A attapulgite-alumina carrier-supported nickel-based catalyst and its preparation and application
By loading the nickel-based catalyst on the attapulgite rod-alumina carrier, the problem of insufficient activity and stability of the existing C4 olefin composite catalyst is solved, and efficient and low-cost C4 olefin conversion and selectivity are achieved, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202410753414.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Existing C4 olefin stacking catalysts have problems such as insufficient activity, insufficient stability, and high production costs. It is difficult to effectively utilize excess low-value C4 olefins. Especially in the butene stacking reaction, the catalyst is prone to muddying and deactivation. , and are sensitive to butadiene, nitrogen compounds, sulfides, etc., posing safety risks.
Attapulgite rod-alumina carrier is used to support nickel-based catalysts. By using nickel oxides, iron oxides, aluminum, zinc, tin and other metal oxides as the main active and co-active components, it combines high specific surface area and microporous structure. The composite carrier is prepared by surface deposition and kneading forming processes to form a catalyst with high activity and selectivity.
It achieves high conversion rate and excellent selectivity of C4 olefins, reduces production costs, improves the stability and regeneration performance of the catalyst, and is suitable for industrial applications.
Smart Images

Figure CN118594543B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to an attapulgite-alumina carrier-supported nickel-based catalyst and the preparation and application thereof. Background Art
[0002] In various refineries and petrochemical production processes, such as the distillate or residue of catalytic cracking (FCC) of crude oil, steam reforming of hydrocarbons, Fischer-Tropsch synthesis, isobutane dehydrogenation and other thermal technologies, a large amount of C4 olefin fractions are produced, including 1-butene, isobutylene, cis-2-butene and trans-2-butene. At the same time, with the rapid development of domestic coal chemical industry, methanol to olefins (MTO) technology has made continuous breakthroughs, and industrial units have been put into production. It is reported that by 2022, the capacity of MTO projects will reach 15 million tons / year, and the capacity will be expanded year by year. The main components of mixed C4 olefin products are 1-butene, cis-2-butene, isobutylene, and a small amount of 1,3-butadiene, butane, etc. The comprehensive utilization of these large amounts of excess and low-value C4 olefins has become one of the problems that petrochemical companies urgently need to solve.
[0003] So far, researchers have developed a series of schemes for utilizing butene, such as butene alkylation reaction, butene superposition reaction, and the production of methyl ethyl ketone, sec-butyl alcohol, sec-butyl acetate, etc. from butene. Among them, the butene superposition reaction is an effective means of comprehensive utilization of butene. This reaction has the characteristics of wide range of raw materials and wide application of products. The raw materials can be any butene isomers, including the whole fraction of butene and some isomers, such as 1-butene, isobutylene and 2-butene which is difficult to utilize. The products are widely distributed, diverse and have many uses. They can be used directly or after hydrogenation as high-octane gasoline blending components, which are currently in short supply, and can also be used as raw materials for many fine chemicals with high added value. The synthesized dimer C8 olefins such as 2,4,4-trimethyl-1-pentene and 2,4,4-trimethyl-2-pentene can be used to synthesize tert-octylphenol, and can also be used to prepare isononyl alcohol through hydroformylation, or to prepare amine antioxidants through addition reaction. They can also be used to synthesize high-carbon olefins and then synthesize high-carbon olefin fine chemicals; trimer C12 olefins are important intermediates for preparing plasticizers, additives or detergents, and are widely used in medicine, fuel, spices and flavors. It can be seen that the butene superposition reaction is an effective means to solve the problem of butene outlet and comprehensive utilization of butene.
