A bio-based polyphosphazene flame retardant and flame-retardant cable material

By combining bio-based long chain bio-based polyphosphazene flame retardant with melamine cyanurate on the cyclophosphazene skeleton, the problems of circuit cable material hardening, moisture absorption and environmental pollution are solved, and high-efficiency resistance is achieved The combustion effect and good mechanical properties extend the service life of the cable.

CN118598917BActive Publication Date: 2024-11-26宁波聚泰新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078443.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-26
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing circuit cable flame retardants have problems such as hardening, moisture absorption, migration and environmental pollution. The traditional flame retardant materials have insufficient moisture and heat aging resistance and service life of new energy vehicle cables, and they affect the impact of improving flame retardant performance. Mechanical properties of materials.

Method used

Develop a bio-based polyphosphazene flame retardant to form a flame retardant with toughening effect by loading bio-based long chains on the cyclophosphazene skeleton, combining bio-based amines and hexachlorocyclotriphosphazene, and forming a flame retardant with melamine Cyanurate compound is used to prepare flame retardant cable materials.

Benefits of technology

It achieves flame retardant, biocompatible and biodegradable, while improving the mechanical properties and service life of cable materials, reducing fire hazards, and no need to add plasticizers, which is cheaper and more environmentally friendly and green.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118598917B_ABST
    Figure CN118598917B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of flame retardants, and relates to a bio-based polyphosphazene flame retardant and a flame retardant cable material. The present invention discloses a bio-based polyphosphazene flame retardant, and the preparation method thereof comprises: (1) in an inert atmosphere, mixing hexachlorocyclotriphosphazene and tetrahydrofuran to obtain a mixed solution A, and placing the mixed solution A in an ice-water bath for stirring and dissolving; (2) mixing a bio-based amine and tetrahydrofuran to obtain a mixed solution B; (3) dripping the mixed solution B into the mixed solution A, and continuously reacting in the ice-water bath for 1 to 12 hours; after the reaction is complete, the bio-based polyphosphazene flame retardant is obtained by liquid separation, rotary evaporation, and drying. The present invention also discloses a flame retardant cable material, which comprises 1 to 50 wt% of a bio-based polyphosphazene flame retardant. The bio-based polyphosphazene flame retardant of the present invention has a bio-based amine long chain, and the bio-based amine long chain is mainly an aliphatic chain segment, which has good flexibility, and thus can give the matrix a certain toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of flame retardants and relates to a bio-based polyphosphazene flame retardant and a flame retardant cable material. Background Art

[0002] The development of the new energy vehicle industry is a key strategic measure to address climate change and achieve emission reduction targets. In order to promote the industry's transformation to a low-carbon and green one, a number of regulations have been introduced. The in-vehicle circuit cables of new energy vehicles are key components to ensure the normal transmission of current. However, these cables are used in large quantities in new energy vehicles, are frequently bent, and have complex application environments.

[0003] At present, hexaphenoxy cyclotriphosphazene is often used as a flame retardant in the elastomer materials of circuit cables. The molecular structure of this flame retardant is mainly benzene rings, which has a certain rigidity and may cause the cable material to harden, affecting its application performance. In addition, although traditional phosphorus-nitrogen flame retardants, such as ammonium polyphosphate, can provide flame retardant effects, they have problems such as moisture absorption and migration, and their raw materials are mostly from non-renewable resources, which may reduce the moisture and heat aging resistance and service life of flame-retardant modified cable materials.

[0004] Flame retardant systems also face other challenges: (1) Although existing halogen-based flame retardant systems can meet flame retardant requirements, they produce thick smoke and corrosive gases when burned, posing long-term ecological risks to the environment. (2) Some studies have improved the flame retardant properties of cable materials by adding large amounts of hydroxides, such as aluminum hydroxide, but this approach requires a large amount of filler, which not only affects the processability of the material, but also reduces its mechanical properties, such as easy tearing.

