A solid-state lithium-sulfur battery composite positive electrode material and preparation method thereof, solid-state lithium-sulfur battery

By using a three-dimensional hydrogel formed by high-entropy metal selenide and reduced graphene oxide in solid-state lithium-sulfur batteries, the problems of poor conductivity and interface stability are solved, significantly improving the rate performance and cycle performance of the battery, and achieving better performance. High mass specific capacity and electrochemical stability.

CN118588917BActive Publication Date: 2024-10-22SONGSHAN LAKE MATERIALS LAB +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411074111.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The composite cathode material of solid-state lithium-sulfur batteries has poor electronic/ion conductivity, poor interface stability, and volume changes during charge and discharge, resulting in poor rate performance, low mass specific capacity, and poor cycle performance, which limits its commercial application.

Method used

A composite cathode material using MSex-rGO hydrogel/S, polyethylene oxide and lithium salt is used to form a three-dimensional conductive network through high-entropy metal selenide and reduced graphene oxide (rGO) to improve electron/ion transport capabilities and interface compatibility. , the preparation method includes mixing a selenium source, a reducing agent and a solvent, heat treatment and vacuum melting to form a high-entropy metal selenide hydrogel with a cubic or hexagonal crystal structure.

Benefits of technology

It improves the utilization rate and electronic conductivity of active sulfur, suppresses volume expansion, maintains the stability and cycle performance of the electrode structure, and significantly improves the electrochemical performance and service life of solid-state lithium-sulfur batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118588917B_ABST
    Figure CN118588917B_ABST
Patent Text Reader

Abstract

The present invention provides a solid-state lithium-sulfur battery composite positive electrode material and a preparation method thereof, and a solid-state lithium-sulfur battery, which belongs to the field of battery technology and overcomes the defects of the solid-state lithium-sulfur battery in the prior art, such as poor rate performance, low mass specific capacity, and poor cycle performance. The solid-state lithium-sulfur battery composite positive electrode material of the present invention includes MSe x ‑rGO hydrogel / S, polyethylene oxide and lithium salt; x is 1.8-2.2; M includes more than 4 metal atoms among cobalt, molybdenum, nickel, iron, chromium, manganese, tungsten and vanadium; MSe x In ‑rGO hydrogel / S, the mass content of S is 50%~80%; MSe x The mass ratio of ‑rGO hydrogel / S: polyethylene oxide: lithium salt is (4-6): (3-5): (0.5-1). The electrical performance of the solid-state lithium-sulfur battery prepared by using the composite positive electrode material of the present invention is significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries, and in particular relates to a solid-state lithium-sulfur battery composite positive electrode material and a preparation method thereof, and a solid-state lithium-sulfur battery. Background Art

[0002] Lithium-sulfur batteries are considered to be a promising next-generation high-performance battery technology due to their high theoretical mass specific capacity (1675 mAh / g) and high theoretical energy density (2600 Wh / kg). Currently, the most widely used lithium-sulfur battery electrolyte is an organic ether electrolyte, but lithium-sulfur batteries using organic ether electrolytes have problems such as the shuttle effect of polysulfides, flammability of ether electrolytes, and easy thermal runaway.

[0003] Using solid-state electrolytes (SSEs) instead of traditional organic ether electrolytes is a very effective way to solve the polysulfide shuttle effect and battery thermal runaway.

[0004] However, there are still three major problems with the composite cathode materials of solid-state lithium-sulfur batteries: (1) The electronic / ionic conductivity of elemental sulfur, discharge product Li2S and solid electrolyte in the composite cathode materials is poor, resulting in slow electron / ion transmission; (2) The stability of the sulfur (solid) / sulfur host (solid) / solid electrolyte (solid) three-phase interface is poor, with fewer electrochemical active sites and larger charge transfer impedance; (3) During the charge and discharge process, the conversion between elemental sulfur and discharge product Li2S will cause the volume of the cathode to change, causing the battery capacity to decay and even destroying the battery structure. These problems lead to poor rate performance, low mass specific capacity and poor cycle performance of solid-state lithium-sulfur batteries, limiting their commercial application. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the prior art solid-state lithium-sulfur batteries, such as poor rate performance, low mass specific capacity, and poor cycle performance, thereby providing a solid-state lithium-sulfur battery composite positive electrode material and a preparation method thereof, and a solid-state lithium-sulfur battery.

[0006] To this end, the present invention provides the following technical solutions.

[0007] In a first aspect, the present invention provides a solid-state lithium-sulfur battery composite positive electrode material, comprising MSe x -rGO hydrogel / S, polyethylene oxide, and lithium salt;

[0008] x is 1.8 to 2.2; M includes four or more metal atoms selected from the group consisting of cobalt, molybdenum, nickel, iron, chromium, manganese, tungsten and vanadium;

[0009] MS x -rGO hydrogel / S, the mass content of S is 50%~80%;

[0010] MS x -rGO hydrogel / S:polyethylene oxide:lithium salt mass ratio is (4~6):(3~5):(0.5~1).

