Floating structure gallium oxide ultraviolet detector and its preparation method and application
By designing a floating structure that separates the Ga2O3 thin film from the substrate, interface traps are eliminated, improving the detectivity and responsivity of the gallium oxide ultraviolet detector. This resolves the contradiction between responsivity and detectivity in existing technologies and enables the design of a high-performance detector.
Patent Information
- Application Number
- CN202411069192.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-06
AI Technical Summary
Existing Ga2O3 thin-film solar-blind ultraviolet detectors suffer from a contradiction between responsivity and detectivity, failing to meet the requirements of high-performance ultraviolet detectors.
By employing a floating structure design, the Ga2O3 thin film is separated from the substrate to form a gallium oxide ultraviolet detector with an MSM structure, which eliminates interface traps, reduces PPC phenomenon, and improves detectivity and responsivity.
A gallium oxide ultraviolet detector with high detectivity and high responsivity has been achieved, which solves the contradiction between responsivity and detectivity in the existing technology and provides a design concept for high-performance detectors.
Smart Images

Figure CN118588784B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of gallium oxide ultraviolet detectors, and in particular to a gallium oxide ultraviolet detector with a floating structure and a preparation method and application thereof. Background Art
[0002] Ultraviolet radiation can be divided into three bands according to the wavelength of electromagnetic waves: ultraviolet rays in the 320-400 nm band are called UVA, ultraviolet rays in the 280-320 nm band are called UVB, and ultraviolet rays in the 100-280 nm band are called UVC. Due to the presence of the surface ozone layer, ultraviolet rays below 280 nm in solar radiation are difficult to reach the earth's surface, so people generally call the ultraviolet region of 200-280 nm the solar-blind ultraviolet region. Since there is almost no ultraviolet light in the atmosphere, the background noise of ultraviolet radiation in the solar-blind ultraviolet region is very weak, and the signal of the radiation source can be detected very accurately. Therefore, solar-blind ultraviolet detectors are widely used in flame sensing, short-range ultraviolet communication, biological / chemical analysis and testing, missile early warning systems and other fields.
[0003] In traditional technology, devices such as photomultiplier tubes, thermal detectors, and narrowband semiconductor photodiodes represented by Si are mainly used to detect ultraviolet rays, but these devices have their own advantages and disadvantages: photodiodes have high sensitivity, but their disadvantages are large size, heavy weight, high operating voltage, and high energy consumption; the main disadvantage of thermal detectors is that the response speed is particularly slow; silicon-based ultraviolet detectors usually require expensive filters to block incident light in the visible-infrared region, the effective area utilization rate of the device is low, the quantum efficiency is low, and the device is prone to aging due to long-term exposure to ultraviolet radiation. With the development of the times, the demand and expectations for new ultraviolet detectors in fields such as health, environmental monitoring, and artificial intelligence are getting higher and higher. People not only require ultraviolet detectors to have good reliability, high signal-to-noise ratio, strong light sensitivity, and fast response speed, but also hope that the detectors are small in size, flexible and portable, low in energy consumption, and more flexible and intelligent. These demands further prompted researchers to make new breakthroughs in materials and device structures. In recent years, due to the advancement of thin film manufacturing technology, the emergence of wide bandgap semiconductors has provided a new idea for people studying ultraviolet detection technology. Mg x Zn 1-x O、Al x Ga 1-x Materials such as N, Ga2O3, and diamond not only have high optical band gaps, but also have good stability under ultraviolet irradiation. Therefore, research based on these ultra-wide bandgap semiconductor ultraviolet detectors has also received more and more attention. Among various types of wide bandgap semiconductor materials, Al x Ga 1-xWhen the aluminum content of N film is high, a higher deposition temperature is required, and it is difficult to obtain a film with good crystal quality. x Zn 1-x O is prone to phase transition when the Mg content is high, and diamond films have problems such as large band gap and difficulty in doping. The band gap width of Ga2O3 is about 4.9 eV, and its corresponding absorption edge happens to belong to the solar-blind ultraviolet region. Currently, high-quality single crystal bulk materials / epitaxial films can be obtained through a variety of methods. Coupled with good thermal stability and excellent radiation resistance, it is an ideal material for preparing solar-blind detectors.