[0004] At present, a widely used catalyst in the C4 olefin superposition process is the solid phosphoric acid catalyst used in the SPAC process developed by UOP in the United States. It is made by loading phosphoric acid with diatomite as a carrier, but the catalyst is easy to mud, easy to agglomerate, and cannot be regenerated after deactivation, and the waste catalyst contains a large amount of phosphorus. After improvement, such as the addition of boric acid to stabilize the skeleton structure by the Shanghai Petrochemical Research Institute, the problem of easy mudification, low activity, and poor product selectivity of the catalyst was improved. The conversion rate of mixed butene increased from 75% to 91%, and the product was mainly composed of dimer isooctene, and the selectivity of trimer dodecene was less than 10%, and the reaction temperature was high, and the mudification and deactivation of the catalyst was not completely solved. Another is the Dimersol process developed by the French Petroleum Research Institute (IFP), which uses nickel salt as the main catalyst and adds an excess of alkyl aluminum as a co-catalyst Ziegler-Natta catalyst system to catalyze the polymerization of n-butene or mixed C4 olefins. The advantages of this process are that nickel salt is cheap and easy to obtain, and the catalyst has high activity and high selectivity. US4613580 patent describes that the toluene solution containing AlEtCl2 is reacted with anhydrous AlCl3 toluene solution under N2 gas protection, and then impregnated with spherical alumina soaked with Ni(NO3)2, and washed and dried to make a butene dimerization catalyst, and its butene conversion rate can reach 50~90%. EP 0012685A proposes to use divalent Ni compound, alkyl aluminum halide and CF3COOH to form a composite catalyst for butene dimerization, and the single-pass conversion rate of butene is 45~67%. However, the above-mentioned catalyst introduces alkyl aluminum components, which makes the catalyst preparation difficult, and cannot be recycled. It is difficult to separate the reaction product and the catalyst. A large amount of waste water is produced during the aftertreatment of excessive alkyl aluminum. At the same time, alkyl aluminum is flammable and explosive, and there is a large safety risk. Therefore, it is safer and more stable to adopt a supported catalyst without adding alkyl aluminum components. As reported in European patent EP 0439865, the used catalyst is made of SiO2-Al2O3 as a carrier and loaded with NiO. However, the catalyst is sensitive to butadiene, nitrides, sulfides, and oxygen-containing compounds and is easily poisoned, so the raw materials need to be pretreated. 2 / g, 60nm pore size granular SiO2 as a carrier, phosphoric acid is loaded on it, and is used for isobutylene polymerization to make gasoline, but the process for 1-butene polymerization is rare. British patent GB1069296 describes an olefin dimerization catalyst containing aluminum and nickel oxides loaded on SiO2, but the olefin conversion rate of the catalyst is low.
[0005] Attapulgite (ATP) is a widely distributed hydrated magnesium aluminum silicate clay mineral with a layered chain structure. It is abundant and has many unique properties such as high specific surface area, micro-mesoporous structure, surface acidity, good thermal stability and adsorption performance. It is a potential low-cost catalyst carrier. However, the application of ATP carrier in industrial catalysts has not been reported yet.
[0006] In summary, the current reaction of C4 olefins to prepare C8 and C12 olefins still has some problems, such as insufficient catalyst activity, insufficient stability, high production cost, etc. Therefore, it is urgent to develop a catalyst with better performance and lower cost. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide a nickel-based catalyst supported on a attapulgite-alumina carrier with high selectivity, good stability and regeneration performance, and the preparation and application thereof.
[0008] Another technical problem to be solved by the present invention is to provide a method for preparing the attapulgite-alumina carrier-loaded nickel-based catalyst.
[0009] The third technical problem to be solved by the present invention is to provide an application of the attapulgite-alumina carrier loaded with a nickel-based catalyst.
[0010] In order to solve the above problems, the present invention discloses a nickel-based catalyst supported on a attapulgite-alumina carrier, characterized in that: the nickel-based catalyst consists of a main active component, an auxiliary active component and a composite carrier; the main active component is one or more nickel oxides, or one or more nickel oxides and iron oxides, and its loading amount is 2% to 20%; the auxiliary active component is one or more aluminum, zinc, tin, and titanium metal oxides, and its loading amount is 1 to 5%; the composite carrier is a mixture of attapulgite (ATP) and alumina in a mass ratio of 2:8 to 8:2.
[0011] The molar ratio of nickel atoms to iron atoms in the main active component is 1-10:10-1.
[0012] The specific surface area of the composite carrier is 20-500 m 2 / g, the pore diameter is 3~50nm, and the pore volume is 0.3~1.6mL / g.