[0011] rGO is reduced graphene oxide.

[0012] Furthermore, the molar ratio of any two metal atoms in M ​​is (0.8~1.2):(0.8~1.2).

[0013] Furthermore, MS x -rGO hydrogel has a specific surface area of ​​300~1000 m 2 / g, for example, the specific surface area can be 300 m 2 / g, 400 m 2 / g, 500 m 2 / g, 600 m 2 / g, 700 m 2 / g, 800 m 2 / g, 900 m 2 / g, 1000 m 2 / g.

[0014] Furthermore, MS x -rGO hydrogel, MSe x The mass ratio of rGO is (20~150):(60~80), which can be (20~40):(60~80);

[0015] Furthermore, the lithium salt is selected from lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), LiNO3, LiI and Li a S b At least one of, wherein 3≤a≤5, 1≤b≤2.

[0016] In a possible embodiment, M includes nickel, cobalt, and manganese; M also includes at least one of molybdenum, iron, chromium, tungsten, and vanadium. x It has a cubic crystal structure.

[0017] In a possible embodiment, M includes tungsten, cobalt, and molybdenum; M also includes at least one of iron, chromium, and vanadium. x It has a hexagonal crystal structure.

[0018] In a second aspect, the present invention provides a method for preparing a solid-state lithium-sulfur battery composite positive electrode material, comprising the following steps:

[0019] S1. Preparation of MSe x-rGO hydrogel; x is 1.8-2.2; M includes 4 or more metal atoms selected from cobalt, molybdenum, nickel, iron, chromium, manganese, tungsten and vanadium;

[0020] S2, MSe x -rGO hydrogel was mixed with sulfur to obtain a mixture, and then vacuum-melted to obtain MSe x -rGO hydrogel / S; in the mixture, the mass content of S is 50%~80%;

[0021] S3. Add MSe x -rGO hydrogel / S, polyethylene oxide, lithium salt and a first solvent are mixed under a protective atmosphere to obtain a first mixed solution, and the first mixed solution is heated and stirred to obtain a composite positive electrode material;

[0022] MS x -rGO hydrogel / S:polyethylene oxide:lithium salt mass ratio is (4~6):(3~5):(0.5~1).

[0023] Furthermore, the first solvent includes at least one of acetonitrile, acetone or N,N-dimethylformamide.

[0024] Furthermore, the protective atmosphere is argon or nitrogen.

[0025] Further, the S1 includes:

[0026] Mixing a selenium source, a reducing agent and a second solvent to prepare a precursor liquid;

[0027] Mixing rGO with water to prepare an rGO suspension, and mixing a salt containing M with the rGO suspension to prepare a second mixed solution;

[0028] The precursor liquid is mixed with the second mixed liquid to obtain a third mixed liquid, and the third mixed liquid is heated to obtain MSe x -rGO hydrogel.

[0029] Furthermore, S1 satisfies at least one of the following conditions:

[0030] (1) The reducing agent includes at least one of sodium borohydride, hydrazine hydrate and oxalic acid;

[0031] (2) The molar ratio of the reducing agent to the selenium source is (1-3): (1-50);

[0032] (3) The selenium source includes at least one of selenium powder and selenium dioxide;

[0033] (4) heating the third mixed solution by microwave solvothermal method; optionally, the microwave power is 1000-2500 W;

[0034] (5) the second solvent comprises at least one of DMF and NMP;

[0035] (6) In the step of heating the third mixed liquid, the heating temperature is 160-260° C., the heating time is 0.5-3 h, and the pressure is 3 MPa-6 MPa.

[0036] Furthermore, in S1, the mass ratio of the selenium source to rGO is (20-400):200; optionally, (300-400):200.

[0037] Optionally, the solid content of the rGO suspension is 0.5-20 wt%, and illustratively, it can be 0.5 wt%, 1 wt%, 5 wt%, 10 wt%, 15 wt%, or 20 wt%.

[0038] In a possible implementation, the salt containing M includes at least four of cobalt salts, molybdenum salts, nickel salts, iron salts, chromium salts, tungsten salts, manganese salts, and vanadium salts.

[0039] Optionally, the cobalt salt is selected from at least one of C4H6CoO4·4H2O, Co(NO3)2·6H2O and CoSO4·7H2O.

[0040] Optionally, the molybdenum salt is selected from NaMoO4·2H2O and H 24 Mo7N6O 24 At least one of 4H2O.

[0041] Optionally, the nickel salt is selected from at least one of C4H6NiO4·4H2O, NiSO4·6H2O and NiN2O6·6H2O.

[0042] Optionally, the iron salt is selected from C4H6FeO4·4H2O, FeN3O9·9H2O and Fe2S3O 12 At least one of nH2O, wherein n is an integer of 2 to 10.

[0043] Optionally, the chromium salt is selected from at least one of C4H6CrO4·4H2O, CrN3O9·9H2O and Cr2(SO4)3·mH2O, where m is an integer of 2 to 10.