[0004] So far, the research on Ga2O3-based day-blind UV detectors covers various forms of Ga2O3 materials, including bulk materials, thin films and nanostructured materials. Generally speaking, Ga2O3 bulk materials have high photoresponsivity, but at the same time the dark current is also large. However, bulk Ga2O3 is not suitable for commercial applications. This is mainly due to the following two reasons: On the one hand, the synthesis process of bulk materials is complex and the cost is high, which is not conducive to industrial development; on the other hand, the use of bulk materials greatly increases the volume of components, which is not conducive to the miniaturization of electronic devices; nanostructured (nanowires, nanobelts, nanoshells) Ga2O3 materials have a large specific surface area, usually showing higher photoresponsivity and lower current, but nanomaterials are not easy to grow. The preparation area is uniform and the repeatability is poor, so it is not suitable for commercial development. Compared with bulk and nanostructures, thin film materials not only have many preparation methods and mature processes, but also solve the scale problem of samples. Therefore, thin film materials are still the mainstream in the research of Ga2O3-based solar-blind detectors. However, the photocurrent and photoresponsivity of solar-blind ultraviolet detectors based on Ga2O3 thin films are generally low, and the continuous conductivity phenomenon is relatively serious, which cannot meet the performance requirements of high responsiveness and high response speed of devices in practical applications. Therefore, there is an urgent need to improve the performance of Ga2O3 thin film solar-blind ultraviolet detectors. Summary of the invention
[0005] The purpose of the present invention is to provide a floating structure gallium oxide ultraviolet detector and its preparation method and application, by separating the photosensitive channel and the substrate part, eliminating the interface trap between the Ga2O3 channel and the substrate, reducing the PPC phenomenon caused by interface defects while achieving high response of the gallium oxide ultraviolet detector, achieving high detection rate of the gallium oxide ultraviolet detector, solving the contradiction between the responsivity and detection rate of the current Ga2O3 thin film gallium oxide ultraviolet photodetector, and providing new ideas for the design and optimization of high-performance gallium oxide ultraviolet detectors.
[0006] To achieve the above objectives, the present technical solution provides a floating structure gallium oxide ultraviolet detector, comprising: a substrate layer 10, a Ga2O3 film 20 and a metal electrode 30, wherein the surface portion of the substrate layer 10 close to the Ga2O3 film 20 is recessed to form a groove 11, the Ga2O3 film 20 is constructed over the groove 11 to cover the groove 11 to form a floating structure, and the metal electrode 30 is formed on the substrate layer 10 through a patterning and deposition process and forms an ohmic contact with the Ga2O3 film 20 through annealing.
[0007] The structure diagram of the floating structure gallium oxide ultraviolet detector provided by this scheme is as follows Figure 1 As shown, the floating structure gallium oxide ultraviolet detector is a metal-semiconductor-metal MSM structure. The MSM type gallium oxide ultraviolet detector has the advantages of simple manufacturing process and high responsiveness. At the same time, due to the existence of defects in the semiconductor material of the MSM type gallium oxide ultraviolet detector, the carriers usually have a long lifetime, and the gallium oxide ultraviolet detector can often show a high internal gain. However, due to the existence of defect capture states, a serious persistent photoconductivity (PPC) phenomenon is caused to a large extent, resulting in a large leakage current and a low detection rate (D*); and the floating structure gallium oxide ultraviolet detector provided in this scheme is designed with a floating structure on the basis of the MSM structure. The substrate of the floating structure and the ultraviolet photosensitive channel formed by the Ga2O3 film are separated, thereby eliminating the interface traps between the ultraviolet photosensitive channel of the Ga2O3 film and the substrate, thereby retaining the high response brought by the MSM structure and reducing the PPC phenomenon caused by interface defects, thereby achieving a high detection rate of the floating structure gallium oxide ultraviolet detector.
