A kind of UV-proof composite fabric filled with biological natural crystal powder and preparation method thereof
By modifying graphene, including oxidation and grafting, and combining it with nano-titanium dioxide, the problem of graphene agglomeration on the surface of fabric fibers is solved, and the UV resistance of the fabric is improved.
Patent Information
- Application Number
- CN202411037733.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-31
AI Technical Summary
In the existing technology, graphene is easy to agglomerate on the surface of fabric fibers, which affects the improvement of its anti-ultraviolet performance, and the dispersant effect is not obvious.
By modifying graphene, graphene oxide is first prepared under the oxidation of potassium permanganate and hydrogen peroxide, grafted with sodium carboxymethylcellulose to carry a negative charge, and combined with nanometer titanium dioxide to avoid agglomeration and enhance dispersion properties.
It effectively solves the problem of graphene agglomeration, improves its dispersion performance and UV resistance on fabrics, and enhances the UV protection ability of fabrics.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new fabric materials, and in particular to an anti-ultraviolet composite fabric filled with biological natural crystal powder and a preparation method thereof. Background Art
[0002] As the core of the clothing industry, clothing fabrics are the key factors that determine the performance and appearance of clothing. With the advancement of science and technology and the diversification of consumer demand, the innovation of clothing fabrics has become an important driving force for the development of the industry. The current clothing fabric technology on the market is quite mature, but with the improvement of consumer requirements for clothing functionality, comfort, environmental protection, etc., the existing technology faces new challenges. The progress of materials science has provided unlimited possibilities for the innovation of clothing fabrics. The application of cutting-edge technologies such as nanotechnology, bioengineering technology, and smart materials has made fabrics more functional and intelligent.
[0003] Ultraviolet (UV) radiation is a part of sunlight and has certain harmfulness. It not only causes fabric aging and fading, but also may cause damage to human skin, such as sunburn, spots, and even induce skin cancer. Therefore, the development of fabrics with UV resistance has become an important research direction in the textile industry. Graphene, which is mainly composed of a layered structure formed by sp2 hybridization of carbon atoms, has good chemical stability and conductivity. In recent years, graphene and its derivatives (such as graphene) have shown great application potential in the field of UV-resistant fabrics due to their unique physical and chemical properties.
[0004] Chinese patent publication number CN110699945 discloses a sunscreen and anti-ultraviolet sports fabric and its preparation method, which includes the following steps: treating the fabric with a NaOH aqueous solution; immersing the treated fabric in a citric acid solution, adding graphene, stirring at high temperature to react, and after the reaction system cools to room temperature, taking out the fabric and drying it; immersing the fabric in a finishing agent composed of amino silicone oil, triethanolamine, sodium tripolyphosphate, polybutyl acrylate, lauryl methacrylate, carboxymethyl cellulose, sodium lauryl alcohol polyether sulfate, fatty alcohol polyoxyethylene ether, ethanol, and water, and washing and baking to obtain a sunscreen and anti-ultraviolet sports fabric. In this patented technical solution, the fabric is given anti-ultraviolet properties by immersing it in a liquid containing graphene, but graphene is prone to agglomeration, which affects the improvement of graphene on the anti-ultraviolet properties of the fabric. Summary of the invention
[0005] In order to overcome the above problems in the prior art, the present invention provides an anti-ultraviolet composite fabric filled with biological natural crystal powder and a preparation method thereof.
[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0007] A method for preparing an anti-ultraviolet composite fabric filled with biological natural crystal powder comprises the following steps:
[0008] S1, mixing nylon chips, natural crystal powder and spinning aids uniformly to obtain a mixture;
[0009] S2, adding the mixed material into a melt spinning machine for spinning, and then cold-cutting the spun filament bundle into shape;
[0010] S3, applying oil to the formed tow, and then drawing and winding the tow in sequence to obtain nylon fiber;
[0011] S4, blending the cotton fiber with the nylon fiber to obtain a blended yarn, and weaving the blended yarn to obtain a nylon / cotton blended fabric;
[0012] S5, adding graphene to the aqueous polyurethane solution, stirring and mixing evenly to form a suspension, and then immersing the nylon / cotton blended fabric in the suspension. After the immersion is completed, the textile is placed in an oven for drying.