[0005] Therefore, there is an urgent need to develop a new flame retardant that is both environmentally friendly and flame retardant while not affecting mechanical properties, and to apply it to circuit cable materials to extend their service life and adapt to various complex application environments. Summary of the invention

[0006] The purpose of the present invention is to address the above-mentioned problems existing in the prior art and propose a bio-based polyphosphazene flame retardant, which loads bio-based long chains on a cyclophosphazene skeleton and satisfies flame retardancy, biocompatibility and biodegradability at the same time; and the bio-based long chain structure can toughen the flame-retardant thermoplastic elastomer material and extend the service life.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] A bio-based polyphosphazene flame retardant, the general structural formula of which is shown in the following formula (1):

[0009] Formula (1);

[0010] Wherein R1 to R6 are independently selected from -NH-(CH 2 ) 8 -CH=CH-(CH 2 ) 7 -CH 3 、-NH-(CH 2 ) 5 -NH 2 , 、-NH-(CH 2 ) 3 -NH-(CH 2 ) 4 -NH 2 、-NH-(CH 2 ) 3 -NH-(CH 2 ) 4 -NH-(CH 2 ) 3 -NH 2 One of them.

[0011] Preferably, R1-R6 are derived from bio-based amines, and the bio-based amines include one or more of oleylamine, pentamethylenediamine, glucosamine, spermidine, and spermine.

[0012] Preferably, the structural formula of the polyphosphazene flame retardant includes one of the following formulas (2) to (6):

[0013] Formula (2);

[0014] Formula (3);

[0015] Formula (4);

[0016] Formula (5);

[0017] Formula (6).

[0018] A method for preparing a bio-based polyphosphazene flame retardant, comprising:

[0019] (1) In an inert atmosphere, hexachlorocyclotriphosphazene and tetrahydrofuran are mixed to obtain a mixed solution A, which is then placed in an ice water bath and stirred to dissolve;

[0020] (2) mixing the bio-based amine and tetrahydrofuran to obtain a mixed solution B;

[0021] (3) Add mixed solution B dropwise into mixed solution A and continue to react in an ice water bath for 1 to 12 hours. After the reaction is complete, separate the liquids, perform rotary evaporation, and dry to obtain a bio-based polyphosphazene flame retardant.

[0022] Preferably, the molar ratio of hexachlorocyclotriphosphazene to bio-based amine is 1:(3-12).

[0023] Preferably, the mass volume ratio of hexachlorocyclotriphosphazene to tetrahydrofuran in (1) is (3-12) g:50 ml.

[0024] Preferably, the mass volume ratio of bio-based amine to tetrahydrofuran in (2) is (20-50) g:50 ml.

[0025] Preferably, the bio-based amine includes one or more of oleylamine, pentamethylenediamine, glucosamine, spermine and spermidine.

[0026] A flame retardant cable material comprises 1-50wt% of a bio-based polyphosphazene flame retardant.

[0027] A flame-retardant cable material comprises 1-50wt% of a compound flame retardant; the compound flame retardant is composed of a bio-based polyphosphazene flame retardant and melamine cyanurate in a mass ratio of 1:(1-5).

[0028] Preferably, the composite flame retardant consists of a bio-based polyphosphazene flame retardant and melamine cyanurate in a mass ratio of 1:(2-3).

[0029] A method for preparing a flame retardant cable material, comprising:

[0030] Low-density polyethylene (LDPE), styrene-ethylene-butylene-styrene block copolymer (SEBS) and antioxidant are melt-blended in an internal mixer; 0-30wt% of melamine cyanurate and 1-20wt% of bio-based polyphosphazene flame retardant are added and then the mixture is uniformly blended; the mixture is then preheated, hot-pressed and cold-pressed in a flat vulcanizer to obtain the product.

[0031] Preferably, the method for preparing the flame retardant cable material comprises:

[0032] Low-density polyethylene (LDPE), styrene-ethylene-butylene-styrene block copolymer (SEBS) and antioxidant are melt-blended in an internal mixer; 10-30wt% of melamine cyanurate and 4-15wt% of bio-based polyphosphazene flame retardant are added and then blended evenly; then the mixture is preheated, hot-pressed and cold-pressed in a flat vulcanizer to obtain the product.

[0033] Preferably, the mass ratio of low-density polyethylene (LDPE), styrene-ethylene-butylene-styrene block copolymer (SEBS), and antioxidant is (100-300):(100-300):1.

[0034] Preferably, the melt blending temperature is 150-220° C., the rotation speed is 10-100 r / min, and the time is 5-60 min.

