A flame retardant low dielectric polyolefin elastomer for Ethernet
By adding ZIF-8 nano flame retardant material modified with phosphorus nitrogen groups into polyolefin materials, the problem of balancing flame retardancy and dielectric constant of polyolefin materials is solved, and the high flame retardant performance of Ethernet cables is achieved. and low dielectric properties, improving the overall performance of the material.
Patent Information
- Application Number
- CN202411073796.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-07
AI Technical Summary
Existing polyolefin materials have deficiencies in flame retardancy, which makes it difficult to balance high dielectric constant and low flame retardancy, affecting their application in Ethernet cables.
ZIF-8 nano flame retardant material modified with 0.5~10wt% phosphorus and nitrogen groups is used to form phosphorus and nitrogen bonds by reacting with ethylenediamine and phosphorous acid to enhance the flame retardant properties of the material while reducing its dielectric constant. Flame retardant low dielectric polyolefin elastomer for Ethernet.
The flame retardant properties of the polyolefin elastomer for Ethernet are improved, while its dielectric constant is reduced, the oxygen index and dielectric loss performance of the material are improved, and the dual requirements of low dielectric and high flame retardancy are met.
Smart Images

Figure CN118599136B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flame-retardant low-dielectric materials and relates to a flame-retardant low-dielectric polyolefin elastomer for Ethernet. Background Art
[0002] With the advent of the digital age, network communication has become an indispensable part of modern life and work. As a mainstream LAN technology, the performance and stability of Ethernet are crucial to achieving efficient data communication. When building an Ethernet network, it is crucial to choose the right cable. Low-dielectric cables are favored because of their low dielectric constant. Dielectric constant is a physical quantity that measures the effect of a material on an electromagnetic field. A low dielectric constant means that the signal transmission in the cable is less attenuated and distorted. This feature makes low-dielectric cables an ideal choice for high-speed data transmission. With low-dielectric cables, Ethernet networks can support higher data transmission rates, such as Gigabit Ethernet and even higher standards. This is essential to meet the needs of modern networks for fast and stable data transmission, especially in scenarios with high network performance requirements such as enterprises, educational institutions, and data centers.
[0003] Polyolefin elastomer has significant advantages as a material for low-dielectric cables. Its low dielectric constant minimizes attenuation and distortion during signal transmission, thereby improving the quality and rate of data transmission. At the same time, its high elasticity and softness make the manufactured cables have good flexibility and durability, and perform well in complex network wiring environments. In addition, the material has excellent heat resistance and chemical resistance, and can work stably in different temperature and chemical environments. In terms of cost, it is more economical than other materials, making cables based on it more competitive in the market. However, it is limited by its poor flame retardant effect.
[0004] To overcome this limitation, modifying polyolefins is a common method. Modification can be achieved by adding flame retardants, fillers or other modifiers to polyolefins to improve their flame retardant properties. For example, the addition of flame retardants can release inert gases or form a char layer when the material burns, thereby preventing the spread of flames. The addition of fillers can improve the thermal conductivity of the material and form a physical isolation layer to slow down the spread of flames. When flame retardants are added to a polymer matrix, they interact with the matrix and occupy the voids, thereby increasing the overall dielectric constant of the material. This effect is called the filling effect. The filling effect can cause a significant increase in the dielectric constant of the material, especially when the filler content is high. Therefore, it is necessary to propose a flame retardant material that can simultaneously meet the requirements of flame retardancy and low dielectric constant and a polyolefin elastomer containing the flame retardant material. Summary of the invention
[0005] The purpose of the present invention is to address the above-mentioned problems existing in the prior art and to propose a flame-retardant low-dielectric polyolefin elastomer for Ethernet, which is added with 0.5-10wt% of ZIF-8 nano flame-retardant material modified with phosphorus and nitrogen groups. The flame-retardant low-dielectric polyolefin elastomer for Ethernet achieves flame retardancy while reducing the dielectric constant.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A flame retardant low dielectric polyolefin elastomer for Ethernet, comprising 0.5-10wt% of phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material;
[0008] The phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material is prepared by reacting ZIF-8 with ethylenediamine to obtain amine-functionalized ZIF-8, and then heating the amine-functionalized ZIF-8 with a mixed solvent of formaldehyde and water and a phosphorous acid solution in sequence.