[0013] The nylon of the present invention is mixed with natural crystal powder, which produces a unique and stable frequency, can enhance the human immune system, promote the rapid discharge of toxins from the body and increase the oxygen level. Since this special frequency is at the same vibration frequency as that of humans, it has the functions of reducing muscle tension, slowing down the heartbeat, relaxing breathing, increasing the body's oxygen content, releasing pressure and improving sleep.
[0014] As a new type of two-dimensional carbon material, graphene has shown great application potential in the field of UV resistance due to its unique structure and properties. The present invention uses water-based polyurethane as an adhesive to coat the graphene adhesive on the surface of the fabric fiber to form an anti-ultraviolet coating on the surface of the fabric fiber, giving the fabric excellent anti-ultraviolet performance.
[0015] Preferably, in step S1, the mass ratio of nylon chips, natural crystal powder and spinning aid is 1:0.08:0.01.
[0016] Preferably, in step S1, the natural crystal powder is mixed with the following substances:
[0017] Fluorite powder, orange crystal calcite powder, graphite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, rose crystal powder, aventurine powder, red jasper powder, serpentine powder.
[0018] The present invention blends natural crystal powder with nylon slices. Natural crystal powder is a natural energy medium. By interacting with the human energy field, it can regulate and balance the human energy, relieve mental stress and promote relaxation, improve the human energy level, and is beneficial to human health.
[0019] Preferably, in step S4, the blending ratio of cotton fiber to nylon fiber is 1:1-5.
[0020] Preferably, in step S5, the concentration of the aqueous polyurethane solution is 5-10wt%.
[0021] Preferably, in step S5, the graphene is subjected to modification treatment, the steps being as follows:
[0022] S51, adding graphene to a sulfuric acid solution, cooling to below 0°C, adding potassium permanganate, stirring evenly and heating, then adding an aqueous hydrogen peroxide solution for oxidation reaction, filtering and separating the graphene, washing with water and drying to obtain graphene oxide;
[0023] S52, adding TiCl4 to ammonia water, stirring to react, obtaining a white precipitate, adding oxalic acid to the white precipitate, stirring to dissolve, obtaining a titanium oxalate solution; adding graphene oxide, ammonium acetate and citric acid to the titanium oxalate solution, heating and stirring to react, standing for aging, and calcining at high temperature to obtain a titanium dioxide-graphene oxide composite;
[0024] S53, adding sodium carboxymethyl cellulose into water, stirring and dissolving, preparing a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.5%, adding an acid catalyst into the sodium carboxymethyl cellulose solution, stirring and mixing evenly, then adding titanium dioxide-graphene oxide composite, heating to 80°C, keeping warm for reaction, and after the reaction is completed, filtering, washing and drying in sequence to obtain the product.
[0025] The present invention found that when adding graphene to an aqueous polyurethane solution, graphene had agglomeration problems. A large amount of agglomerated graphene existed in a part of the surface of the fabric fiber, while the amount of graphene was scarce in another part, which seriously affected the improvement of the anti-ultraviolet performance of the fabric fiber by graphene. However, the dispersion effect of graphene by using a general dispersant was not obvious. Therefore, the present invention modified the graphene, firstly preparing graphene oxide under the oxidation action of potassium permanganate and hydrogen peroxide, so that the graphene surface was loaded with active functional groups such as epoxy and hydroxyl groups. Under the action of an acidic catalyst, the reaction activity of the epoxy group was used to react with the hydroxyl groups on the sodium carboxymethyl cellulose molecules to undergo a ring-opening reaction, thereby loading the carboxymethyl cellulose on the graphene surface. The sodium carboxymethyl cellulose grafted on the graphene surface would ionize -COO in the polyurethane aqueous solution. - , so that the graphene surface carries a negative charge. Under the action of electrostatic repulsion, the graphenes repel each other, thus solving the problem of graphene agglomeration.