[0035] Preferably, the preheating temperature in the flat vulcanizer is 150-220°C, the hot pressing pressure is 10-50 MPa, the time is 1-30 min, and the temperature is 180-210°C, and the cold pressing pressure is 10-50 MPa, the time is 1-30 min, and the temperature is 15-25°C.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] 1. The bio-based polyphosphazene flame retardant of the present invention has a bio-based amine long chain, which is mainly an aliphatic chain segment and has good flexibility, thus giving the matrix a certain toughness;

[0038] 2. The bio-based polyphosphazene flame retardant of the present invention has amino groups, which can produce non-flammable gases such as ammonia and nitrogen after thermal decomposition, which helps to dilute the oxygen concentration and reduce the risk of fire;

[0039] 3. The present invention uses hexachlorocyclotriphosphazene containing a phosphorus oxychloride structure, which can react with bio-based amines containing hydroxyl groups, amino groups, etc. to form amino groups, and the reaction is simple and controllable;

[0040] 4. The flame-retardant cable material of the present invention contains a bio-based polyphosphazene flame retardant, or a composite flame retardant composed of a bio-based polyphosphazene flame retardant and melamine cyanurate, which can achieve a flame retardant effect; and improve the defect that high-filling flame retardants (such as melamine cyanurate, magnesium hydroxide, aluminum hydroxide, etc.) are easy to harden the cable material; and has a better flame retardant effect and better mechanical properties;

[0041] 5. The flame-retardant cable material of the present invention does not require the addition of plasticizers or other additives, thereby reducing costs and being more environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is an infrared spectrum of the bio-based polyphosphazene flame retardant, hexachlorocyclotriphosphazene and oleylamine prepared in Example 1 of the present invention.

[0043] Figure 2 Thermogravimetric curves of Application Examples 1, 2, and 5 of the present invention and Comparative Examples 1 and 2 are shown. DETAILED DESCRIPTION

[0044] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.

[0045] Unless otherwise specified, the materials used in the present invention are conventional commercial products, and the methods used are conventional technical means.

[0046] The test instrument used in the present invention comprises:

[0047] Infrared spectrometer: Thermo Scientific Nicolet iS20, USA;

[0048] Thermogravimetric analyzer: TGA200F1D00.00-00, NETZSCH Instrument Manufacturing Co., Ltd., Germany;

[0049] Oxygen index tester: F101 Shanghai Qianshi Precision Electromechanical Technology Co., Ltd.;

[0050] Universal testing machine: ED26.104 Yice Testing Equipment (Hangzhou) Co., Ltd.;

[0051] Cone calorimeter: vouch6810, Suzhou Yangyi Walch Testing Technology Co., Ltd. Example 1

[0052] Preparation method of bio-based polyphosphazene flame retardant

[0053] First, use pure nitrogen to remove all the air in a 250 ml three-necked flask, weigh 6.95 g (0.02 mol) of hexachlorocyclotriphosphazene and 50 ml of tetrahydrofuran, add them into the three-necked flask, and place it in an ice water bath for stirring and dissolving.

[0054] Weigh 32 g of oleylamine (0.12 mol) and dissolve it in 50 ml of tetrahydrofuran. Then transfer the oleylamine solution into a dropping funnel and install it on the above three-necked flask.

[0055] Adjust the speed of the mechanical stirring instrument to 2000 rpm, and slowly drip the solution in the dropping funnel at a rate of 1 drop per second until the dripping is complete. Continue stirring the reaction for 4 hours. After the reaction is completed, transfer the reaction solution in the three-necked flask to a separatory funnel, and add 100 ml of deionized water, and let it stand until the upper liquid and the lower liquid are completely separated. Among them, the upper liquid is a polyphosphazene flame retardant PPZ-OA dissolved in tetrahydrofuran, and the lower liquid is water. Take the upper liquid and perform rotary evaporation for 4 hours, and set the temperature to 65°C until all the solvent is evaporated. After the rotary evaporation is completed, transfer the residue to a watch glass, and then place it in a vacuum drying oven and dry it to constant weight, and finally obtain a bio-based polyphosphazene flame retardant, recorded as PPZ-OA.

[0056] Its structural formula is formula (2):

[0057] Formula (2). Example 2

[0058] Compared with Example 1, the difference is that oleylamine is replaced by pentamethylenediamine.

[0059] The structural formula of the bio-based polyphosphazene flame retardant in this embodiment is shown in formula (3):

[0060] Formula (3). Example 3

[0061] Compared with Example 1, the difference is that oleylamine is replaced by glucosamine.