[0009] Preferably, the flame-retardant low-dielectric polyolefin elastomer for Ethernet includes 1-5 wt % of phosphorus-nitrogen group-modified ZIF-8 nano flame-retardant material.
[0010] Preferably, the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material has a cubic structure.
[0011] Preferably, the average size of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material is 200-500 nm.
[0012] Preferably, the method for preparing the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material comprises:
[0013] (1) dissolving 2-methylimidazole and zinc nitrate hexahydrate in solvents respectively and mixing them to obtain a mixed solution, and then subjecting the mixed solution to a first heating reaction and centrifugal washing to obtain ZIF-8;
[0014] (2) Mixing ZIF-8 and ethylenediamine and subjecting them to a second heating reaction to obtain amine-functionalized ZIF-8;
[0015] (3) The amine-functionalized ZIF-8 is mixed with a mixed solvent of formaldehyde and water and subjected to a third heating reaction; a phosphorous acid solution is then added, and a fourth heating reaction is performed and vacuum rotary evaporation is performed to obtain a phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material.
[0016] Preferably, the mass ratio of 2-methylimidazole to zinc nitrate hexahydrate in (1) is 1:(1-10).
[0017] Preferably, the solvent in (1) is one or more of methanol, ethanol and water.
[0018] Preferably, the mass volume ratio of the total mass of 2-methylimidazole and zinc nitrate hexahydrate to the solvent in the mixed solution (1) is (20-50) g: (50-200) ml.
[0019] Preferably, the first heating reaction temperature in (1) is 30-60° C. and the time is 10-60 min.
[0020] Preferably, the centrifugal washing speed in (1) is 7000-12000 rpm, and the washing time is 1-40 min.
[0021] Preferably, the mass volume ratio of ZIF-8 and ethylenediamine in (2) is (5-12) g: (80-200) ml.
[0022] Preferably, the second heating reaction temperature in (2) is 90-150° C. and the time is 12-48 h.
[0023] Preferably, the mass volume ratio of amine-functionalized ZIF-8 and mixed solvent in (3) is (5-12) g: (20-80) ml.
[0024] Preferably, the mass ratio of amine-functionalized ZIF-8 to formaldehyde in (3) is 1:(0.8-5).
[0025] (3) Excessive formaldehyde may lead to the formation of formaldehyde polymers or other unwanted organic byproducts; insufficient formaldehyde may cause the amine groups on the surface of ZIF-8 to fail to react fully and form sufficient phosphorus and nitrogen groups, thereby affecting the performance of the material.
[0026] Preferably, the concentration of the phosphorous acid solution in (3) is 0.1-1.6 g / mL.
[0027] Preferably, the mass ratio of the amine-functionalized ZIF-8 to the phosphorous acid in the phosphorous acid solution in (3) is 1:(0.5-10).
[0028] Preferably, the third heating reaction temperature in (3) is 30-50°C and the time is 30-90 min.
[0029] Preferably, the fourth heating reaction temperature in (3) is 40-90° C. and the time is 8-24 h.
[0030] Preferably, the flame-retardant low-dielectric polyolefin elastomer for Ethernet includes 2 wt % of ZIF-8 nano flame-retardant material modified with phosphorus and nitrogen groups.
[0031] More preferably, the dielectric constant of the flame-retardant low-dielectric polyolefin elastomer for Ethernet is as low as 2.17, the dielectric loss is lower than 0.050, and the oxygen index is 26.5%.
[0032] A method for preparing a flame-retardant low-dielectric polyolefin elastomer for Ethernet, comprising:
[0033] (1) Mixing polyolefin elastomer SEBS, phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material and organic solvent to obtain a pre-curing solution;
[0034] (2) After the pre-curing solution is poured, it is dried and cured to obtain a flame-retardant low-dielectric polyolefin elastomer for Ethernet.
[0035] Preferably, the amount of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material added in (1) is 0.5-10 wt % of the mass of the polyolefin elastomer SEBS.