[0013] When the content of attapulgite (ATP) is 20% to 70%, the surface area of the composite carrier is 50 to 200 m 2 / g, pore size is 10~20nm.
[0014] The alumina in the composite carrier is γ-Al2O3, which is prepared by calcining pseudo-boehmite at a high temperature of 400-600°C; the specific surface area of the pseudo-boehmite is 200-500 m 2 / g, the pore diameter is 3~50nm, and the pore volume is 0.3~1.6mL / g.
[0015] The method for preparing a nickel-based catalyst supported on a attapulgite-alumina carrier as described above is characterized in that: the carrier attapulgite (ATP) and alumina (γ-Al2O3) are mixed in proportion and immersed in a nickel metal salt solution or a nickel and iron metal salt solution for 5 to 24 hours, placed on a quartz plate after drying and then transferred into the cavity of an atomic layer deposition device, using N2 as a carrier gas and an ethanol solution of an auxiliary metal for surface deposition cycles of 10 to 100 times and then calcined to obtain a catalyst A.
[0016] The method for preparing a nickel-based catalyst supported on a attapulgite-alumina carrier as described above is characterized in that: the carrier attapulgite and alumina are mixed in proportion, and a kneading agent is added for kneading and molding, and a molded ATP / γ-Al2O3 composite carrier is obtained through drying and calcining. The composite carrier is immersed in a nickel metal salt solution or a nickel and iron metal salt solution for 5 to 24 hours, and after drying, it is placed on a quartz sheet and then transferred into the cavity of an atomic layer deposition device. With N2 as the carrier gas, an ethanol solution of the auxiliary metal is used for surface deposition for 10 to 100 cycles, and then calcined to obtain catalyst B.
[0017] Catalyst A was mechanically crushed into powder by a pulverizer, and then a kneading agent was added to knead it into a shape. After drying, it was placed on a quartz plate and then transferred into the cavity of an atomic layer deposition device. With N2 as a carrier gas, an ethanol solution of an auxiliary metal was used for surface deposition cycles of 10 to 100 times, and then calcined to obtain catalyst C.
[0018] The nickel metal salt solution or the nickel and iron metal salt solution refers to one or more of nitrates, sulfates, acetates, acetates, and chlorides of nickel metal or nickel and iron metal, and the concentration of the solution is 1 mol / L to 5 mol / L.
[0019] The auxiliary metal in the auxiliary metal ethanol solution refers to one or more of isopropanol or sec-butanol of metal aluminum, zinc, tin, and titanium, and the concentration of the solution is 1 mol / L to 5 mol / L.
[0020] The drying conditions refer to a temperature of 60°C to 150°C and a time of 1 to 24 hours; the calcination conditions refer to a temperature of 400°C to 600°C and a time of 6 to 12 hours.
[0021] The kneading agent refers to one or more of dilute nitric acid, dilute sulfuric acid and dilute phosphoric acid with a mass fraction of 1% to 10%.
[0022] The use of a nickel-based catalyst supported on a attapulgite-alumina carrier as described above is characterized in that: the nickel-based catalyst is contacted with C4 olefins in a fixed bed reactor at a temperature of 50-180°C, a pressure of 2.0-5.0 MPa, and a volume space velocity of 0.1-5.0 h-1 in the case of a raw material liquid. -1 The superposition reaction was carried out under the conditions of .
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] 1. In the present invention, a composite carrier of attapulgite having a layered chain structure and alumina having multiple acidic sites is used to load one or more oxides of active metal nickel, or one or more oxides of nickel and iron. Therefore, the obtained catalyst has the characteristics of high activity and selectivity, good stability and regeneration performance.
[0025] 2. The present invention can effectively improve the polymerization activity of C4 olefins and the distribution of C8 and C12 olefin products by changing the ratio of the catalyst carrier, the content of the metal active component, and the type of the auxiliary agent.
[0026] 3. The preparation process of the present invention is simple and low in cost, and can achieve a C4 olefin conversion rate of 60% to 95%, a C8 olefin selectivity of 45% to 75%, and a C12 olefin selectivity of 25% to 35%, and has extremely strong industrial value and prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.