[0026] Further research found in the experimental process: although the grafting of sodium carboxymethyl cellulose on the graphene surface can improve the dispersion performance of graphene, carboxymethyl cellulose will cause a certain shielding effect on the anti-ultraviolet performance of graphene. To solve the above problems, the present invention uses TiCl4 as a titanium source and deposits a certain amount of nano-titanium dioxide on the graphene surface. On the one hand, nano-titanium dioxide is combined with the graphene surface, reducing a certain amount of epoxy group binding sites on the graphene surface, thereby reducing the carboxymethyl cellulose grafted on the graphene surface. Avoid excessive carboxymethyl cellulose from causing a shielding effect on the anti-ultraviolet performance of graphene. On the other hand, nano-titanium dioxide reflects and scatters ultraviolet rays, further enhancing the anti-ultraviolet performance of the fabric.
[0027] Preferably, in step S51, the mass ratio of graphene to potassium permanganate is 1:3-8.
[0028] Preferably, in step S51, the concentration of the aqueous hydrogen peroxide solution is 10-20 wt %.
[0029] Preferably, in step S53, the insulation reaction time is controlled within a range of 120-152 minutes.
[0030] A UV-proof composite fabric filled with biological natural crystal powder is prepared by the above method.
[0031] The present invention has the following beneficial effects:
[0032] 1) Natural crystal powder is mixed into nylon. Natural crystal powder produces a unique and stable frequency that can enhance the human immune system, promote the rapid discharge of toxins from the body and increase oxygen levels. Since this special frequency is at the same vibration frequency as humans, it has the functions of reducing muscle tension, slowing down heartbeat, relaxing breathing, increasing body oxygen content, releasing stress and improving sleep;
[0033] 2) Using water-based polyurethane as adhesive, graphene adhesive is applied to the surface of fabric fibers to form an anti-ultraviolet coating on the surface of fabric fibers, giving the fabric excellent anti-ultraviolet properties;
[0034] 3) Sodium carboxymethyl cellulose grafted on the graphene surface will ionize -COO in polyurethane aqueous solution - , so that the graphene surface carries a negative charge. Under the action of electrostatic repulsion, the graphenes repel each other, thus improving the dispersion performance of graphene.
[0035] 4) Deposit a certain amount of nano-titanium dioxide on the graphene surface. On the one hand, nano-titanium dioxide is combined with the graphene surface, reducing a certain amount of epoxy group binding sites on the graphene surface, thereby reducing the carboxymethyl cellulose grafted on the graphene surface. Avoid excessive carboxymethyl cellulose from shielding the graphene's anti-ultraviolet properties; on the other hand, nano-titanium dioxide reflects and scatters ultraviolet rays, further enhancing the fabric's anti-ultraviolet properties. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0037] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.
[0038] Example 1
[0039] A method for preparing an anti-ultraviolet composite fabric filled with biological natural crystal powder comprises the following steps:
[0040] S1, mixing nylon 6 slices, natural crystal powder and spinning aid calcium stearate evenly, wherein the mass ratio of nylon slices, natural crystal powder and spinning aid is 1:0.08:0.01, to obtain a mixture;
[0041] As mentioned above, the natural crystal powder is mixed by the following substances in equal quantities:
[0042] Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, rose crystal powder, aventurine powder, red jasper powder, serpentine powder;
[0043] S2, adding the mixed material into a melt spinning machine for spinning, the spinning temperature is controlled at 220°C, and after the silk fibroin is ejected from the spinneret, it is cold cut into shape at room temperature;
[0044] S3, applying oil to the formed tow, and then drawing and winding the tow in sequence to obtain nylon fiber;
[0045] S4, blending the cotton fiber and the nylon fiber in a mass ratio of 1:4 to obtain a blended yarn, and weaving the blended yarn to obtain a nylon / cotton blended fabric;
[0046] S5, adding the modified graphene into an 8wt% aqueous polyurethane solution at a mass volume ratio of 1g / 200mL, stirring and mixing evenly to form a suspension, and then immersing the nylon / cotton blended fabric in the above suspension. After the immersion is completed, the textile is placed in an oven at 60°C for drying to obtain.