[0044] Optionally, the manganese salt is selected from at least one of MnC4H6O4·4H2O, Mn(NO3)2·pH2O and MnSO4·H2O, and p is an integer of 2 to 10.

[0045] Optionally, the tungsten salt is selected from Na2WO4·2H2O and (NH4) 10 At least one of H2(W2O7)6.

[0046] Optionally, the vanadium salt is selected from at least one of NH4VO3 and NaVO3.

[0047] Furthermore, in S2, the vacuum melting temperature is 150-160°C and the time is 10-15 h.

[0048] Furthermore, in the step of heating and stirring the first mixed solution in S3, the heating temperature is 50-100° C. and the heating time is 5-10 h.

[0049] In a third aspect, the present invention provides a solid-state lithium-sulfur battery, comprising a positive electrode plate, wherein the positive electrode plate comprises the above-mentioned solid-state lithium-sulfur battery composite positive electrode material or the solid-state lithium-sulfur battery composite positive electrode material prepared according to the above-mentioned solid-state lithium-sulfur battery composite positive electrode material preparation method.

[0050] Furthermore, in the positive electrode sheet, the sulfur loading is 0.8-20 mg / cm 2 .

[0051] The solid-state lithium-sulfur battery market of the present invention is mainly used in drones, electric vehicles, electric aircraft, electric ships / yachts, aerospace and static energy storage; it can also be used in flexible electronic devices and wearable electronic devices.

[0052] The technical solution of the present invention has the following advantages:

[0053] 1. The solid-state lithium-sulfur battery composite positive electrode material of the present invention includes MSe x -rGO hydrogel / S, polyethylene oxide and lithium salt; x is 1.8-2.2; M includes more than 4 metal atoms among cobalt, molybdenum, nickel, iron, chromium, manganese, tungsten and vanadium; MSe x -rGO hydrogel / S, the mass content of S is 50%~80%; MSe x -rGO hydrogel / S:polyethylene oxide:lithium salt mass ratio is (4~6):(3~5):(0.5~1).

[0054] In the present invention, M includes more than 4 high entropy metal elements. Compared with monovalent, divalent, and ternary metal selenides, the present invention has more metal components that can act as active sites. These different types of metal atoms can chemically bond with active sulfur (sulfur or Li2S) during the redox process, and the multiple atoms can synergistically regulate the chemical bonding strength to active sulfur, thereby avoiding the agglomeration of active sulfur on its surface and improving the effective utilization rate of active sulfur. These metal elements can interact with each other to regulate their electronic structure and increase their electronic conduction ability; at the same time, the different radii between the metal elements will produce certain lattice distortions and a small amount of vacancy defects. The presence of these vacancy defects is more conducive to the electrons and Li + Therefore, MSex -rGO hydrogel as a sulfur host material can effectively improve the electron / ion transport of active sulfur during the redox process.

[0055] During the charge and discharge process, the limited number of active sites of low-medium entropy metal selenides will cause active sulfur to agglomerate on its surface, hindering the further conversion of internal active substances, thereby reducing the utilization rate of sulfur. In addition, the agglomerated active sulfur expands in volume during the conversion process until cracks appear in the electrode material, separating the active sulfur, the sulfur host and the solid electrolyte, thereby collapsing the electrode structure, and ultimately leading to the rapid decay of the capacity of the solid-state lithium-sulfur battery. The present invention uses high-entropy metal selenides, because different types of atoms in the same lattice can serve as active sites, accelerating the rapid conversion between sulfur and Li2S, thereby avoiding a large amount of sulfur or Li2S agglomeration on the surface of the metal selenide, and effectively alleviating the volume expansion caused by the conversion between sulfur and Li2S.

[0056] MS x -rGO hydrogel is a conductive network with a three-dimensional structure. This structure can not only serve as an electron / ion transmission channel, but also has excellent flexibility and mechanical properties. During the charge and discharge process, it can suppress the volume expansion problem to the greatest extent, thereby maintaining a good conductive skeleton and the electrode structure of the active material, improving the mass specific capacity stability and the service life of the battery, and greatly improving the electrochemical performance of the solid-state lithium-sulfur battery. At the same time, this three-dimensional structure can also wrap the active sulfur well, and the three-dimensional structure can also disperse the active sites of high-entropy metal selenide on the rGO surface to the maximum extent, so that it can play the greatest sulfur fixation effect from the physical and chemical aspects.

[0057] In the composite cathode material of the present invention, polyethylene oxide (PEO) as a binder and solid electrolyte has excellent deformation ability. x -rGO hydrogel and S have good interface compatibility, and a stable three-phase solid interface can be formed between the three, thereby improving the cycle stability of solid-state lithium-sulfur batteries.

[0058] 2. In the preparation method of the solid-state lithium-sulfur battery composite positive electrode material of the present invention, S1 comprises: mixing a selenium source, a reducing agent and a second solvent to obtain a precursor liquid; mixing rGO with water to obtain an rGO suspension liquid, mixing a salt containing M with the rGO suspension liquid to obtain a second mixed liquid; mixing the precursor liquid with the second mixed liquid to obtain a third mixed liquid, and heating the third mixed liquid to obtain MSe x -rGO hydrogel.