[0008] Specifically, the groove 11 formed on the substrate layer 10 is a groove with a length of 60%-80% of the length of the Ga2O3 film 20, a width much larger than the width of the Ga2O3 film, and a depth greater than 50 nm. The advantage of such a design is that the interface defects between the ultraviolet photosensitive channel formed by the suspended Ga2O3 film and the substrate can be completely eliminated, thereby greatly improving the absorption efficiency of ultraviolet light.
[0009] In some embodiments, the Ga2O3 film is completely suspended in the groove 11 to form a floating structure. Correspondingly, the groove 11 is designed as a complete groove so that the Ga2O3 film can be completely suspended on the groove 11. Specifically, the ultraviolet photosensitive channel formed by the Ga2O3 film is completely suspended on the groove 11 so that the Ga2O3 film has almost no contact with the dielectric layer. The advantage of such a design is that interface defects can be completely eliminated.
[0010] In some embodiments, the metal electrode is selected to be a laminated metal. The use of the laminated metal can optimize the physical and electrical properties of the electrode, such as improving the contact quality with the semiconductor material, increasing conductivity, enhancing mechanical stability, and preventing metal diffusion.
[0011] In the embodiment of the present scheme, the metal electrode is selected as a stacked metal of Ti, Al, Ni, and Au, wherein Ti / Al can be used as an ohmic contact layer of the metal electrode, and Ni / Au can be used as an adhesion layer and a barrier layer of the metal electrode.
[0012] In other embodiments of the present scheme, the metal electrode is selected to be Ti and Au stacked metal.
[0013] The floating structure gallium oxide ultraviolet detector provided in this solution adopts an MSM structure and uses a Ga2O3 film between two metal electrodes to detect light signals. When photons are absorbed by the semiconductor material and generate electron-hole pairs, these carriers are collected under the action of the electric field formed between the metal electrodes, thereby generating a measurable current change.
[0014] In some embodiments, the substrate material of the substrate layer needs to match the Ga2O3 film, and the substrate material of the substrate layer is selected from sapphire, single crystal silicon, silicon dioxide, gallium nitride, silicon carbide, quartz, gallium oxide, or a combination of any two or more thereof. Preferably, the substrate material is selected from single crystal silicon covered with a silicon dioxide layer.
[0015] As described above, the floating structure gallium oxide ultraviolet detector provided by the present invention is based on the MSM structure, and designs a floating structure in which the ultraviolet photosensitive channel and the substrate are separated to eliminate the interface traps between the ultraviolet photosensitive channel formed by the Ga2O3 thin film and the substrate, thereby achieving a high detection rate while realizing a high response of the floating structure gallium oxide ultraviolet detector.
[0016] In a second aspect, the present solution provides a method for preparing the floating structure gallium oxide ultraviolet detector mentioned in the first aspect, and the preparation method has the advantage of a simple preparation process, comprising the following steps:
[0017] S1: cleaning and drying the substrate layer 10;
[0018] S2: Photolithography and etching to form a groove 11 on the surface of the substrate layer;
[0019] S3: transferring the peeled Ga2O3 film 20 to above the groove 11 to form a floating structure;
[0020] S4: depositing a laminated metal after photolithography of an electrode pattern on the substrate layer, and peeling off to form a metal electrode 30;
[0021] S3: Annealing allows the metal electrode 30 to form an ohmic contact with the Ga2O3 film.
[0022] The preparation method of the floating structure gallium oxide ultraviolet detector provided in this scheme etches a groove on the substrate layer, and transfers the mechanically peeled Ga2O3 film to the top of the groove to form a floating structure, so as to make up for the interface defect problem caused by the MSM structure, and then prepare a floating structure gallium oxide ultraviolet detector with high responsiveness and high detection rate.
[0023] In step S1, the substrate material needs to match the Ga2O3 film, and the substrate material of the substrate layer is selected to be one or a combination of any two or more of sapphire, single crystal silicon, silicon dioxide, gallium nitride, silicon carbide, quartz, and gallium oxide.