[0047] Preparation method of modified graphene:
[0048] S51, adding graphene to a sulfuric acid solution at a mass volume ratio of 1g / 80mL, cooling to below 0°C, adding potassium permanganate, the mass ratio of graphene to potassium permanganate is 1:7, stirring evenly and heating to 70°C, keeping warm for 50min, then adding a 18wt% aqueous hydrogen peroxide solution for oxidation reaction, the volume ratio of sulfuric acid solution to hydrogen peroxide solution is 1:0.8, filtering and separating the graphene, washing with water and drying to obtain graphene oxide;
[0049] S52, adding TiCl4 to ammonia water, the volume ratio of TiCl4 to ammonia water is 1:4, stirring to react, obtaining a white precipitate, adding the white precipitate to oxalic acid with a mass concentration of 10% at a mass volume ratio of 1g / 100mL, stirring to dissolve, and obtaining a titanium oxalate solution; adding graphene oxide, ammonium acetate and citric acid to the titanium oxalate solution, the mass ratio of graphene oxide, ammonium acetate and citric acid is 10:2:1, the mass volume ratio of graphene oxide to the titanium oxalate solution is 1g / 80mL, heating to 80°C, stirring to react for 2h, standing to age for 10h, separating, placing at 180°C for 20min, and then calcining at 600°C for 3h to obtain a titanium dioxide-graphene oxide composite;
[0050] S53, adding sodium carboxymethyl cellulose into water and stirring to dissolve to prepare a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.5%, adding an acid catalyst to the sodium carboxymethyl cellulose solution, the acid catalyst added in an amount of 0.05wt% of the acid in the sodium carboxymethyl cellulose aqueous solution, the catalyst being a mixture of SnCl4 and 10wt% hydrochloric acid, the mass volume ratio of the two being 0.001:1, stirring to mix evenly, and then adding titanium dioxide-graphene oxide composite at a mass volume ratio of 1g / 150mL, heating to 80°C, keeping the temperature for reaction for 150min, filtering, washing and drying in sequence after the reaction is completed to obtain the product.
[0051] Example 2
[0052] A method for preparing an anti-ultraviolet composite fabric filled with biological natural crystal powder comprises the following steps:
[0053] S1, mixing nylon 6 slices, natural crystal powder and spinning aid calcium stearate evenly, wherein the mass ratio of nylon slices, natural crystal powder and spinning aid is 1:0.08:0.01, to obtain a mixture;
[0054] As mentioned above, the natural crystal powder is mixed by the following substances in equal quantities:
[0055] Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, rose crystal powder, aventurine powder, red jasper powder, serpentine powder;
[0056] S2, adding the mixed material into a melt spinning machine for spinning, the spinning temperature is controlled at 220°C, and after the silk fibroin is ejected from the spinneret, it is cold cut into shape at room temperature;
[0057] S3, applying oil to the formed tow, and then drawing and winding the tow in sequence to obtain nylon fiber;
[0058] S4, blending the cotton fiber and the nylon fiber in a mass ratio of 1:2 to obtain a blended yarn, and weaving the blended yarn to obtain a nylon / cotton blended fabric;
[0059] S5, adding the modified graphene to a 6wt% aqueous polyurethane solution at a mass volume ratio of 1g / 200mL, stirring and mixing evenly to form a suspension, and then immersing the nylon / cotton blended fabric in the above suspension. After the immersion is completed, the textile is placed in an oven at 60°C for drying to obtain.