[0059] rGO has a high specific surface area and rich OH - and O 2- Functional groups, which are negatively charged and can attract positively charged metal cations (Mo4+ ,Co 2+ , W 4+ , Fe 3+ ,Cr 2+ , V 4+ , Ni 2+ , Mn 2+ ). When the pressure and temperature reach certain conditions, the high entropy metal selenide MSe with hexagonal or cubic crystal structure x In situ growth on the surface of rGO, and during the growth, rGO is also cross-linked to form a three-dimensional network structure. Therefore, the present invention can prepare MSe x -rGO three-dimensional structured hydrogel.

[0060] 3. The third mixed solution is heated by microwave solvothermal method. Microwave heating has a fast heating speed and is more likely to generate pure phase high entropy metal selenide and avoid the generation of impurity phase. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0062] Figure 1 The MSe prepared in Example 1 x -SEM image of rGO hydrogel;

[0063] Figure 2 The MSe prepared in Example 1 x -XRD pattern of rGO hydrogel;

[0064] Figure 3 This is a SEM image of the composite positive electrode material prepared in Example 1;

[0065] Figure 4 The MSe prepared in Example 2 x -XRD pattern of rGO hydrogel;

[0066] Figure 5 This is a cycle curve diagram of 100 cycles of a solid-state lithium-sulfur battery made from the composite positive electrode material of Example 1. DETAILED DESCRIPTION

[0067] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0068] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0069] The PEO used in the embodiments and comparative examples is Aladdin reagent with a specification of Mw~500000.

[0070] Example 1

[0071] This embodiment provides a method for preparing a solid-state lithium-sulfur battery composite positive electrode material, comprising the following steps:

[0072] 1. Preparation of MSe x -rGO hydrogel:

[0073] 330 mg of selenium powder, 180 mg of reducing agent sodium borohydride and 20 ml of solvent DMF were mixed in a beaker to obtain a precursor solution.

[0074] 200 mg of rGO was mixed with 20 ml of deionized water to obtain rGO suspension.

[0075] C4H6CoO4·4H2O, C4H6NiO4·4H2O, C4H6CrO4·4H2O, MnC4H6O4·4H2O, and NH4VO3 with a total molar amount of 2 mmol of metal atoms were added to the rGO suspension at a metal atom molar ratio of 1:1:1:1:1, and magnetic stirring was performed for 20 minutes, and then the precursor liquid was uniformly mixed. After the mixed solution was stirred for 5 minutes, it was transferred into a microwave autoclave for heating treatment, and stirring was performed while heating. The microwave heating power was 2000w, the stirring rate was 50r / min, the reaction time of the heating treatment was 1h, the reaction temperature was 180℃, and the pressure was 5 MPa.

[0076] The product after the reaction was separated into solid and liquid, and the obtained precipitate was washed alternately with alcohol and deionized water until the solution was neutral, and then the precipitate was freeze-dried to obtain MSe x -rGO hydrogel, in which MSe x It is a cubic crystal. x The specific surface area of ​​rGO hydrogel is 850 m 2 / g.

[0077] 2. Preparation of MSe x -rGO hydrogel / S:

[0078] MSe x -rGO hydrogel and sublimated sulfur were mixed and ground to obtain a mixture with a sulfur content of 70% by mass. The mixture was placed in a sealed tube, the air in the tube was evacuated, the temperature was controlled at 160°C, and the insulation time was controlled at 12 h to allow the sublimated sulfur to evenly melt into the MSe x -rGO hydrogel to obtain MSe x -rGO hydrogel / S.

[0079] 3. 100 mg of MSe x -rGO hydrogel / S, 80 mg of PEO, 20 mg of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) (i.e., MSe x -rGO hydrogel / S:PEO:lithium salt (mass ratio of 5:4:1) was stirred in 30 ml of acetonitrile solvent and heated at 80 °C for 8 h under nitrogen atmosphere to obtain a composite cathode material.

[0080] Figure 1 The MSe prepared in Example 1 x -rGO hydrogel SEM image. Figure 1 It can be seen that MSe x -rGO hydrogel has a three-dimensional network structure.

[0081] Figure 2 The MSe prepared in Example 1 x XRD pattern of -rGO hydrogel. Figure 2 It can be seen that MSe x MSe in rGO hydrogel x There are no stray peaks caused by phase separation. Compared with the PDF standard card (PDF#97-004-0330), it can be seen that MSe x It is a cubic crystal.

[0082] Figure 3 This is the SEM image of the composite positive electrode material prepared in Example 1. Figure 3 There are no large agglomerated particles, which shows that the sulfur in the composite positive electrode material is evenly distributed and there is no obvious agglomeration.