[0028] Figure 1 This is a TEM characterization image of the NiO / ATP catalyst of the present invention.
[0029] Figure 2 This is a SEM characterization image of the surface morphology of the NiO / ATP catalyst of the present invention.
[0030] Figure 3 This is a diagram of the NiO / ATP-γ-Al2O3 extrusion molding catalyst of the present invention. DETAILED DESCRIPTION
[0031] A nickel-based catalyst supported on a attapulgite-alumina carrier, the nickel-based catalyst consisting of a main active component, an auxiliary active component and a composite carrier. The main active component is one or more of nickel oxides, or one or more of nickel oxides and iron oxides, and the loading mass percentage thereof is 2% to 20%, preferably 10% to 15%. The auxiliary active component is one or more of aluminum, zinc, tin, and titanium metal oxides, and the loading amount thereof is 1 to 5%. The composite carrier is a mixture of attapulgite (ATP) with a mass ratio (g / g) of 2:8 to 8:2 and the balance being alumina. The content of ATP is preferably 30 to 60%.
[0032] Wherein: the molar ratio of nickel atoms to iron atoms in the main active component is 1-10:10-1, and preferably the molar ratio of nickel atoms to iron atoms is 2-3:3-2.
[0033] The specific surface area of the composite carrier is 20~500 m 2 / g, the pore diameter is 3~50nm, and the pore volume is 0.3~1.6mL / g.
[0034] When the content of attapulgite is 20%~70%, the surface area of the composite carrier is 50~200m 2 / g, pore size is 10~20nm.
[0035] The alumina in the composite carrier is γ-Al2O3, which is prepared by calcining pseudo-boehmite at a high temperature of 400-600℃; the specific surface area of pseudo-boehmite is 200-500 m 2 / g, the pore diameter is 3~50nm, and the pore volume is 0.3~1.6mL / g.
[0036] A method for preparing a nickel-based catalyst supported on a attapulgite-alumina carrier, comprising three methods.
[0037] The first method: the carrier attapulgite (ATP) and alumina (γ-Al2O3) are mixed in proportion and immersed in a nickel metal salt solution or a nickel and iron metal salt solution for 5 to 24 hours. After drying at 60°C to 150°C for 1 to 24 hours, the mixture is placed on a quartz wafer and then transferred into the chamber of an atomic layer deposition device. With N2 as the carrier gas and an ethanol solution of the auxiliary metal, the surface deposition cycle is carried out for 10 to 100 times and then calcined at 400°C to 600°C for 6 to 12 hours to obtain catalyst A.
[0038] The second method: the carrier attapulgite (ATP) and alumina (γ-Al2O3) are mixed in proportion, and a kneading agent is added to knead and form, and the molded ATP / γ-Al2O3 composite carrier is obtained by drying at 60℃~150℃ for 1~24h and calcining at 400℃~600℃ for 6~12h. The composite carrier is immersed in a nickel metal salt solution or a nickel and iron metal salt solution for 5~24h, dried at 60℃~150℃ for 1~24h, placed on a quartz wafer and then transferred into the atomic layer deposition equipment cavity. With N2 as the carrier gas, the surface deposition is carried out using an ethanol solution of the auxiliary metal, and then calcined at 400℃~600℃ for 6~12h to obtain catalyst B.
[0039] The third method: After the catalyst A is mechanically ground into powder by a pulverizer, a kneading agent is added to knead it into a powder, and then it is placed on a quartz plate after being dried at 60℃~150℃ for 1~24h and then transferred into the cavity of the atomic layer deposition equipment. With N2 as the carrier gas, an ethanol solution of the auxiliary metal is used for surface deposition cycles of 10~100 times, and then it is calcined at 400℃~600℃ for 6~12h to obtain the catalyst C.
[0040] The above-mentioned nickel metal salt solution or nickel and iron metal salt solution refers to one or more of nitrates, sulfates, acetates, acetates, and chlorides of nickel metal or nickel and iron metal, and the concentration of the solution is 1 mol / L to 5 mol / L.