[0024] Preferably, in step S1, the substrate layer 10 is ultrasonically cleaned with acetone, isopropanol and deionized water respectively and then dried with a nitrogen gun. This has the advantage of ensuring that the surface of the substrate layer 10 is clean and free of impurities, providing a clean interface for subsequent processing. In some embodiments, the ultrasonic cleaning is performed for 4-6 minutes, preferably, for 5 minutes.
[0025] In other embodiments, in order to effectively remove dangling bonds, surface states and stubborn contamination on the surface of the substrate layer, the substrate layer 10 is cleaned organically with acetone and isopropanol, then cleaned with piranha solution for a set period of time, and then ultrasonically cleaned with deionized water. After cleaning, it is dried with a nitrogen gun, wherein the piranha solution is a solution prepared with a volume ratio of concentrated sulfuric acid and hydrogen peroxide solution of 3:1.
[0026] In step S2 , after a groove pattern is photolithographically formed on the surface of the substrate layer 10 , a groove 11 is formed by etching based on the groove pattern.
[0027] In some embodiments, a photoresist is coated on the substrate layer 10 , wherein the photoresist can change its properties under light irradiation so as to form a pattern in a subsequent development process. In this solution, a groove pattern is formed after the photoresist is coated on the substrate layer 10 .
[0028] In some embodiments, one or more of inductively coupled plasma etching (ICP) and reactive ion etching (RIE) are used for etching. ICP etching is to generate plasma in an etching chamber by a high-frequency power supply, and the active particles in the plasma react with the substrate material to convert it into volatile compounds, thereby achieving etching; RIE is another dry etching technology, which achieves material etching by bombarding the material surface with ions in the plasma combined with chemical reactions.
[0029] In some embodiments, inductively coupled plasma etching is used for etching, wherein the etching gas is selected as one or more of CF4 and SF6. In an embodiment of this scheme, the CF4 flow rate is 5 sccm, the SF6 flow rate is 15 sccm, the etching pressure is 15 mTorr, the RF power is 10 W, the ICP power is 80 W, and the etching time is 30 s.
[0030] Specifically, the groove 11 formed on the substrate layer 10 is a groove with a length of 60%-70% of the length of the Ga2O3 film 20, a width much larger than the width of the Ga2O3 film, and a depth greater than 50 nm.
[0031] In step S3, the mechanically peeled Ga2O3 film is transferred to the prefabricated groove 11 by a 2D transfer platform to form a floating structure.
[0032] It is particularly emphasized that the Ga2O3 film transferred by this scheme is completely suspended in the groove and covers the groove. This structure can minimize the interaction with the substrate and improve the performance of the device.
[0033] In step S4, the position of the metal electrode is defined on the Ga2O3 film and the substrate layer by photolithography technology, and then metal is deposited to form the metal electrode.
[0034] In the embodiment of the present scheme, the laminated metal is deposited by any deposition process of electron beam evaporation, thermal evaporation and magnetron sputtering. Electron beam evaporation is to heat the metal material by focusing the electron beam to evaporate it. The electron beam can be precisely controlled to provide a very high energy density, so the metal can be evaporated quickly without damaging the substrate; thermal evaporation (or resistance heating evaporation) is to evaporate the metal by resistance heating. The metal is placed in a heating boat and heated to the evaporation point by an electric current; magnetron sputtering is a physical vapor deposition (PVD) technology that sputters the metal target through the combined action of a magnetic field and an electric field, and the generated metal atoms or ions are deposited on the substrate.
[0035] In some embodiments, the metal electrode is selected to be a laminated metal. The use of the laminated metal can optimize the physical and electrical properties of the electrode, such as improving the contact quality with the semiconductor material, increasing conductivity, enhancing mechanical stability, and preventing metal diffusion.