[0036] Further preferably, the amount of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material added in (1) is 1-5 wt % of the mass of the polyolefin elastomer SEBS.
[0037] More preferably, the amount of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material added in (1) is 2 wt % of the mass of the polyolefin elastomer SEBS.
[0038] Preferably, the organic solvent in (1) includes one or more of formaldehyde, acetaldehyde, acetone, methanol, ethanol, toluene, xylene, and isopropanol.
[0039] Preferably, in (1), the stirring speed is 1500-3000 rpm, the stirring temperature is 15-35° C., and the stirring time is 1-10 h.
[0040] Preferably, the concentration of the polyolefin elastomer SEBS in the pre-curing solution in (1) is 0.1-0.5 g / mL.
[0041] Preferably, the drying and curing temperature in (2) is 60-100°C and the drying and curing time is 1-30h.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] 1. The present invention adds 0.5-5wt% of phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material to the raw material formula of flame retardant low-dielectric polyolefin elastomer for Ethernet, thereby giving it a flame retardant effect and reducing the dielectric constant of polyolefin elastomer SEBS;
[0044] 2. In the preparation process of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material of the present invention, ZIF-8 is first reacted with ethylenediamine to obtain amine-functionalized ZIF-8. The amine group on the amine-functionalized ZIF-8 is a functional group with high reactivity. The present invention introduces an amine group into ZIF-8 to increase the chemical activity of ZIF-8, so that phosphorous acid reacts with the amine group to form a phosphorus-nitrogen bond.
[0045] 3. In the preparation process of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material of the present invention, amine-functionalized ZIF-8, a mixed solvent of formaldehyde and water, and a phosphorous acid solution are heated and reacted in sequence; compared with other phosphorus compounds, the phosphorous acid selected in the present invention has the following advantages: first, phosphorous acid is a strong reducing agent with high reactivity, and can more easily react with the amino group on the surface of amine-functionalized ZIF-8 to form a stable phosphorus-nitrogen bond; second, phosphorous acid can usually react with amine compounds under mild conditions, which may mean that effective phosphorus-nitrogen group modification can be carried out at a lower temperature, thereby reducing damage to the ZIF-8 structure; thirdly, phosphorous acid has good solubility in water, which allows it to react with amine-functionalized ZIF-8 in an aqueous medium, which is beneficial to the uniformity of surface modification; finally, phosphorous acid molecules are small and can more easily enter the pores of ZIF-8 for surface modification, thereby increasing the loading capacity, while macromolecules such as polyphosphates are difficult to enter these microporous structures;
[0046] 4. The present invention modifies phosphorus-nitrogen groups on the surface of ZIF-8 nano flame retardant material to achieve flame retardancy while reducing the dielectric constant of polyolefin elastomer material. The porous material ZIF-8 contains a large number of pores filled with low dielectric air (dielectric constant = 1) medium. The air medium replaces part of the solid material with high dielectric constant, so that the overall polarization degree is reduced;
[0047] 5. The phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material of the present invention can also be applied to other resin materials and can also achieve excellent flame retardant effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is the XRD spectrum of the ZIF-8 nano flame retardant material modified with phosphorus and nitrogen groups in Example 1 of the present invention.
[0049] Figure 2 TEM image and EDS analysis of the ZIF-8 nano flame retardant material modified with phosphorus and nitrogen groups in Example 1 of the present invention.
[0050] Figure 3 This is a graph showing the variation of the dielectric constant and dielectric loss of the flame-retardant low-dielectric polyolefin elastomer for Ethernet with frequency in Application Examples 1 to 4 and Application Comparative Example 1 of the present invention.
[0051] Figure 4 It is the oxygen index of the flame retardant low dielectric polyolefin elastomer for Ethernet when the addition amount of the ZIF-8 nano flame retardant material modified with different phosphorus and nitrogen groups in Application Examples 1 to 4 and Application Comparative Example 1 of the present invention is used. DETAILED DESCRIPTION
[0052] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.
[0053] Unless otherwise specified, the materials used in the present invention are conventional commercial products, and the methods used are conventional technical means.
[0054] Test 1: X-ray diffraction (XRD) test: The test was performed using a D8 ADVANCE XRD tester from Bruker, Germany, with a scanning range of 5-35°.