[0060] Preparation method of modified graphene:
[0061] S51, adding graphene to a sulfuric acid solution at a mass volume ratio of 1g / 80mL, cooling to below 0°C, adding potassium permanganate, the mass ratio of graphene to potassium permanganate is 1:4, stirring evenly and heating to 70°C, keeping warm for 50min, then adding a 12wt% aqueous hydrogen peroxide solution for oxidation reaction, the volume ratio of sulfuric acid solution to hydrogen peroxide solution is 1:0.8, filtering and separating the graphene, washing with water and drying to obtain graphene oxide;
[0062] S52, adding TiCl4 to ammonia water, the volume ratio of TiCl4 to ammonia water is 1:4, stirring to react, obtaining a white precipitate, adding the white precipitate to oxalic acid with a mass concentration of 10% at a mass volume ratio of 1g / 100mL, stirring to dissolve, and obtaining a titanium oxalate solution; adding graphene oxide, ammonium acetate and citric acid to the titanium oxalate solution, the mass ratio of graphene oxide, ammonium acetate and citric acid is 10:2:1, the mass volume ratio of graphene oxide to the titanium oxalate solution is 1g / 80mL, heating to 80°C, stirring to react for 2h, standing to age for 10h, separating, placing at 180°C for 20min, and then calcining at 600°C for 3h to obtain a titanium dioxide-graphene oxide composite;
[0063] S53, adding sodium carboxymethyl cellulose into water, stirring and dissolving to prepare a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.5%, adding an acid catalyst to the sodium carboxymethyl cellulose solution, the acid catalyst added in an amount of 0.05wt% of the acid in the sodium carboxymethyl cellulose aqueous solution, the catalyst being a mixture of SnCl4 and 10wt% hydrochloric acid, the mass volume ratio of the two being 0.001:1, stirring and mixing evenly, and then adding titanium dioxide-graphene oxide composite at a mass volume ratio of 1g / 150mL, heating to 80°C, keeping the temperature for reaction for 125min, filtering, washing and drying in sequence after the reaction is completed to obtain the product.
[0064] Example 3
[0065] A method for preparing an anti-ultraviolet composite fabric filled with biological natural crystal powder comprises the following steps:
[0066] S1, mixing nylon 6 slices, natural crystal powder and spinning aid calcium stearate evenly, wherein the mass ratio of nylon slices, natural crystal powder and spinning aid is 1:0.08:0.01, to obtain a mixture;
[0067] As mentioned above, the natural crystal powder is mixed by the following substances in equal quantities:
[0068] Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, rose crystal powder, aventurine powder, red jasper powder, serpentine powder;
[0069] S2, adding the mixed material into a melt spinning machine for spinning, the spinning temperature is controlled at 220°C, and after the silk fibroin is ejected from the spinneret, it is cold cut into shape at room temperature;
[0070] S3, applying oil to the formed tow, and then drawing and winding the tow in sequence to obtain nylon fiber;
[0071] S4, blending the cotton fiber and the nylon fiber in a mass ratio of 1:3 to obtain a blended yarn, and weaving the blended yarn to obtain a nylon / cotton blended fabric;
[0072] S5, adding the modified graphene into a 7wt% aqueous polyurethane solution at a mass volume ratio of 1g / 200mL, stirring and mixing evenly to form a suspension, and then immersing the nylon / cotton blended fabric in the above suspension. After the immersion is completed, the textile is placed in an oven at 60°C for drying to obtain.
[0073] Preparation method of modified graphene:
[0074] S51, adding graphene to a sulfuric acid solution at a mass volume ratio of 1g / 80mL, cooling to below 0°C, adding potassium permanganate, the mass ratio of graphene to potassium permanganate is 1:5, stirring evenly and heating to 70°C, keeping warm for 50min, then adding a 15wt% aqueous hydrogen peroxide solution for oxidation reaction, the volume ratio of sulfuric acid solution to hydrogen peroxide solution is 1:0.8, filtering and separating the graphene, washing with water and drying to obtain graphene oxide;
[0075] S52, adding TiCl4 to ammonia water, the volume ratio of TiCl4 to ammonia water is 1:4, stirring to react, obtaining a white precipitate, adding the white precipitate to oxalic acid with a mass concentration of 10% at a mass volume ratio of 1g / 100mL, stirring to dissolve, and obtaining a titanium oxalate solution; adding graphene oxide, ammonium acetate and citric acid to the titanium oxalate solution, the mass ratio of graphene oxide, ammonium acetate and citric acid is 10:2:1, the mass volume ratio of graphene oxide to the titanium oxalate solution is 1g / 80mL, heating to 80°C, stirring to react for 2h, standing to age for 10h, separating, placing at 180°C for 20min, and then calcining at 600°C for 3h to obtain a titanium dioxide-graphene oxide composite;
[0076] S53, adding sodium carboxymethyl cellulose into water, stirring and dissolving to prepare a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.5%, adding an acid catalyst to the sodium carboxymethyl cellulose solution, the acid catalyst added in an amount of 0.05wt% of the acid in the sodium carboxymethyl cellulose aqueous solution, the catalyst being a mixture of SnCl4 and 10wt% hydrochloric acid, the mass volume ratio of the two being 0.001:1, stirring and mixing evenly, and then adding titanium dioxide-graphene oxide composite at a mass volume ratio of 1g / 150mL, heating to 80°C, keeping the temperature for reaction for 135min, and filtering, washing and drying in sequence after the reaction is completed to obtain the product.