[0036] In the embodiment of this scheme, the metal electrode is selected as a stacked metal of Ti, Al, Ni, and Au, wherein Ti / Al can be used as an ohmic contact layer of the metal electrode, and Ni / Au can be used as an adhesion layer and a barrier layer of the metal electrode. At this time, the thickness of the metal layer of the Ti, Al, Ni, and Au stacked metal is 20 / 100 / 60 / 80 nm, respectively.
[0037] In other embodiments of the present solution, the metal electrode is selected as Ti or Au.
[0038] In step S5, the metal electrode 30 is annealed using a rapid thermal annealing device or a tubular annealing furnace device to form an ohmic contact with the Ga2O3 film.
[0039] In some embodiments, when the metal electrode 30 is annealed using a rapid thermal annealing device, the annealing is performed in a nitrogen atmosphere at an annealing temperature of 470° C. for 1 min, so that a good ohmic contact can be formed between the UV-sensitive channel and the metal electrode.
[0040] On the third aspect, this scheme provides an application of a floating structure gallium oxide ultraviolet detector. The floating structure gallium oxide ultraviolet detector prepared in the first aspect is used to detect ultraviolet light, which can be used for flame sensing, short-range ultraviolet communication, biological / chemical analysis and testing, missile early warning systems, etc.
[0041] Compared with the prior art, the technical solution has the following characteristics and beneficial effects: The solution provides a method for preparing a floating structure gallium oxide ultraviolet detector. The preparation method is simple in process. The prepared floating structure gallium oxide ultraviolet detector completely separates the ultraviolet photosensitive channel from the substrate interface based on the MSM structure, aiming to improve the continuous photoconductivity phenomenon of the detector caused by interface defects while retaining the high response of the MSM type gallium oxide ultraviolet detector, and at the same time achieve high detection rate and high responsivity of the gallium oxide ultraviolet detector. Specifically, the floating structure in the floating structure gallium oxide ultraviolet detector separates the ultraviolet photosensitive channel from the substrate part, eliminates the interface traps between the Ga2O3 channel and the substrate, reduces the PPC phenomenon caused by interface defects while achieving high response of the photodetector, achieves high detection rate of the gallium oxide ultraviolet detector, solves the contradiction between responsivity and detection rate that is common in the current gallium oxide ultraviolet photodetector, and provides a new idea for the design and optimization of high-performance Ga2O3 day-blind photodetectors. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0043] Figure 1 This is a schematic diagram of the structure of the floating structure gallium oxide ultraviolet detector provided in this scheme.
[0044] Figure 2 The floating structure gallium oxide UV detector provided by this scheme is the same as the conventional MSM type gallium oxide UV detector at 250 nm 0.01 μW / cm 2 IV curve under UV light.
[0045] Figure 3 It curves of the floating structure gallium oxide ultraviolet detector provided by this scheme and the conventional MSM type gallium oxide ultraviolet detector under 250 nm ultraviolet light.
[0046] Figure 4 It is the rising and attenuation edges of the It curve of the floating structure gallium oxide ultraviolet detector provided by this scheme and the conventional MSM type gallium oxide ultraviolet detector under 250 nm ultraviolet light. DETAILED DESCRIPTION
[0047] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The implementations described in the following exemplary embodiments do not represent all implementations consistent with one or more embodiments of this specification. Instead, they are merely examples of devices and methods consistent with some aspects of one or more embodiments of this specification as detailed in the appended claims.
[0048] It should be noted that: in other embodiments, the steps of the corresponding method are not necessarily performed in the order shown and described in this specification. In some other embodiments, the steps included in the method may be more or less than those described in this specification. In addition, a single step described in this specification may be decomposed into multiple steps for description in other embodiments; and multiple steps described in this specification may be combined into a single step for description in other embodiments.