[0041] The auxiliary metal in the ethanol solution of the auxiliary metal refers to one or more of isopropanol or sec-butanol of metal aluminum, zinc, tin, and titanium, and the concentration of the solution is 1 mol / L to 5 mol / L.
[0042] The kneading agent refers to one or more of dilute nitric acid, dilute sulfuric acid, and dilute phosphoric acid with a mass fraction of 1% to 10%.
[0043] Application of a attapulgite-alumina carrier loaded with nickel-based catalyst:
[0044] The nickel-based catalyst is contacted with C4 olefins in a fixed bed reactor at a temperature of 50-180°C, a pressure of 2.0-5.0 MPa, and a volume space velocity of 0.1-5.0 h / min. -1 The preferred reaction conditions are: temperature of 70-150°C, pressure of 2.0-3.0 MPa, and volumetric space velocity of 0.2-2.0 h -1 . After the reaction stabilizes, the liquid product is taken for chromatographic analysis 24 hours later, and the C4 olefin conversion rate is calculated according to the following formula, and the product selectivity is calculated by gas chromatography quantitative analysis.
[0045]
[0046] Wherein: C4 olefins include one or more of mixed butenes, 1-butene, 2-butene (cis and trans), the C4 olefin content is greater than 25%, in addition to C4 olefins, there are C4 alkanes (isobutane, normal butane), C3 olefins and alkanes.
[0047] The impurity content of C4 olefin raw materials is less than 500ppm of butadiene, less than 1ppm of nitrides (basic or non-basic nitrides), less than 5ppm of sulfides (such as sulfides, hydrosulfides, carbonyl sulfides), and less than 200ppm of oxygen-containing compounds (such as water, alcohols, ketones, ethers, etc.).
[0048] The present invention is applied to the selective superposition of C4 olefins to prepare C8 olefins and C12 olefins, wherein the C8 product is mainly methylheptene and dimethylhexene, and the C12 product is mainly nonene and its isomers. The product distribution is shown below.
[0049]
[0050] Comparative Example
[0051] Preparation method using catalyst A (without adding alumina):
[0052] Weigh 10.74g NiSO4·H2O and dissolve it in 40ml deionized water. After dissolution, pour it into a three-necked flask, add 23.67g calcined ATP, and then add 200ml deionized water. Place the three-necked flask in an oil bath and raise the temperature to 70℃. Stir mechanically for 2h and then take it out. Pour the suspension in the three-necked flask into a round-bottomed flask and place it in a rotary evaporator to evaporate it until it is completely dry. Keep the obtained solid powder in an oven at a constant temperature of 110℃. o C for 12 hours, place the dried solid powder on a quartz plate and then put it into the cavity of the atomic layer deposition equipment, weigh 5.0g of aluminum isopropoxide and dissolve it in ethanol solution, use N2 as the carrier gas, and after 10 deposition cycles, take out the catalyst, place it in a muffle furnace and program the temperature to 500℃ and bake it for 4 hours, grind the obtained solid powder and sieve it, weigh 20g of solid particles larger than 100 mesh and put them into an aluminum box, set a pressure of 10MPa on the tablet press for tableting, grind and sieve after tableting, take 20~40 mesh particles to obtain catalyst A-1. Figure 1 and Figure 2 The TEM and SEM characterization images of catalyst A-1 show that the carrier attapulgite has a layered chain structure and metal oxide particles are loaded on its surface.
[0053] The catalyst A-1 was used for the superposition reaction of the mixed butenes whose components are listed in Table 1, at a reaction temperature of 90°C, a reaction pressure of 3.0 MPa, and a liquid hourly space velocity of 0.4 h -1After 24 hours of operation, the liquid product was collected in a wide-mouth bottle and analyzed by gas chromatography. The conversion of mixed butenes was 57.8%, the selectivity of C8 products was 54.6%, and the selectivity of C12 products was 23.7%.
[0054] Table 1: Composition of mixed butenes
[0055]
[0056] Example 1
[0057] Preparation method using catalyst A:
[0058] Weigh 5.46g Fe2(SO4)3•9H20 and 1.34g Ni(NO3)2•6H20, dissolve in 40ml deionized water to prepare a metal salt solution, pour into a three-necked flask, weigh 10.0g ATP and 15.0g γ-Al2O3 powder, add 200ml deionized water. The remaining catalyst preparation steps are the same as the comparative example to obtain catalyst A-2.