[0055] Test 2: High-resolution transmission electron microscopy (TEM) images and EDS surface element analysis: High-resolution transmission electron microscopy images were captured using a FEITecnai F20 at an accelerating voltage of 250 kV, and surface element distribution was measured by EDS.
[0056] Test 3: Dielectric performance test: Use a broadband dielectric impedance analyzer to test the dielectric properties of the sample; the test is carried out at room temperature and the test frequency range is set to 100~10 6 Hz.
[0057] Test 4: Oxygen Index (LOI) Test: In the oxygen index tester, the volume fraction of the minimum oxygen concentration required for the test sample to maintain stable combustion. Clamp the sample vertically on the iron clamp and then ignite it; adjust the ratio of oxygen and nitrogen, start timing when the sample can burn, and observe the burning distance of the sample after 3 minutes; reduce the oxygen concentration when it exceeds the mark, and increase the oxygen concentration when it does not reach the mark. The oxygen content when it reaches the mark in 3 minutes is the oxygen index of the composite material.
[0058] Example 1
[0059] (1) 8.2 g of 2-methylimidazole and 29.7 g of zinc nitrate hexahydrate were dissolved in 50 mL of methanol and stirred for 10 minutes to obtain a mixed solution. The mixed solution was subjected to a first heating reaction and heated to 40° C. for 30 minutes, and then centrifuged at 9000 rpm for 20 minutes. The precipitate was collected, washed with methanol three times, and dried at 60° C. for 12 hours to obtain ZIF-8;
[0060] (2) Add 10 g ZIF-8 to 100 mL ethylenediamine solution, mix well and place in an oven for a second heating reaction, perform solvent thermal treatment at 110 °C for 24 hours, react and cool, wash the product with deionized water and methanol solution three times, and dry at 60 °C for 24 hours to obtain amine-functionalized ZIF-8;
[0061] (3) 10 g of amine-functionalized ZIF-8 was mixed with 10 ml of formaldehyde and 30 mL of deionized water and placed in a three-necked flask with a reflux condenser for a third heating reaction, and the mixture was stirred at 50 °C for 1 hour; 10 g of phosphorous acid was dissolved in 20 mL of deionized water to obtain a phosphorous acid solution (0.5 g / ml), which was then added dropwise to the three-necked flask while being vigorously stirred; a fourth heating reaction was then carried out, and the mixture was reacted at 70 °C for 12 hours; after the reaction was complete, the solvent and unreacted formaldehyde were removed by reduced pressure rotary evaporation to obtain a phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material, which was recorded as N\P-ZIF-8.
[0062] Figure 1 This is the XRD spectrum of the ZIF-8 nano flame retardant material modified with phosphorus and nitrogen groups in this embodiment; it can be seen that the characteristic peaks are located at 7.16°, 10.18°, 12.54° and 17.86°, corresponding to the (011), (002), (112) and (222) crystal planes respectively; that is, it is a cubic crystal system.
[0063] Figure 2 The TEM image and EDS analysis of the ZIF-8 nano flame retardant material modified by phosphorus and nitrogen groups in this embodiment show that the ZIF-8 nano flame retardant material modified by phosphorus and nitrogen groups has a cubic structure, and phosphorus and nitrogen elements are evenly distributed on its surface.
[0064] Example 2
[0065] (1) 8.2 g of 2-methylimidazole and 29.7 g of zinc nitrate hexahydrate were dissolved in 50 mL of methanol and stirred for 10 minutes to obtain a mixed solution. The mixed solution was subjected to a first heating reaction and heated to 35° C. for 30 minutes, and then centrifuged at 8000 rpm for 20 minutes. The precipitate was collected, washed with methanol three times, and dried at 60° C. for 12 hours to obtain ZIF-8;
[0066] (2) 8 g ZIF-8 was added to 100 mL ethylenediamine solution, mixed and placed in an oven for a second heating reaction, and solvent thermal treatment was performed at 130 °C for 24 hours. After reaction and cooling, the product was washed three times with deionized water and methanol solution, and dried at 60 °C for 24 hours to obtain amine-functionalized ZIF-8;
[0067] (3) 8 g of amine-functionalized ZIF-8 was mixed with 8 ml of formaldehyde and 30 mL of deionized water and placed in a three-necked flask with a reflux condenser for a third heating reaction, and the mixture was stirred at 50 °C for 1 hour; 15 g of phosphorous acid was dissolved in 20 mL of deionized water to obtain a phosphorous acid solution (0.75 g / ml), which was then added dropwise to the three-necked flask while being vigorously stirred; a fourth heating reaction was then carried out, and the mixture was reacted at 80 °C for 12 hours; after the reaction was complete, the solvent and unreacted formaldehyde were removed by reduced pressure rotary evaporation to obtain a phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material, which was recorded as N\P-ZIF-8'.
