then the solid product was calcined at 300 ° C in a nitrogen environment for 4 h to obtain a first modified MoS2;
[0049] 4 g of the first modified MoS2 was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g of 1H,1H,2H,2H-perfluorododecanethiol was added dropwise and reacted for 24 h under stirring conditions; then filtered, washed with deionized water 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain the second modified MoS2;
[0050] (2) Preparation of lubricating oil:
[0051] 0.1 g of secondary modified MoS2 was added to 5 g of perfluoropolyether, and then 0.075 g of trichloro(1H,1H,2H,2H-tridecafluorooctyl)silane was added dropwise, followed by 0.05 g of oleylamine, 0.05 g of SPAN 80 and 0.05 g of hexadecyltrimethylammonium bromide. The mixture was stirred for 5 min and then ultrasonically treated for 2 h (power of 300 W and frequency of 20 kHz) to obtain a friction-reducing and anti-wear high-temperature lubricating oil.
[0052] Example 3
[0053] (1)Modification of MoS2:
[0054] 4 g of MoS2 powder (average particle size of 800 nm) was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g of polydopamine was added and reacted for 24 h under stirring conditions; then filtered, washed with deionized water 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain a solid product; then the solid product was calcined at 300 ° C in a nitrogen environment for 4 h to obtain a first modified MoS2;
[0055] 4 g of the first modified MoS2 was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g of trimethoxy (1H, 1H, 2H, 2H-heptadecafluorodecyl) silane was added dropwise and reacted for 24 h under stirring; then filtered, washed with deionized water 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain the second modified MoS2;
[0056] (2) Preparation of lubricating oil:
[0057] 0.1 g of secondary modified MoS2 was added to 5 g of perfluoropolyether, and then 0.075 g of trichloro(1H,1H,2H,2H-tridecafluorooctyl)silane was added dropwise, stirred for 5 min, and then ultrasonically treated for 2 h (power of 300 W and frequency of 20 kHz) to obtain a friction-reducing and anti-wear high-temperature lubricating oil.
[0058] Example 4
[0059] (1)Modification of MoS2:
[0060] 4 g of MoS2 powder (average particle size of 800 nm) was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g of polydopamine was added and reacted for 24 h under stirring conditions; then filtered, washed with deionized water 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain a solid product; then the solid product was calcined at 300 ° C in a nitrogen environment for 4 h to obtain a first modified MoS2;
[0061] 4 g of the first modified MoS2 was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g of trimethoxy (1H, 1H, 2H, 2H-heptadecafluorodecyl) silane was added dropwise and reacted for 24 h under stirring; then filtered, washed with deionized water 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain the second modified MoS2;
[0062] (2) Preparation of lubricating oil:
[0063] 0.1 g of secondary modified MoS2 was added to 5 g of perfluoropolyether, and then 0.075 g of trichloro(1H,1H,2H,2H-tridecafluorooctyl)silane was added dropwise, followed by 0.05 g of oleylamine, 0.05 g of SPAN 80 and 0.05 g of hexadecyltrimethylammonium bromide. The mixture was stirred for 5 min and then ultrasonically treated for 2 h (power of 300 W and frequency of 20 kHz) to obtain a friction-reducing and anti-wear high-temperature lubricating oil.
[0064] Comparative Example 1
[0065] (1)Modification of MoS2:
[0066] 4 g MoS2 powder (average particle size of 800 nm) was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g 1H,1H,2H,2H-perfluorododecanethiol was added dropwise and reacted for 24 h under stirring conditions; then the mixture was filtered, washed with deionized water for 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain modified MoS2;
[0067] (2) Preparation of lubricating oil:
[0068] 0.1 g of modified MoS2 was added to 5 g of perfluoropolyether, and then 0.075 g of trichloro(1H,1H,2H,2H-tridecafluorooctyl)silane was added dropwise, stirred for 5 min, and then ultrasonically treated for 2 h (power of 300 W and frequency of 20 kHz) to obtain high-temperature lubricating oil.
[0069] Comparative Example 2
[0070] (1)Modification of MoS2:
[0071] 4 g of MoS2 powder (average particle size of 800 nm) was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g of polydopamine was added and reacted for 24 h under stirring conditions; then filtered, washed with deionized water 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain a solid product; then the solid product was calcined at 300 ° C in a nitrogen environment for 4 h to obtain a first modified MoS2;
[0072] 4 g of the first modified MoS2 was dispersed in 500 mL of 45% ethanol aqueous solution and ultrasonically treated for 8 h (power of 300 w, frequency of 20 kHz); then 2 g of 1H,1H,2H,2H-perfluorododecanethiol was added dropwise and reacted for 24 h under stirring conditions; then filtered, washed with deionized water 3 times and freeze-dried (temperature of -50 ° C, vacuum degree of -0.1 kPa, time of 24 h) to obtain the second modified MoS2;
[0073] (2) Preparation of lubricating oil:
[0074] 0.1 g of secondary modified MoS2 was added to 5 g of perfluoropolyether, stirred for 5 min, and then ultrasonically treated for 2 h (power of 300 W and frequency of 20 kHz) to obtain high-temperature lubricating oil.
[0075] Test Case
[0076] The friction coefficients of pure perfluoropolyether and the high-temperature lubricating oils provided in Examples 1 to 4 and Comparative Examples 1 to 2 at 200° C. were tested using a UMT5 friction and wear tester, and the results are shown in Table 1. The specific steps include: using a UMT5 friction and wear tester, the materials of the upper and lower samples are both GCr15, the upper sample is a 6 mm ball, the lower sample is a disc, the upper sample rotates on the surface of the lower sample, the rotation radius is 3 mm, the rotation speed is 300 rpm, the load is 1 N, and the test time is 2000 s.