[0049] Embodiment 1
[0050] The Si substrate covered with SiO2 with a thickness of 120 nm was cleaned with propanol, isopropanol and deionized water for 5 minutes, and then dried with a nitrogen gun to obtain a substrate layer. The ICP method was used to etch a groove with a length of 110 um, a depth of 80 nm and a width much larger than the width of the gallium oxide film on the substrate layer. The ICP method used CF4 and SF6 gases, and the CF4 flow rate was 5 sccm, the SF6 flow rate was 15 sccm, the etching pressure was 15 mTorr, the RF power was 10 W, the ICP power was 80 W, and the etching time was 30 s. The Ga2O3 film with a thickness of 200 nm, a length of 150 um and a width of 30 um was mechanically peeled off using a 2D transfer platform and transferred to the top of the groove. The electrode pattern was formed on the substrate layer by photolithography, and Ti, Al, Ni, and Au stacked metals were deposited in sequence by electron beam evaporation, and the thickness of each layer of the Ti, Al, Ni, and Au stacked metals was 20 / 100 / 60 / 80 nm, a metal electrode is formed after peeling, and the RTP method is used to make the metal electrode form an ohmic contact with the Ga2O3 film, wherein the annealing conditions are: in a nitrogen atmosphere, the annealing temperature is 470 ℃, and annealing is carried out for 1 min.
[0051] Comparative Example 1 Gallium Oxide UV Detector with Conventional MSM Structure
[0052] The Si substrate covered with 120 nm thick SiO2 was cleaned with propanol, isopropanol and deionized water for 5 minutes, and then dried with a nitrogen gun to obtain the substrate layer. The Ga2O3 film with a thickness of 200 nm, a length of 150 um and a width of 30 um was mechanically peeled off using a 2D transfer platform and transferred to the top of the groove; the electrode pattern was photolithographically formed on the substrate layer and Ti, Al, Ni, and Au stacked metals were deposited in sequence by electron beam evaporation, and the thickness of each layer of the Ti, Al, Ni, and Au stacked metals was 20 / 100 / 60 / 80 nm. After peeling, a metal electrode was formed, and the RTP method was used to make the metal electrode form an ohmic contact with the Ga2O3 film. The annealing conditions were: in a nitrogen atmosphere, the annealing temperature was 470 ℃, and annealing was performed for 1 min.
[0053] The only difference between the comparative example and the first embodiment is that no grooves are formed on the surface of the substrate layer of the conventional MSM structure gallium oxide ultraviolet detector provided in the first comparative example, and the Ga2O3 film does not form a floating structure with the grooves.
[0054] Test performance:
[0055] Test Example 1:
[0056] The detectors obtained in Example 1 and Comparative Example 1 were placed in a dark room without illumination to test the dark current. The UV light source was adjusted to a wavelength of 250 nm and the light intensity was controlled at 0.01 μW / cm². The light source was aimed at the detector to start measuring the IV curve. Starting from zero bias, the forward and reverse bias voltages were gradually increased, and the current value at each bias point was recorded. The above process was repeated until the preset maximum bias range was reached to obtain the test data and draw the IV curve as shown in FIG. Figure 2 As shown, it is necessary to ensure that the light source is stable and without fluctuations during the entire process. Figure 2 The left picture shows a conventional MSM structure gallium oxide UV detector. Figure 2 The right picture in the figure shows a floating structure gallium oxide ultraviolet detector. It can be seen that the floating structure gallium oxide ultraviolet detector provided in Example 1 has a higher detection degree for ultraviolet light.
[0057] Test Example 2:
[0058] The detectors obtained in Example 1 and Comparative Example 1 were placed in a dark room without illumination to test the initial dark current and transient current signals. The ultraviolet light source was adjusted to a wavelength of 250 nm, the ultraviolet light source was turned on and the transient photocurrent changes of different detectors were immediately recorded. The time for the photocurrent to rise to the maximum value (response time) was observed and recorded. The ultraviolet light source was turned off and the time for the photocurrent to drop to the initial dark current level (recovery time) was recorded to obtain the test data and draw the It curve as shown in FIG. Figure 3 shown. Figure 3 The left picture shows a conventional MSM structure gallium oxide UV detector. Figure 3 The right picture in the figure shows a floating structure gallium oxide ultraviolet detector. It can be seen that the floating structure gallium oxide ultraviolet detector provided in Example 1 has a better response to ultraviolet light.