[0083] Example 2

[0084] This embodiment provides a method for preparing a solid-state lithium-sulfur battery composite positive electrode material, comprising the following steps:

[0085] 1. Preparation of MSe x -rGO hydrogel:

[0086] 330 mg of selenium powder, 180 mg of reducing agent sodium borohydride and 20 ml of solvent DMF were mixed in a beaker to obtain a precursor solution.

[0087] 200 mg of rGO was mixed with 20 ml of deionized water to obtain rGO suspension.

[0088] C4H6CoO4·4H2O, NaMoO4·2H2O, C4H6FeO4·4H2O, C4H6CrO4·4H2O, Na2WO4·2H2O, and NH4VO3 with a total molar amount of 2 mmol of metal atoms were added to the rGO suspension at a metal atom molar ratio of 1:1:1:1:1:1, and magnetic stirring was performed for 10 minutes, and then the mixture was uniformly mixed with the precursor liquid. After stirring the mixed solution for 10 minutes, it was transferred into a microwave autoclave for heating treatment, and stirred while heating. The microwave heating power was 2000w, the stirring rate was 50r / min, the reaction time of the heating treatment was 1h, the reaction temperature was 200℃, and the pressure was 5 MPa.

[0089] The product after the reaction was separated into solid and liquid, and the obtained precipitate was washed alternately with alcohol and deionized water until the solution was neutral, and then the precipitate was freeze-dried to obtain MSe x -rGO hydrogel, in which MSe x It is a hexagonal crystal. x -rGO hydrogel has a specific surface area of ​​720 m 2 / g.

[0090] from Figure 4 It can be seen that the MSe prepared in this embodiment x MSe in rGO hydrogel x There are no impurity peaks caused by phase separation. Compared with the PDF standard card (PDF#00-038-1338), it can be seen that MSe x It is a hexagonal crystal.

[0091] 2. Preparation of MSe x -rGO hydrogel / S:

[0092] MSe x -rGO hydrogel and sublimated sulfur were mixed and ground to obtain a mixture with a sulfur content of 60% by mass. The mixture was placed in a sealed tube, the air in the tube was evacuated, the temperature was controlled at 160°C, and the insulation time was controlled at 12 h to allow the sublimated sulfur to evenly melt into the MSe x -rGO hydrogel to obtain MSe x -rGO hydrogel / S.

[0093] 3. Add 120 mg of MSe x -rGO hydrogel / S, 60 mgPEO, 20 mgLiTFSI (i.e., MSe x -rGO hydrogel / S:PEO:lithium salt (mass ratio 6:3:1) was stirred in 30 ml of acetonitrile solvent and heated at 80 °C for 8 h under nitrogen atmosphere to obtain a composite cathode material.

[0094] Example 3

[0095] This embodiment provides a method for preparing a solid-state lithium-sulfur battery composite positive electrode material, comprising the following steps:

[0096] 1. Preparation of MSe x -rGO hydrogel:

[0097] 330 mg of selenium powder, 50 mg of reducing agent hydrazine hydrate and 10 ml of solvent DMF were mixed in a beaker to obtain a precursor solution.

[0098] 200 mg of rGO was mixed with 10 ml of deionized water to obtain an rGO suspension.

[0099] C4H6CoO4·4H2O, C4H6NiO4·4H2O, C4H6CrO4·4H2O, MnC4H6O4·4H2O, and NH4VO3 with a total molar amount of 2 mmol of metal atoms were added to the rGO suspension at a metal atom molar ratio of 1:1:1:1:1, and magnetic stirring was performed for 20 minutes, and then the mixture was uniformly mixed with the precursor liquid. After stirring the mixed solution for 20 minutes, it was transferred into a microwave autoclave for heating treatment, and stirred while heating. The microwave heating power was 2000w, the stirring rate was 50r / min, the reaction time of the heating treatment was 2 h, the reaction temperature was 200℃, and the pressure was 5 MPa.

[0100] The product after the reaction was separated into solid and liquid, and the obtained precipitate was washed alternately with alcohol and deionized water until the solution was neutral, and then the precipitate was freeze-dried to obtain MSe x -rGO hydrogel, in which MSe x It is a cubic crystal. x -rGO hydrogel has a specific surface area of ​​756 m 2 / g.

[0101] 2. Preparation of MSe x -rGO hydrogel / S:

[0102] MSe x-rGO hydrogel and sublimated sulfur were mixed and ground to obtain a mixture with a sulfur content of 60% by mass. The mixture was placed in a sealed tube, the air in the tube was evacuated, the temperature was controlled at 160°C, and the insulation time was controlled at 12 h to allow the sublimated sulfur to evenly melt into the MSe x -rGO hydrogel to obtain MSe x -rGO hydrogel / S.

[0103] 3. 120 mg of MSe x -rGO hydrogel / S, 70 mgPEO, 10 mg LiTFSI (i.e., MSe x -rGO hydrogel / S:PEO:lithium salt (mass ratio 6:3.5:0.5) was stirred in 30 ml of acetonitrile solvent and heated at 80 °C for 8 h under nitrogen atmosphere to obtain a composite cathode material.