[0077] Example 4
[0078] A method for preparing an anti-ultraviolet composite fabric filled with biological natural crystal powder comprises the following steps:
[0079] S1, mixing nylon 6 slices, natural crystal powder and spinning aid calcium stearate evenly, wherein the mass ratio of nylon slices, natural crystal powder and spinning aid is 1:0.08:0.01, to obtain a mixture;
[0080] As mentioned above, the natural crystal powder is mixed by the following substances in equal quantities:
[0081] Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, rose crystal powder, aventurine powder, red jasper powder, serpentine powder;
[0082] S2, adding the mixed material into a melt spinning machine for spinning, the spinning temperature is controlled at 220°C, and after the silk fibroin is ejected from the spinneret, it is cold cut into shape at room temperature;
[0083] S3, applying oil to the formed tow, and then drawing and winding the tow in sequence to obtain nylon fiber;
[0084] S4, blending the cotton fiber and the nylon fiber in a mass ratio of 1:5 to obtain a blended yarn, and weaving the blended yarn to obtain a nylon / cotton blended fabric;
[0085] S5. Add the modified graphene to a 10wt% aqueous polyurethane solution at a mass volume ratio of 1g / 200mL, stir and mix evenly to form a suspension, and then immerse the nylon / cotton blended fabric in the suspension. After the immersion is completed, place the textile in an oven at 60°C for drying to obtain the product.
[0086] Preparation method of modified graphene:
[0087] S51, adding graphene to a sulfuric acid solution at a mass volume ratio of 1g / 80mL, cooling to below 0°C, adding potassium permanganate, the mass ratio of graphene to potassium permanganate is 1:8, stirring evenly and heating to 70°C, keeping warm for 50min, then adding a 20wt% aqueous hydrogen peroxide solution for oxidation reaction, the volume ratio of sulfuric acid solution to hydrogen peroxide solution is 1:0.8, filtering and separating the graphene, washing with water and drying to obtain graphene oxide;
[0088] S52, adding TiCl4 to ammonia water, the volume ratio of TiCl4 to ammonia water is 1:4, stirring to react, obtaining a white precipitate, adding the white precipitate to oxalic acid with a mass concentration of 10% at a mass volume ratio of 1g / 100mL, stirring to dissolve, and obtaining a titanium oxalate solution; adding graphene oxide, ammonium acetate and citric acid to the titanium oxalate solution, the mass ratio of graphene oxide, ammonium acetate and citric acid is 10:2:1, the mass volume ratio of graphene oxide to the titanium oxalate solution is 1g / 80mL, heating to 80°C, stirring to react for 2h, standing to age for 10h, separating, placing at 180°C for 20min, and then calcining at 600°C for 3h to obtain a titanium dioxide-graphene oxide composite;
[0089] S53, adding sodium carboxymethyl cellulose into water, stirring and dissolving to prepare a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.5%, adding an acid catalyst to the sodium carboxymethyl cellulose solution, the acid catalyst added in an amount of 0.05wt% of the acid in the sodium carboxymethyl cellulose aqueous solution, the catalyst being a mixture of SnCl4 and 10wt% hydrochloric acid, the mass volume ratio of the two being 0.001:1, stirring and mixing evenly, and then adding titanium dioxide-graphene oxide composite at a mass volume ratio of 1g / 150mL, heating to 80°C, keeping the temperature for reaction for 152min, and filtering, washing and drying in sequence after the reaction is completed to obtain the product.