[0059] Test Example 3:
[0060] The detectors obtained in Example 1 and Comparative Example 1 were placed in a dark room without illumination to test the initial dark current and transient current signal. The ultraviolet light source was quickly turned on to generate a short 250nm pulse light. The transient photocurrent signal of the detector was recorded using an oscilloscope. The time points when the photocurrent increased from 10% to 90% and decreased from 90% to 10%, i.e., the rising edge and the attenuation edge, were identified and marked. The light source was turned off, and the detector was waited for to cool to the initial state to obtain the test data and draw the schematic diagram of the rising and attenuation edges of the It curve as shown in the figure. Figure 4 As shown, Figure 4 The left picture shows a conventional MSM structure gallium oxide UV detector. Figure 4 The right picture in the figure shows a floating structure gallium oxide ultraviolet detector.
[0061] Those skilled in the art should understand that the technical features of the above embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0062] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A floating structure gallium oxide ultraviolet detector, characterized in that: include: A substrate layer (10), a Ga2O3 film (20), and a metal electrode (30), wherein a surface portion of the substrate layer (10) close to the Ga2O3 film (20) is recessed to form a groove (11), the Ga2O3 film (20) is placed on the groove (11) to cover the groove (11) to form a floating structure, the metal electrode (30) is formed on the substrate layer (10) through a deposition and patterning process and forms an ohmic contact with the Ga2O3 film (20) through an annealing treatment, and the groove (11) formed on the substrate layer (10) is a groove with a length of 60% to 80% of the length of the Ga2O3 film (20), a width much larger than the width of the Ga2O3 film (20), and a depth greater than 50 nm, so that the interface defects between the ultraviolet light-sensitive channel formed by the suspended Ga2O3 film and the substrate can be completely eliminated.
2. The floating structure gallium oxide ultraviolet detector according to claim 1, characterized in that: The metal electrode is selected as a laminated metal.
3. A method for preparing a floating structure gallium oxide ultraviolet detector, characterized in that: The following steps are involved: S1: cleaning and drying the substrate layer (10); S2: photolithography and etching to form a groove (11) on the surface of the substrate layer; S3: The peeled Ga2O3 film (20) is transferred to the top of the groove (11) to form a floating structure, wherein the groove (11) formed on the substrate layer (10) is a groove having a length of 60%-80% of the length of the Ga2O3 film (20), a width much larger than the width of the Ga2O3 film (20), and a depth greater than 50 nm, so that the interface defects between the ultraviolet sensitive channel formed by the suspended Ga2O3 film and the substrate can be completely eliminated; S4: depositing a stacked metal after photolithography of an electrode pattern on the substrate layer, and then peeling off to form a metal electrode (30); S5: Annealing allows the metal electrode (30) to form an ohmic contact with the Ga2O3 film.
4. The method for preparing the floating structure gallium oxide ultraviolet detector according to claim 3, characterized in that: In step S1, the substrate layer (10) is ultrasonically cleaned with acetone, isopropanol and deionized water respectively and then blown dry with a nitrogen gun.
5. The method for preparing the floating structure gallium oxide ultraviolet detector according to claim 3, characterized in that: The etching is performed by using one or more of inductively coupled plasma etching and reactive ion etching, wherein the etching is performed by using inductively coupled plasma etching, wherein the etching gas is selected to be one or more of CF4 and SF6.
6. The method for preparing the floating structure gallium oxide ultraviolet detector according to claim 3, characterized in that: The stacked metal is deposited by any deposition process including electron beam evaporation, thermal evaporation and magnetron sputtering.
7. The method for preparing the floating structure gallium oxide ultraviolet detector according to claim 3, characterized in that: In step S5, a rapid thermal annealing device or a tubular annealing furnace device is used to anneal the metal electrode (30) to form an ohmic contact with the Ga2O3 film.
8. An application method of a floating structure gallium oxide ultraviolet detector, characterized in that: The floating structure gallium oxide ultraviolet detector according to any one of claims 1 to 2 is used for ultraviolet detection.