[0059] The catalyst A-2 is used for the superposition reaction of the mixed butenes whose components are listed in Table 1, at a reaction temperature of 80°C, a reaction pressure of 3.0 MPa, and a liquid hourly space velocity of 0.4 h -1 After 24 hours of operation, the liquid product was collected in a wide-mouth bottle and the product composition was analyzed by gas chromatography. The mixed butene conversion was 65.6%, the C8 olefin product selectivity was 51.2%, and the C12 olefin product selectivity was 22.0%.
[0060] Example 2
[0061] Preparation method using catalyst A:
[0062] Weigh 5.50g Fe2(SO4)3•9H20 and dissolve it in 40ml deionized water to prepare a metal salt solution and pour it into a three-necked flask. Weigh 12.0g ATP and 6.8g γ-Al2O3 powder and add 200ml deionized water. Place the three-necked flask in an oil bath and raise the temperature to 70°C. Take it out after mechanical stirring for 2h. Pour the suspension in the three-necked flask into a round-bottom flask and place it in a rotary evaporator to completely dry. Keep the temperature constant at 110°C in an oven and dry it for 12h. Place the dried solid powder on a quartz plate and put it into the cavity of the atomic layer deposition equipment. Weigh 5.0g titanium isopropoxide and dissolve it in ethanol solution. Use N2 as the carrier gas. After 10 deposition cycles, take out the catalyst. The remaining catalyst preparation steps are the same as those in the comparative example to obtain catalyst A-3.
[0063] The catalyst A-3 is used for the superposition reaction of the mixed butenes whose components are listed in Table 1, at a reaction temperature of 80°C, a reaction pressure of 3.0 MPa, and a liquid hourly space velocity of 0.5 h -1 After 24 hours of operation, the liquid product was collected in a wide-mouth bottle and the product composition was analyzed by gas chromatography. The mixed butene conversion was 64.8%, the C8 olefin product selectivity was 55.9%, and the C12 olefin product selectivity was 21.6%.
[0064] Example 3
[0065] Preparation method using catalyst A:
[0066] Weigh 10.74g Ni(NO3)2·6H2O and 2.92g Al2(SO4)3·18H2O and dissolve them in 40ml deionized water. Pour them into a three-necked flask after dissolution. Weigh 13.20g ATP and 8.8g γ-Al2O3 powder and add 200ml deionized water. The remaining catalyst preparation steps are the same as those of the comparative example to obtain catalyst A-4.
[0067] The catalyst A-4 is used for the superposition reaction of the mixed butenes whose components are listed in Table 1, at a reaction temperature of 80°C, a reaction pressure of 3.0 MPa, and a liquid hourly space velocity of 0.5 h -1 After 24 hours of operation, the liquid product was collected in a wide-mouth bottle and the product composition was analyzed by gas chromatography. The conversion of mixed butenes was 76.4%, the selectivity of C8 olefins was 56.5%, and the selectivity of C12 olefins was 19.5%.
[0068] Embodiments 4 to 8
[0069] This example illustrates the catalytic reaction effects of catalysts having different active metal contents including promoter metal contents.
[0070] The same catalyst preparation method and process reaction conditions as in Example 1 were used to carry out the superposition reaction of 1-butene (99.3%). The results are listed in Table 2.