[0077] The wear rate of pure perfluoropolyether and the high temperature lubricating oil provided in Examples 1 to 4 and Comparative Examples 1 to 2 was tested using a three-dimensional white light tester, and the results are shown in Table 1. The test procedure for the wear rate is the same as the test procedure for the friction coefficient. After the test is completed, the wear rate of the sample is analyzed using a three-dimensional white light tester. The calculation formula for the wear rate is as follows:
[0078] W = (△V) / (F × d); where W is the wear rate, in m 2 / N; △V is the wear volume, unit is m 3 ; F is the normal load, unit is N; d is the total stroke, unit is m.
[0079] Table 1
[0080]
[0081] It can be seen from Table 1 that at 200°C, the friction coefficient of the anti-friction and anti-wear high-temperature lubricating oil provided by the embodiment of the present invention can reach 0.041, which is 56.8% lower than the friction coefficient of 0.095 of pure perfluoropolyether. At the same time, the anti-friction and anti-wear high-temperature lubricating oil provided by the embodiment of the present invention achieves almost zero wear. Compared with the high-temperature lubricating oil provided by Comparative Examples 1 to 2, the friction coefficient of the anti-friction and anti-wear high-temperature lubricating oil provided by the embodiment of the present invention is reduced, and the wear is greatly reduced.
[0082] In summary, the friction-reducing and anti-wear high-temperature lubricating oil provided by the present invention has excellent friction-reducing ability, wear-resisting ability and lubricating performance at high temperatures.
Claims
1. A method for preparing a friction-reducing and anti-wear high-temperature lubricating oil, comprising the following steps: (1) Modification of MoS2: Dispersing MoS2 powder in a first solvent and subjecting it to ultrasonic treatment for a period of time; Then, polydopamine is added and reacted for a period of time under stirring conditions; then, a solid product is obtained through separation, washing and drying; and the solid product is calcined in a protective gas environment to obtain a first modified MoS2; Dispersing the once modified MoS2 in a second solvent and subjecting it to ultrasonic treatment for a period of time; Then, perfluoroalkylthiol is added and reacted for a period of time under stirring conditions; after separation, washing and drying, the secondary modified MoS2 is obtained; Wherein, the first solvent comprises an ethanol aqueous solution with a volume concentration of 30-60%; the volume mass ratio of the first solvent to the MoS2 powder is 100-500mL:1g; the time for dispersing the MoS2 powder in the first solvent and performing ultrasonic treatment is 2-16h; The second solvent comprises an ethanol aqueous solution with a volume concentration of 30-60%; the volume mass ratio of the second solvent to the once-modified MoS2 is 100-500mL:1g; the time for dispersing the once-modified MoS2 in the second solvent and performing ultrasonic treatment is 2-16h; (2) Preparation of lubricating oil: The secondary modified MoS2, perfluoropolyether and fluorinated silane obtained in step (1) are mixed, stirred for a period of time, and then ultrasonically treated for a period of time to obtain the friction-reducing and anti-wear high-temperature lubricating oil; The fluorine-containing silane includes one or a combination of trichloro(1H,1H,2H,2H-tridecafluorooctyl)silane, perfluorodecyltriethoxysilane and trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane.
2. The preparation method according to claim 1, wherein In step (1), the mass ratio of the MoS2 powder to the polydopamine is 1-5:1; In step (1), after adding polydopamine, the reaction time under stirring conditions is 10-48 hours; In step (1), the solid product is calcined in a protective gas environment at a temperature of 200-350° C. for a time of 2-12 hours.
3. The preparation method according to claim 1, wherein In step (1), the mass ratio of the primary modified MoS2 to the perfluoroalkylthiol is 1-5:1; In step (1), the perfluoroalkylthiol includes 1H,1H,2H,2H-perfluorooctanethiol and / or 1H,1H,2H,2H-perfluorododecanethiol; In step (1), the reaction time after adding perfluoroalkylthiol under stirring conditions is 10-48 hours.
4. The preparation method according to claim 1, wherein In step (2), the mixing mass ratio of the secondary modified MoS2, the perfluoropolyether and the fluorinated silane is 0.1:(5-10):(0.01-0.2).
5. The preparation method according to claim 1, wherein Step (2) comprises: mixing the secondary modified MoS2, perfluoropolyether and fluorinated silane obtained in step (1), adding additives, stirring for a period of time, and ultrasonically treating for a period of time to obtain the friction-reducing and anti-wear high-temperature lubricating oil.
6. The preparation method according to claim 5, wherein: In step (2), the additives include oleylamine, SPAN80 and cetyltrimethylammonium bromide; based on 1 part by mass of the perfluoropolyether, the amount of oleylamine added is 0.01-0.1 part by mass, the amount of SPAN 80 added is 0.01-0.1 part by mass, and the amount of cetyltrimethylammonium bromide added is 0.01-0.1 part by mass.
7. The preparation method according to claim 1 or 5, wherein: In step (2), the stirring time is 5-30 min, and the ultrasonic treatment time is 2-15 h.
8. A friction-reducing, anti-wear, high-temperature lubricating oil, which is prepared by the method for preparing the friction-reducing, anti-wear, high-temperature lubricating oil according to any one of claims 1 to 7.