[0062] The structural formula of the bio-based polyphosphazene flame retardant in this embodiment is shown in formula (4):

[0063] Formula (4). Example 4

[0064] Compared with Example 1, the difference is that oleylamine is replaced by spermidine.

[0065] The structural formula of the bio-based polyphosphazene flame retardant in this embodiment is shown in formula (5):

[0066] Formula (5). Example 5

[0067] Compared with Example 1, the difference is that oleylamine is replaced by spermine.

[0068] The structural formula of the bio-based polyphosphazene flame retardant in this embodiment is shown in formula (6):

[0069] Formula (6).

[0070] Application Example 1

[0071] 50 parts of low-density polyethylene (LDPE), 50 parts of styrene-ethylene-butylene-styrene block copolymer (SEBS), and 0.3 parts of antioxidant 1010 were weighed and melt-blended at 190 °C and 60 r / min for 10 min, and then 30 parts of melamine cyanurate (MCA) and 5 parts of the bio-based polyphosphazene flame retardant (PPZ-OA) in Example 1 were added to the internal mixer and blended for 10 min under the same conditions. After the blending was completed, the mixed material was preheated at 190 °C for 5 min using a flat vulcanizer, and then hot-pressed at 30 MPa for 3 min and cold-pressed for 3 min to obtain a flame-retardant thermoplastic elastomer material, recorded as TPE / 30MCA / 5PPZ-OA.

[0072] The properties of the flame retardant thermoplastic elastomer material prepared are shown in Table 1.

[0073] Application Example 2

[0074] 50 parts of low-density polyethylene (LDPE), 50 parts of styrene-ethylene-butylene-styrene block copolymer (SEBS), and 0.3 parts of antioxidant 1010 were weighed and melt-blended at 190 °C and 60 r / min for 10 min, and then 25 parts of melamine cyanurate (MCA) and 10 parts of the bio-based polyphosphazene flame retardant (PPZ-OA) in Example 1 were added to the internal mixer and blended for 10 min under the same conditions. After the blending was completed, the mixed material was preheated at 190 °C for 5 min using a flat vulcanizer, and then hot-pressed at 30 MPa for 3 min and cold-pressed for 3 min to obtain a flame-retardant thermoplastic elastomer material, recorded as TPE / 25MCA / 10PPZ-OA.

[0075] The properties of the flame retardant thermoplastic elastomer material prepared are shown in Table 1.

[0076] Application Example 3

[0077] 50 parts of low-density polyethylene (LDPE), 50 parts of styrene-ethylene-butylene-styrene block copolymer (SEBS), and 0.3 parts of antioxidant 1010 were weighed and melt-blended at 190 °C and 60 r / min for 10 min, and then 15 parts of melamine cyanurate (MCA) and 15 parts of the bio-based polyphosphazene flame retardant (PPZ-OA) in Example 1 were added to the internal mixer and blended for 10 min under the same conditions. After the blending was completed, the mixed material was preheated at 190 °C for 5 min using a flat vulcanizer, and then hot-pressed at 30 MPa for 3 min and cold-pressed for 3 min to obtain a flame-retardant thermoplastic elastomer material, recorded as TPE / 15MCA / 15PPZ-OA.

[0078] The properties of the flame retardant thermoplastic elastomer material prepared are shown in Table 1.

[0079] Application Example 4

[0080] 50 parts of low-density polyethylene (LDPE), 50 parts of styrene-ethylene-butylene-styrene block copolymer (SEBS), and 0.3 parts of antioxidant 1010 were weighed and melt-blended at 190 °C and 60 r / min for 10 min, and then 10 parts of melamine cyanurate (MCA) and 4 parts of the bio-based polyphosphazene flame retardant (PPZ-OA) in Example 1 were added to the internal mixer and blended for 10 min under the same conditions. After the blending was completed, the mixed material was preheated at 190 °C for 5 min using a flat vulcanizer, and then hot-pressed at 30 MPa for 3 min and cold-pressed for 3 min to obtain a flame-retardant thermoplastic elastomer material, recorded as TPE / 10MCA / 4PPZ-OA.

[0081] The properties of the flame retardant thermoplastic elastomer material prepared are shown in Table 1.