[0071] Table 2: Effect of different active metal contents on the selective polymerization reaction of 1-butene
[0072]
[0073] Example 9
[0074] Preparation method using catalyst B:
[0075] Weigh 60g ATP and 20g γ-Al2O3 powder and mix them mechanically. Add deionized water at a water-powder mass ratio of 0.8, knead for 3-5h and shape into a strip carrier with a diameter of 2.0mm. Keep the temperature constant at 110℃ in an oven and dry for 12h. Roast in a muffle furnace at 500℃ for 4h. Slightly grind the carrier and sieve it to get a 20-40 mesh cylindrical carrier. Weigh 10.74g NiSO4•H2O was dissolved in 20 ml of deionized water to obtain a metal salt solution. 23.67 g of the prepared ATP / γ-Al2O3 composite carrier was weighed and immersed in the metal salt solution for 10 to 20 hours. The carrier was dried in an oven at 110°C for 12 hours. The dried solid particles were placed on a quartz plate and then placed in the cavity of the atomic layer deposition equipment. 10.0 g of aluminum isopropoxide was weighed and dissolved in an ethanol solution. N2 was used as the carrier gas. After 15 deposition cycles, the catalyst was taken out and placed in a muffle furnace and heated to 500°C for 4 hours to obtain catalyst B-1. Figure 3 This is the catalyst B-1 after extrusion molding, with a complete shape and metallic luster.
[0076] The catalyst B-1 is used for the superposition reaction of 1-butene at a reaction temperature of 90°C, a reaction pressure of 3.0 MPa, and a liquid hourly space velocity of 1.0 h -1 Under the conditions, after running for 24 hours, the liquid product was collected in a wide-mouth bottle and the product composition was analyzed by gas chromatography; the analysis showed that the 1-butene conversion rate was 85.7%, the C8 olefin product selectivity was 56.5%, and the C12 olefin product selectivity was 19.7%.
[0077] Example 10
[0078] Preparation method using catalyst C:
[0079] Weigh 100g of catalyst A-2 prepared in Example 1 and grind it into powder with a pulverizer. Add 10g of dilute nitric acid with a mass fraction of 5%, add deionized water with a water-powder mass ratio of 0.8, knead for 3-5h and shape it into a strip catalyst with a diameter of 2.0mm. Keep the temperature constant at 110°C in an oven and dry it for 12h. Place the dried molded catalyst on a quartz sheet and put it into the cavity of an atomic layer deposition equipment. Weigh 5.0g of titanium isopropoxide and dissolve it in ethanol solution. Use N2 as carrier gas. After 5 deposition cycles, take out the catalyst and heat it to 500°C in a muffle furnace and calcine it for 4h. Grind the obtained catalyst slightly and sieve it. Take a 20-40 mesh cylindrical catalyst to obtain catalyst C-1.
[0080] The catalyst C-1 was used for the polymerization reaction of 1-butene at a reaction temperature of 90°C, a reaction pressure of 3.0 MPa, and a liquid hourly space velocity of 1.0 h -1Under the conditions, after running for 24 hours, the liquid product was collected in a wide-mouth bottle and the product composition was analyzed by gas chromatography; the analysis showed that the 1-butene conversion rate was 86.5%, the C8 olefin product selectivity was 45.8%, and the C12 olefin product selectivity was 24.5%.
[0081] Embodiment 11
[0082] This example illustrates that the catalyst provided by the present invention has good stability.
[0083] Catalyst A-2 prepared in Example 1 was used to carry out a butene superposition experiment according to the process conditions of the comparative example, with mixed C4 olefins as substrates: the conversion rate was 45%-65%, the C8 olefin selectivity was 48%-65%, the C12 olefin selectivity was 17%-28%, and the lifespan was 600h; then, 1-butene was switched as the raw material, the conversion rate was 65-85%, the C8 olefin selectivity was 45%-70%, the C12 olefin selectivity was 15%-30%, and the lifespan was 600h.
[0084] It should be understood that the examples and embodiments discussed herein are for illustrative purposes only and that various modifications and changes may occur to those skilled in the art and are intended to be included within the spirit and scope of this application and the appended claims.
Claims
1. An application of a attapulgite-alumina carrier to support a nickel-based catalyst, characterized in that: The nickel-based catalyst is contacted with C4 olefins in a fixed bed reactor at a temperature of 50-180°C, a pressure of 2.0-5.0 MPa, and a volume space velocity of 0.1-5.0 h-1. -1 The superposition reaction is carried out under the conditions of; the nickel-based catalyst is composed of a main active component, an auxiliary active component and a composite carrier; the main active component is one or more of nickel oxides, or nickel oxides and iron oxides, and its loading amount is 2% to 20%; the auxiliary active component is one or more of aluminum, zinc, tin, and titanium metal oxides, and its loading amount is 1 to 5%; the composite carrier is a mixture of attapulgite and alumina in a mass ratio of 2:8 to 8:
2.