[0104] Example 4

[0105] This embodiment provides a method for preparing a solid-state lithium-sulfur battery composite positive electrode material, comprising the following steps:

[0106] 1. Preparation of MSe x -rGO hydrogel:

[0107] 330 mg of selenium powder, 50 mg of reducing agent hydrazine hydrate and 10 ml of solvent DMF were mixed in a beaker to obtain a precursor solution.

[0108] 200 mg of rGO was mixed with 10 ml of deionized water to obtain rGO suspension.

[0109] C4H6CoO4·4H2O, NaMoO4·2H2O, C4H6FeO4·4H2O, C4H6CrO4·4H2O, Na2WO4·2H2O, and NH4VO3 with a total molar amount of 2 mmol of metal atoms were added to the rGO suspension at a metal atom molar ratio of 1:1:1:1:1:1, and magnetic stirring was performed for 10 minutes, and then the mixture was uniformly mixed with the precursor liquid. The mixed solution was stirred for 10 minutes and then transferred to a microwave autoclave for heating treatment, and stirred while heating. The microwave heating power was 2000w, the stirring rate was 50r / min, the reaction time of the heating treatment was 1h, the reaction temperature was 200℃, and the pressure was 5 MPa.

[0110] The product after the reaction was separated into solid and liquid, and the obtained precipitate was washed alternately with alcohol and deionized water until the solution was neutral, and then the precipitate was freeze-dried to obtain MSe x -rGO hydrogel, in which MSe x It is a hexagonal crystal. xThe specific surface area of ​​rGO hydrogel is 892 m 2 / g.

[0111] 2. Preparation of MSe x -rGO hydrogel / S:

[0112] MSe x -rGO hydrogel and sublimated sulfur were mixed and ground to obtain a mixture with a sulfur content of 60% by mass. The mixture was placed in a sealed tube, the air in the tube was evacuated, the temperature was controlled at 160°C, and the insulation time was controlled at 12 h to allow the sublimated sulfur to evenly melt into the MSe x -rGO hydrogel to obtain MSe x -rGO hydrogel / S.

[0113] 3. 80 mg of MSe x -rGO hydrogel / S, 100 mg of PEO, 20 mg of LiTFSI (i.e., MSe x -rGO hydrogel / S:PEO:lithium salt (mass ratio 4:5:1) was stirred in 30 ml of acetonitrile solvent and heated at 80 °C for 8 h under nitrogen atmosphere to obtain a composite cathode material.

[0114] Example 5

[0115] This embodiment provides a method for preparing a solid-state lithium-sulfur battery composite positive electrode material, comprising the following steps:

[0116] 1. Preparation of MSe x -rGO hydrogel:

[0117] 330 mg of selenium powder, 180 mg of reducing agent sodium borohydride and 20 ml of solvent DMF were mixed in a beaker to obtain a precursor solution.

[0118] 200 mg of rGO was mixed with 20 ml of deionized water to obtain rGO suspension.

[0119] C4H6CoO4·4H2O, NaMoO4·2H2O, C4H6FeO4·4H2O, C4H6CrO4·4H2O, Na2WO4·2H2O, NH4VO3, MnC4H6O4·4H2O, C4H6NiO4·4H2O with a total molar amount of 2 mmol of metal atoms were added to the rGO suspension at a metal atom molar ratio of 1:1:1:1:1:1:1:1, and magnetic stirring was performed for 10 minutes, and then the mixture was uniformly mixed with the precursor liquid. The mixed solution was stirred for 10 minutes and then transferred into a microwave autoclave for heating treatment, and stirred while heating. The microwave heating power was 2000w, the stirring rate was 50r / min, the reaction time of the heating treatment was 1 h, the reaction temperature was 200℃, and the pressure was 5MPa.

[0120] The product after the reaction was separated into solid and liquid, and the obtained precipitate was washed alternately with alcohol and deionized water until the solution was neutral, and then the precipitate was freeze-dried to obtain MSe x -rGO hydrogel, in which MSe x It is a cubic crystal. x -rGO hydrogel has a specific surface area of ​​963 m 2 / g.

[0121] 2. Preparation of MSe x -rGO hydrogel / S:

[0122] MSe x -rGO hydrogel and sublimated sulfur were mixed and ground to obtain a mixture with a sulfur content of 60% by mass. The mixture was placed in a sealed tube, the air in the tube was evacuated, the temperature was controlled at 160°C, and the insulation time was controlled at 12 h to allow the sublimated sulfur to evenly melt into the MSe x -rGO hydrogel to obtain MSe x -rGO hydrogel / S.

[0123] 3. Add 120 mg of MSe x -rGO hydrogel / S, 60 mg of PEO, 20 mg of LiTFSI (i.e., MSe x -rGO hydrogel / S:PEO:lithium salt (mass ratio 6:3:1) was stirred in 30 ml of acetonitrile solvent and heated at 80 °C for 8 h under nitrogen atmosphere to obtain a composite cathode material.