[0068] Comparative Example 1
[0069] Compared with Example 1, the difference is that phosphorous acid, ethylenediamine, formaldehyde solution and water are mixed to perform Mannheim reaction and then reacted with ZIF-8.
[0070] Comparative Example 2
[0071] Compared with Example 1, the difference is that triethyl phosphate is used to replace phosphorous acid.
[0072] Comparative Example 3
[0073] Compared with Example 1, the difference is that the mass ratio of amine-functionalized ZIF-8 to formaldehyde in (3) is 1:0.5.
[0074] Application Example 1
[0075] (1) 5 g of SEBS and 0.025 g of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material (0.5 wt%) in Example 1 were placed in a glass bottle, 15 mL of toluene was added, and the bottle was placed on a magnetic stirrer and stirred for 4 h to uniformly dissolve the SEBS in the solution to obtain a pre-cured solution;
[0076] (2) The pre-cured solution was cast into a polytetrafluoroethylene mold with a size of 80 mm*10 mm*4 mm, and then the cast sample was placed in an oven at 80 °C for curing for 6 h to obtain a flame-retardant low-dielectric polyolefin elastomer sample for Ethernet, which was recorded as SEBS-0.5N\P-ZIF-8.
[0077] The flame retardant low dielectric polyolefin elastomer sample SEBS-0.5N\P-ZIF-8 for Ethernet was tested.
[0078] The dielectric constant of SEBS-0.5N\P-ZIF-8 is 2.58, and the dielectric loss is below 0.040; the oxygen index of SEBS-0.5N\P-ZIF-8 is 20.8%.
[0079] Application Example 2
[0080] (1) 5 g of SEBS and 0.05 g of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material (1 wt%) in Example 1 were placed in a glass bottle, 15 mL of toluene was added, and the bottle was placed on a magnetic stirrer and stirred for 4 h to uniformly dissolve the SEBS in the solution to obtain a pre-cured solution;
[0081] (2) The pre-cured solution was cast into a polytetrafluoroethylene mold with a size of 80 mm*10 mm*4 mm, and then the cast sample was placed in an oven at 80°C for curing for 6 h to obtain a flame-retardant low-dielectric polyolefin elastomer sample for Ethernet, which was recorded as SEBS-1N\P-ZIF-8.
[0082] The flame retardant low dielectric polyolefin elastomer sample SEBS-1N\P-ZIF-8 for Ethernet was tested.
[0083] The dielectric constant of SEBS-1N\P-ZIF-8 is 2.30, and the dielectric loss is below 0.035; the oxygen index of SEBS-1N\P-ZIF-8 is 25.2%.
[0084] Application Example 3
[0085] (1) 5 g of SEBS and 0.1 g of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material (2 wt%) in Example 1 were placed in a glass bottle, 15 mL of toluene was added, and the bottle was placed on a magnetic stirrer and stirred for 4 h to uniformly dissolve the SEBS in the solution to obtain a pre-cured solution;
[0086] (2) The pre-cured solution was cast into a polytetrafluoroethylene mold with a size of 80 mm*10 mm*4 mm, and then the cast sample was placed in an oven at 80°C for curing for 6 h to obtain a flame-retardant low-dielectric polyolefin elastomer sample for Ethernet, which was recorded as SEBS-2N\P-ZIF-8.
[0087] The flame retardant low dielectric polyolefin elastomer sample SEBS-2N\P-ZIF-8 for Ethernet was tested.