[0082] Application Example 5

[0083] 50 parts of low-density polyethylene (LDPE), 50 parts of styrene-ethylene-butylene-styrene block copolymer (SEBS), and 0.3 parts of antioxidant 1010 were weighed and melt-blended at 190 °C and 60 r / min for 10 min, and then 15 parts of the bio-based polyphosphazene flame retardant (PPZ-OA) in Example 1 were added to the internal mixer and blended for 10 min under the same conditions. After the blending was completed, the mixed material was preheated at 190 °C for 5 min using a flat vulcanizer, and then hot-pressed at 30 MPa for 3 min and cold-pressed for 3 min to obtain a flame-retardant thermoplastic elastomer material, which was recorded as TPE / 15PPZ-OA.

[0084] The properties of the flame retardant thermoplastic elastomer material prepared are shown in Table 1.

[0085] Application Comparative Example 1

[0086] 50 parts of low-density polyethylene (LDPE), 50 parts of styrene-ethylene-butylene-styrene block copolymer (SEBS), and 0.3 parts of antioxidant 1010 were weighed and melt-blended at 190 °C and 60 r / min for 20 minutes. After the blending, the mixed material was preheated at 190 °C for 5 minutes using a flat vulcanizer, and then hot-pressed at 30 MPa for 3 minutes and cold-pressed for 3 minutes to obtain a thermoplastic elastomer material, which was recorded as TPE.

[0087] The properties of the flame retardant thermoplastic elastomer material prepared are shown in Table 1.

[0088] Application Comparative Example 2

[0089] 50 parts of low-density polyethylene (LDPE), 50 parts of styrene-ethylene-butylene-styrene block copolymer (SEBS), and 0.3 parts of antioxidant 1010 were weighed and melt-blended at 190 °C and 60 r / min for 10 min, and then 35 parts of melamine cyanurate (MCA) were added to the internal mixer and blended for 10 min under the same conditions. After the blending was completed, the mixed material was preheated at 190 °C for 5 min using a flat vulcanizer, and then hot-pressed at 30 MPa for 3 min and cold-pressed for 3 min to obtain a flame-retardant thermoplastic elastomer material, recorded as TPE / 35MCA.

[0090] The properties of the flame retardant thermoplastic elastomer material prepared are shown in Table 1.

[0091] Table 1. Performance data of flame retardant thermoplastic elastomer materials

[0092]

[0093] According to the above table, the flame-retardant thermoplastic elastomer material to which the bio-based polyphosphazene flame retardant is added in the present invention can achieve a good flame retardant effect; the flame-retardant thermoplastic elastomer material obtained by compounding the bio-based polyphosphazene flame retardant and melamine cyanurate in the present invention has a better flame retardant effect and better mechanical properties.

[0094] The bio-based polyphosphazene flame retardants prepared in Examples 1 to 5 of the present invention can all achieve good flame retardant effects, and after being compounded with melamine cyanurate, the thermoplastic elastomer material can achieve both flame retardancy and good mechanical properties.

[0095] In Application Example 2, when the total amount of flame retardant is 35 parts and the mass ratio of MCA to PPZ-OA is 2.5:1, the peak heat release rate (pHRR) and total release rate (THR) are the lowest, the limiting oxygen index (LOI) reaches 22.5%, and the char residual is 4.2wt%.

[0096] The thermogravimetric curves of application examples 1, 2, and 5 and comparative examples 1 and 2 are as follows: Figure 2 As shown in Figure 2, it can be seen that both MCA and PPZ-OA can reduce the initial decomposition temperature of TPE (T 5% ), but with the increase of PPZ-OA addition, the maximum thermal decomposition temperature (T max ) and residual carbon (RC) will increase significantly, indicating that PPZ-OA can improve the thermal stability of TPE materials by increasing the carbonization amount of the material at high temperature.

[0097] Compared with the flame retardant thermoplastic elastomer material to which only melamine cyanurate (MCA) is added, the flame retardant thermoplastic elastomer material to which only bio-based polyphosphazene flame retardant (PPZ-OA) is added has an increased elongation at break and a reduced elastic modulus, indicating that the bio-based polyphosphazene flame retardant of the present invention has a good toughening effect, can avoid the problem of increased rigidity of cable materials caused by the addition of MCA alone, and the cable material remains soft.