2. The use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 1, characterized in that: The molar ratio of nickel atoms to iron atoms in the main active component is 1-10:10-1.
3. The use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 1, characterized in that: The specific surface area of the composite carrier is 20-500 m 2 / g, the pore diameter is 3~50nm, and the pore volume is 0.3~1.6mL / g.
4. The use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 3, characterized in that: When the content of attapulgite is 20% to 70%, the surface area of the composite carrier is 50 to 200 m 2 / g, pore size is 10~20nm.
5. The use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 1, characterized in that: The alumina in the composite carrier is γ-Al2O3, which is prepared by calcining pseudo-boehmite at a high temperature of 400-600°C; the specific surface area of the pseudo-boehmite is 200-500 m 2 / g, the pore diameter is 3~50nm, and the pore volume is 0.3~1.6mL / g.
6. The use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 1, characterized in that: The preparation method of the nickel-based catalyst is as follows: the carrier attapulgite and alumina are mixed in proportion, the mixture is immersed in a nickel metal salt solution or a nickel and iron metal salt solution for 5 to 24 hours, the mixture is dried and placed on a quartz plate and then transferred into an atomic layer deposition equipment cavity, N2 is used as a carrier gas, an ethanol solution of an auxiliary metal is used for surface deposition for 10 to 100 cycles, and then the mixture is calcined to obtain a catalyst A.
7. The use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 1, characterized in that: The preparation method of the nickel-based catalyst is as follows: carrier attapulgite and alumina are mixed in proportion, and a kneading agent is added for kneading and molding, and a molded ATP / γ-Al2O3 composite carrier is obtained through drying and calcining. The composite carrier is immersed in a nickel metal salt solution or a nickel and iron metal salt solution for 5 to 24 hours, and after drying, it is placed on a quartz sheet and then transferred into an atomic layer deposition equipment cavity, and N2 is used as a carrier gas, and an ethanol solution of an auxiliary metal is used for surface deposition for 10 to 100 cycles, and then calcined to obtain a catalyst B.
8. The use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 6, characterized in that: Catalyst A was mechanically ground into powder using a pulverizer, and then a kneading agent was added to knead it into a powder. After drying, it was placed on a quartz plate and then transferred into the chamber of an atomic layer deposition device. With N2 as a carrier gas, an ethanol solution of an auxiliary metal was used for surface deposition cycles of 10 to 100 times, and then calcined to obtain catalyst C.
9. Use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 6 or 7, characterized in that: The nickel metal salt solution or the nickel and iron metal salt solution refers to one or more of nitrates, sulfates, acetates, and chlorides of nickel metal or nickel and iron metal, and the concentration of the solution is 1 mol / L to 5 mol / L.
10. Use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 6, 7 or 8, characterized in that: The auxiliary metal in the auxiliary metal ethanol solution refers to one or more of isopropanol or sec-butanol of metal aluminum, zinc, tin, and titanium, and the concentration of the solution is 1 mol / L to 5 mol / L.
11. Use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 6, 7 or 8, characterized in that: The drying conditions refer to a temperature of 60°C to 150°C and a time of 1 to 24 hours; the calcination conditions refer to a temperature of 400°C to 600°C and a time of 6 to 12 hours.
12. Use of a attapulgite-alumina carrier for supporting a nickel-based catalyst as claimed in claim 7 or 8, characterized in that: The kneading agent refers to one or more of dilute nitric acid, dilute sulfuric acid and dilute phosphoric acid with a mass fraction of 1% to 10%.
Citation Information
Patent Citations
A method of making a catalyst based on silicon dioxide and phosphoric acid
EP0371938A1
Polymerisation process
GB1069296A
Process for the oligomerization of olefins and a catalyst thereof
US4613580A
Composite adsorption desulfurizing agent and preparation method thereof
CN101322915A
Olefin oligomerization method
CN107159278A