[0090] Example 5
[0091] A method for preparing an anti-ultraviolet composite fabric filled with biological natural crystal powder comprises the following steps:
[0092] S1, mixing nylon 6 slices, natural crystal powder and spinning aid calcium stearate evenly, wherein the mass ratio of nylon slices, natural crystal powder and spinning aid is 1:0.08:0.01, to obtain a mixture;
[0093] As mentioned above, the natural crystal powder is mixed by the following substances in equal quantities:
[0094] Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, rose crystal powder, aventurine powder, red jasper powder, serpentine powder;
[0095] S2, adding the mixed material into a melt spinning machine for spinning, the spinning temperature is controlled at 220°C, and after the silk fibroin is ejected from the spinneret, it is cold cut into shape at room temperature;
[0096] S3, applying oil to the formed tow, and then drawing and winding the tow in sequence to obtain nylon fiber;
[0097] S4, blending the cotton fiber and the nylon fiber in a mass ratio of 1:1 to obtain a blended yarn, and weaving the blended yarn to obtain a nylon / cotton blended fabric;
[0098] S5, adding the modified graphene into a 5wt% aqueous polyurethane solution at a mass volume ratio of 1g / 200mL, stirring and mixing evenly to form a suspension, and then immersing the nylon / cotton blended fabric in the above suspension. After the immersion is completed, the textile is placed in an oven at 60°C for drying to obtain.
[0099] Preparation method of modified graphene:
[0100] S51, adding graphene to a sulfuric acid solution at a mass volume ratio of 1g / 80mL, cooling to below 0°C, adding potassium permanganate, the mass ratio of graphene to potassium permanganate is 1:3, stirring evenly and heating to 70°C, keeping warm for 50min, then adding a 10wt% aqueous hydrogen peroxide solution for oxidation reaction, the volume ratio of sulfuric acid solution to hydrogen peroxide solution is 1:0.8, filtering and separating the graphene, washing with water and drying to obtain graphene oxide;
[0101] S52, adding TiCl4 to ammonia water, the volume ratio of TiCl4 to ammonia water is 1:4, stirring to react, obtaining a white precipitate, adding the white precipitate to oxalic acid with a mass concentration of 10% at a mass volume ratio of 1g / 100mL, stirring to dissolve, and obtaining a titanium oxalate solution; adding graphene oxide, ammonium acetate and citric acid to the titanium oxalate solution, the mass ratio of graphene oxide, ammonium acetate and citric acid is 10:2:1, the mass volume ratio of graphene oxide to the titanium oxalate solution is 1g / 80mL, heating to 80°C, stirring to react for 2h, standing to age for 10h, separating, placing at 180°C for 20min, and then calcining at 600°C for 3h to obtain a titanium dioxide-graphene oxide composite;
[0102] S53, adding sodium carboxymethyl cellulose into water and stirring to dissolve to prepare a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.5%, adding an acid catalyst to the sodium carboxymethyl cellulose solution, the acid catalyst added in an amount of 0.05wt% of the acid in the sodium carboxymethyl cellulose aqueous solution, the catalyst being a mixture of SnCl4 and 10wt% hydrochloric acid, the mass volume ratio of the two being 0.001:1, stirring to mix evenly, and then adding titanium dioxide-graphene oxide composite at a mass volume ratio of 1g / 150mL, heating to 80°C, keeping the temperature for reaction for 120min, filtering, washing and drying in sequence after the reaction is completed.
[0103] Comparative Example 1
[0104] The difference between Comparative Example 1 and Example 1 is that:
[0105] In step S5, the modified graphene is replaced with ordinary graphene;
[0106] The remaining steps are the same as those in Example 1.
[0107] Comparative Example 2
[0108] The difference between Comparative Example 2 and Example 1 is:
[0109] Eliminate the S52 operation steps;
[0110] The remaining steps are the same as those in Example 1.
[0111] Comparative Example 3
[0112] The difference between Comparative Example 3 and Example 1 is that:
[0113] No natural crystal powder is added in step S1;
[0114] The remaining steps are the same as those in Example 1.