[0098] Within a certain range, as the addition amount of bio-based polyphosphazene flame retardant PPZ-OA increases, the elastic modulus decreases and the elongation at break increases.

[0099] The total amount of bio-based polyphosphazene flame retardant (PPZ-OA) and melamine cyanurate (MCA) added remains unchanged, the proportion of bio-based polyphosphazene flame retardant in the two increases, the elastic modulus decreases, and the elongation at break increases.

[0100] Within a certain range, when the proportion of bio-based polyphosphazene flame retardant (PPZ-OA) and melamine cyanurate (MCA) remains unchanged as a composite flame retardant, the total amount of the composite flame retardant added increases, the elastic modulus decreases, and the elongation at break decreases.

[0101] In summary, the bio-based polyphosphazene flame retardant of the present invention has a bio-based amine long chain, which is mainly an aliphatic chain segment and has good flexibility, so it can give the matrix a certain toughness; and the bio-based polyphosphazene flame retardant has an amino group, which can also produce non-flammable gases such as ammonia and nitrogen after thermal decomposition, which helps to dilute the oxygen concentration and reduce the risk of fire; the bio-based polyphosphazene flame retardant is used for flame-retardant cable materials, which can achieve a flame retardant effect and make it have good mechanical properties.

[0102] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A bio-based polyphosphazene flame retardant, It is characterized in that Its structural formula is shown in the following formula (2): Formula (2).

2. A method for preparing the bio-based polyphosphazene flame retardant according to claim 1, It is characterized in that The preparation method comprises: (1) In an inert atmosphere, hexachlorocyclotriphosphazene and tetrahydrofuran are mixed to obtain a mixed solution A, which is then placed in an ice water bath and stirred to dissolve; (2) mixing the bio-based amine and tetrahydrofuran to obtain a mixed solution B; (3) Adding the mixed solution B dropwise into the mixed solution A, and continuing the reaction in an ice water bath for 1 to 12 hours; after the reaction is complete, the mixture is separated, rotary evaporated, and dried to obtain a bio-based polyphosphazene flame retardant; the bio-based amine is oleylamine.

3. The method for preparing the bio-based polyphosphazene flame retardant according to claim 2, It is characterized in that The molar ratio of the hexachlorocyclotriphosphazene to the bio-based amine is 1:(3-12).

4. The method for preparing the bio-based polyphosphazene flame retardant according to claim 2, It is characterized in that The mass volume ratio of the bio-based amine and tetrahydrofuran in (2) is (20-50) g:50 ml.

5. A flame retardant cable material, It is characterized in that The invention comprises 1 to 50 wt % of the bio-based polyphosphazene flame retardant according to claim 1.

6. The flame retardant cable material according to claim 5, It is characterized in that It comprises 1-50wt% of a compound flame retardant; the compound flame retardant is composed of the bio-based polyphosphazene flame retardant according to claim 1 and melamine cyanurate in a mass ratio of 1:(1-5).

7. A method for preparing a flame retardant cable material, It is characterized in that The preparation method comprises: placing low-density polyethylene, styrene-ethylene-butylene-styrene block copolymer and antioxidant in an internal mixer for melt blending; adding 0-30wt% melamine cyanurate and 1-20wt% of the bio-based polyphosphazene flame retardant as claimed in claim 1 and continuing to blend evenly; and then placing in a flat vulcanizer for preheating, hot pressing and cold pressing to obtain the product.

8. The method for preparing the flame-retardant cable material according to claim 7, It is characterized in that The mass ratio of low-density polyethylene, styrene-ethylene-butylene-styrene block copolymer and antioxidant is (100~300):(100~300):

1.

9. The method for preparing the flame-retardant cable material according to claim 7, It is characterized in that The melt blending temperature is 150~220°C, the rotation speed is 10~100r / min, and the time is 5~60min.

10. The method for preparing the flame-retardant cable material according to claim 7, It is characterized in that The preheating temperature in the flat vulcanizer is 150~220℃.

11. The method for preparing a flame retardant cable material according to claim 7, It is characterized in that The hot pressing pressure is 10~50Mpa, the time is 1~30min, and the temperature is 180~210℃.

12. The method for preparing a flame retardant cable material according to claim 7, It is characterized in that The cold pressing pressure is 10~50Mpa, the time is 1~30min, and the temperature is 15~25℃.