[0124] Example 6

[0125] This embodiment provides a method for preparing a solid-state lithium-sulfur battery composite positive electrode material, comprising the following steps:

[0126] 1. Preparation of cubic MSe x-rGO hydrogel:

[0127] 330 mg of selenium powder, 180 mg of reducing agent sodium borohydride and 20 ml of solvent DMF were mixed in a beaker to obtain a precursor solution.

[0128] 200 mg of rGO was mixed with 20 ml of deionized water to obtain rGO suspension.

[0129] C4H6CoO4·4H2O, C4H6CrO4·4H2O, MnC4H6O4·4H2O, and C4H6NiO4·4H2O with a total molar amount of 2 mmol of metal atoms were added to the rGO suspension at a metal atom molar ratio of 1:1:1:1, and magnetic stirring was performed for 10 minutes, and then the precursor liquid was uniformly mixed. The mixed solution was stirred for 10 minutes and then transferred to a microwave autoclave for heating treatment, and stirred while heating. The microwave heating power was 2000w, the stirring rate was 50r / min, the heating treatment, the reaction time was 1 h, the reaction temperature was 200℃, and the pressure was 5 MPa.

[0130] The product after the reaction was separated into solid and liquid, and the obtained precipitate was washed alternately with alcohol and deionized water until the solution was neutral, and then the precipitate was freeze-dried to obtain MSe x -rGO hydrogel, in which MSe x It is a cubic crystal. x -rGO hydrogel has a specific surface area of ​​630 m 2 / g.

[0131] 2. Preparation of MSe x -rGO hydrogel / S:

[0132] MSe x -rGO hydrogel was mixed and ground with sulfur to obtain a mixture with a sulfur content of 60% by mass. The mixture was placed in a sealed tube, the air in the tube was evacuated, the temperature was controlled at 160°C, and the insulation time was controlled at 12 h to allow the sublimated sulfur to evenly melt into the MSe x -rGO hydrogel to obtain MSe x -rGO hydrogel / S.

[0133] 3. Add 120 mg of MSe x -rGO hydrogel / S, 60 mg of PEO, 20 mg of LiTFSI (i.e., MSe x -rGO hydrogel / S:PEO:lithium salt (mass ratio 6:3:1) was stirred in 30 ml of acetonitrile solvent and heated at 80 °C for 8 h under nitrogen atmosphere to obtain a composite cathode material.

[0134] Comparative Example 1

[0135] This comparative example is basically the same as Example 1, except that the MSe x During the preparation of -rGO hydrogel, only C4H6NiO4·4H2O with a total molar amount of metal atoms of 2 mmol was added, and no other types of metal salts were added. x -rGO hydrogel has a specific surface area of ​​360 m 2 / g.

[0136] Comparative Example 2

[0137] This comparative example is basically the same as Example 1, except that the MSe x During the preparation of -rGO hydrogel, only 1 mmol of C4H6NiO4·4H2O and 1 mmol of C4H6CoO4·4H2O were added, and no other types of metal salts were added. x -rGO hydrogel has a specific surface area of ​​425 m 2 / g.

[0138] Comparative Example 3

[0139] This comparative example is basically the same as Example 1, except that the MSe x During the preparation of -rGO hydrogel, only C4H6NiO4·4H2O, C4H6CrO4·4H2O and C4H6CoO4·4H2O with a total molar amount of 2 mmol of metal atoms were added, and the molar ratio of the three was 1:1:1, and no other types of metal salts were added. x -rGO hydrogel has a specific surface area of ​​580 m 2 / g.

[0140] Test example

[0141] The composite positive electrode materials prepared in the embodiment and the comparative example were respectively used to prepare solid-state lithium-sulfur batteries according to conventional methods. The specific steps are: preparing the composite positive electrode material into a slurry and coating it evenly on the carbon-coated aluminum foil. The loading amount of the composite positive electrode material on the carbon-coated aluminum foil is 4 g / cm 2 , dried in a vacuum oven at 80°C for 10 h, and cut into circular pole pieces with a diameter of 12 mm after drying. The circular pole piece prepared above is used as the positive electrode, the lithium indium alloy (lithium indium mass ratio 4:1) is used as the negative electrode, and the solid electrolyte is PEO-LiTFSI (where PEO:LiTFSI mass ratio 7:3).

[0142] The solid-state lithium-sulfur battery was tested by cyclic charge and discharge for 100 cycles at a current density of 0.1C. The test results are shown in Figure 5 and Table 1.

[0143] The test process of rate performance is to cycle five times at current densities of 0.2C, 0.5C and 2C respectively, and take the average value of the discharge mass specific capacity of the five cycles as the discharge mass specific capacity at the test rate. The test results are shown in Table 2.

[0144] Table 1 Electrical properties of solid-state lithium-sulfur batteries

[0145]

[0146] Table 2 Rate performance of solid-state lithium-sulfur batteries

[0147]

[0148] As shown in Table 1, the mass specific capacity of the solid-state lithium-sulfur battery prepared by the composite positive electrode material of the present invention is significantly improved. Figure 5 It can also be seen that the solid-state lithium-sulfur battery made from the composite positive electrode material of the present invention has good cycle performance and rate performance.