[0115] Performance Testing
[0116] 1. Test of UV protection performance of fabrics: The UV protection index UPF of the fabrics of Examples 1-5 and Comparative Examples 1-2 was tested using a Labsphere UV-1000F fabric UV tester. Each piece of fabric was tested 5 times and the average value was taken. The test results are shown in Table 1:
[0117] Table 1
[0118]
[0119] 2. The fabric materials prepared in Examples 1-5 were tested for wrinkle recovery angle using a YG541B fabric wrinkle elasticity tester according to the method specified in GB / T3819-1997, and for tensile breaking strength using a YG065 electronic fabric strength tester. The test results are shown in Table 2:
[0120] Table 2:
[0121]
[0122] 3. The far-infrared emission performance of textile fabrics was tested using the GB / T30127-2013 method. The test results are shown in Table 3:
[0123] Table 3
[0124]
[0125] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing an anti-ultraviolet composite fabric filled with biological natural crystal powder, It is characterized in that The following steps are involved: S1, mixing nylon chips, natural crystal powder and spinning aids uniformly to obtain a mixture; S2, adding the mixed material into a melt spinning machine for spinning, and then cold-cutting the spun filament bundle into shape; S3, applying oil to the formed tow, and then drawing and winding the tow in sequence to obtain nylon fiber; S4, blending the cotton fiber with the nylon fiber to obtain a blended yarn, and weaving the blended yarn to obtain a nylon / cotton blended fabric; S5, adding graphene to the aqueous polyurethane solution, stirring and mixing to form a suspension, and then dipping the nylon / cotton blended fabric in the suspension, and after the dipping is completed, placing the fabric in an oven for drying, to obtain; The natural crystal powder is mixed with the following substances: Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, rose crystal powder, aventurine powder, red jasper powder, serpentine powder; The graphene is modified by the following steps: S51, adding graphene to a sulfuric acid solution, cooling to below 0°C, adding potassium permanganate, stirring evenly and heating, then adding an aqueous hydrogen peroxide solution for oxidation reaction, filtering and separating the graphene, washing with water and drying to obtain graphene oxide; S52, TiCl 4 Add ammonia water, stir to react, obtain a white precipitate, add oxalic acid to the white precipitate, stir to dissolve, and obtain a titanium oxalate solution; add graphene oxide, ammonium acetate and citric acid to the titanium oxalate solution, heat and stir to react, stand for aging, and calcine to obtain a titanium dioxide-graphene oxide composite; S53, adding sodium carboxymethyl cellulose into water, stirring and dissolving, preparing a sodium carboxymethyl cellulose aqueous solution with a mass concentration of 0.5%, adding an acid catalyst into the sodium carboxymethyl cellulose solution, stirring and mixing evenly, then adding titanium dioxide-graphene oxide composite, heating to 80°C, keeping warm for reaction, and after the reaction is completed, filtering, washing and drying in sequence to obtain the product.
2. A method for preparing a UV-proof composite fabric filled with biological natural crystal powder according to claim 1, It is characterized in that In the step S1, the mass ratio of nylon slices, natural crystal powder and spinning aid is 1:0.08:0.
01.
3. A method for preparing a UV-proof composite fabric filled with biological natural crystal powder according to claim 1, It is characterized in that In the step S4, the blending ratio of cotton fiber to nylon fiber is 1:1-5.
4. The method for preparing the UV-proof composite fabric filled with biological natural crystal powder according to claim 1, It is characterized in that In step S5, the concentration of the aqueous polyurethane solution is 5-10 wt %.
5. The method for preparing the UV-proof composite fabric filled with biological natural crystal powder according to claim 1, It is characterized in that In the step S51, the mass ratio of graphene to potassium permanganate is 1:3-8.
6. A method for preparing a UV-proof composite fabric filled with biological natural crystal powder according to claim 1, It is characterized in that In the step S51, the concentration of the aqueous hydrogen peroxide solution is 10-20 wt %.
7. The method for preparing the UV-proof composite fabric filled with biological natural crystal powder according to claim 1, It is characterized in that In step S53, the insulation reaction time is controlled within 120-152 minutes.
8. A UV-proof composite fabric filled with biological natural crystal powder, It is characterized in that The method is prepared by any one of claims 1 to 7.
Citation Information
Patent Citations
Negative ion polyamide fibre and manufacturing method therefor
CN101109114A
Composite electrochemical biosensor, and preparation method and application of same
CN107607601A
Far infrared textile fabric preparation method
CN108221363A
Carboxylated graphene oxide as well as preparation and application methods thereof
CN114162811A