[0149] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A solid-state lithium-sulfur battery composite positive electrode material, characterized in that: Including MSe x -rGO hydrogel / S, polyethylene oxide, and lithium salt; x is 1.8~2.2; M is a combination of cobalt, nickel, chromium, manganese and vanadium; or M is a combination of cobalt, molybdenum, iron, chromium, tungsten and vanadium; or M is a combination of cobalt, molybdenum, nickel, iron, chromium, manganese, tungsten and vanadium; MS x -rGO hydrogel / S, the mass content of S is 50%~80%; MS x -rGO hydrogel / S:polyethylene oxide:lithium salt mass ratio is (4~6):(3~5):(0.5~1); The molar ratio of every two metal atoms in M ​​is (0.8~1.2):(0.8~1.2).

2. The solid-state lithium-sulfur battery composite positive electrode material according to claim 1, characterized in that: At least one of the following conditions is met: (1) MSe x -rGO hydrogel has a specific surface area of ​​300~1000 m 2 / g; (2) The lithium salt is selected from lithium bis(trifluoromethanesulfonyl)imide, LiNO3, LiI and Li a S b At least one of, wherein 3≤a≤5, 1≤b≤2.

3. A method for preparing a solid-state lithium-sulfur battery composite positive electrode material, characterized in that: The following steps are involved: S1. Preparation of MSe x -rGO hydrogel; x is 1.8~2.2; M is a combination of cobalt, nickel, chromium, manganese and vanadium; or M is a combination of cobalt, molybdenum, iron, chromium, tungsten and vanadium; or M is a combination of cobalt, molybdenum, nickel, iron, chromium, manganese, tungsten and vanadium; The molar ratio of every two metal atoms in M ​​is (0.8~1.2):(0.8~1.2); S2, MSe x -rGO hydrogel was mixed with sulfur to obtain a mixture, and then vacuum-melted to obtain MSe x -rGO hydrogel / S; in the mixture, the mass content of S is 50%~80%; S3. Transfer MSe x -rGO hydrogel / S, polyethylene oxide, lithium salt and a first solvent are mixed under a protective atmosphere to obtain a first mixed solution, and the first mixed solution is heated and stirred to obtain a composite positive electrode material; MS x -rGO hydrogel / S:polyethylene oxide:lithium salt mass ratio is (4~6):(3~5):(0.5~1).

4. The method for preparing a solid-state lithium-sulfur battery composite positive electrode material according to claim 3, characterized in that: The S1 includes: Mixing a selenium source, a reducing agent and a second solvent to prepare a precursor liquid; Mixing rGO with water to prepare an rGO suspension, and mixing a salt containing M with the rGO suspension to prepare a second mixed solution; The precursor liquid is mixed with the second mixed liquid to obtain a third mixed liquid, and the third mixed liquid is heated to obtain MSe x -rGO hydrogel.

5. The method for preparing a solid-state lithium-sulfur battery composite positive electrode material according to claim 4, characterized in that: The S1 satisfies at least one of the following conditions: (1) The reducing agent includes at least one of sodium borohydride, hydrazine hydrate and oxalic acid; (2) The molar ratio of the reducing agent to the selenium source is (1-3): (1-50); (3) The selenium source includes at least one of selenium powder and selenium dioxide; (4) heating the third mixed liquid by microwave solvothermal method; (5) the second solvent comprises at least one of DMF and NMP; (6) In the step of heating the third mixed liquid, the heating temperature is 160-260° C., the heating time is 0.5-3 h, and the pressure is 3 MPa-6 MPa.

6. The method for preparing a solid-state lithium-sulfur battery composite positive electrode material according to claim 3, characterized in that: In S2, the vacuum melting temperature is 150-160°C and the time is 10-15 h; and / or In the step S3 of heating and stirring the first mixed solution, the heating temperature is 50-100° C. and the heating time is 5-10 hours.

7. A solid-state lithium-sulfur battery, characterized in that: Including positive electrode, The positive electrode plate comprises the solid-state lithium-sulfur battery composite positive electrode material according to any one of 1 to 2 or the solid-state lithium-sulfur battery composite positive electrode material prepared by the method for preparing the solid-state lithium-sulfur battery composite positive electrode material according to any one of claims 3 to 6.

8. The solid-state lithium-sulfur battery according to claim 7, characterized in that: In the positive electrode sheet, the sulfur loading is 0.8~20 mg / cm 2 .

Citation Information

Patent Citations

  • CoSe<2> / graphene composite material preparation method and use

    CN109473643A

  • Composite positive electrode, all-solid-state lithium-sulfur battery and dry preparation methods of composite positive electrode and all-solid-state lithium-sulfur battery

    CN112599724A

  • Positive electrode / negative electrode material of lithium-sulfur battery and preparation method of positive electrode / negative electrode material

    CN114335468A

  • High energy-density lithium-sulfur battery and method for making the same

    US20240113388A1