[0088] The dielectric constant of SEBS-2N\P-ZIF-8 is 2.17, and the dielectric loss is below 0.032; the oxygen index of SEBS-2N\P-ZIF-8 is 26.5%.
[0089] Application Example 4
[0090] (1) 5 g of SEBS and 0.25 g of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material (5 wt%) in Example 1 were placed in a glass bottle, 15 mL of toluene was added, and the bottle was placed on a magnetic stirrer and stirred for 4 h to uniformly dissolve the SEBS in the solution to obtain a pre-cured solution;
[0091] (2) The pre-cured solution was cast into a polytetrafluoroethylene mold with a size of 80 mm*10 mm*4 mm, and then the cast sample was placed in an oven at 80°C for curing for 6 hours to obtain a flame-retardant low-dielectric polyolefin elastomer sample for Ethernet, which was recorded as SEBS-5N\P-ZIF-8.
[0092] The flame retardant low dielectric polyolefin elastomer sample SEBS-5N\P-ZIF-8 for Ethernet was tested.
[0093] The dielectric constant of SEBS-5N\P-ZIF-8 is 2.40, and the dielectric loss is below 0.050; the oxygen index of SEBS-5N\P-ZIF-8 is 28%.
[0094] Application Example 5
[0095] (1) 5 g of SEBS and 0.5 g of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material (10 wt%) in Example 1 were placed in a glass bottle, 15 mL of toluene was added, and the bottle was placed on a magnetic stirrer and stirred for 4 h to uniformly dissolve the SEBS in the solution to obtain a pre-cured solution;
[0096] (2) The pre-cured solution was cast into a polytetrafluoroethylene mold with a size of 80 mm*10 mm*4 mm, and then the cast sample was placed in an oven at 80°C for curing for 6 h to obtain a flame-retardant low-dielectric polyolefin elastomer sample for Ethernet, which was recorded as SEBS-10N\P-ZIF-8.
[0097] The flame retardant low dielectric polyolefin elastomer sample SEBS-10N\P-ZIF-8 for Ethernet was tested.
[0098] The dielectric constant of SEBS-10N\P-ZIF-8 is 2.5, and the dielectric loss is below 0.05; the oxygen index of SEBS-10N\P-ZIF-8 is 31.0%.
[0099] Application Example 6
[0100] The phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material N\P-ZIF-8' in Example 2 was used in accordance with the method in Application Example 3 to prepare a flame retardant low dielectric polyolefin elastomer sample SEBS-2N\P-ZIF-8' for Ethernet.
[0101] The dielectric constant of SEBS-2N\P-ZIF-8' is 2.15, and the dielectric loss is below 0.030; the oxygen index of SEBS-2N\P-ZIF-8' is 24%.
[0102] Application Comparative Example 1
[0103] (1) Take 5 g of SEBS and put it into a glass bottle, add 15 mL of toluene and place it on a magnetic stirrer and stir for 4 h to make SEBS evenly dissolved in the solution to obtain a pre-curing solution of SEBS elastomer;
[0104] (2) The pre-curing solution was cast into a polytetrafluoroethylene mold with a size of 80 mm*10 mm*4 mm, and then the cast sample was placed in an oven at 80°C for curing for 6 h to obtain a polyolefin elastomer sample, which was recorded as SEBS-0.
[0105] The polyolefin elastomer sample SEBS-0 was tested.
[0106] The dielectric constant of SEBS-0 is 2.97, and the dielectric loss is below 0.015; the oxygen index of SEBS-0 is 17.8%, which proves that its flame retardant effect is poor.
[0107] Application Comparative Examples 2~4
[0108] The phosphorus-nitrogen group-modified ZIF-8 nano flame retardant materials in Comparative Examples 1 to 3 were used in accordance with the method in Application Example 3 to prepare flame retardant low dielectric polyolefin elastomer samples for Ethernet.
[0109] The dielectric constant of the flame-retardant low-dielectric polyolefin elastomer sample for Ethernet in Application Comparative Example 2 is 2.61, the dielectric loss is below 0.040, and the oxygen index is 18.5%.
[0110] The dielectric constant of the flame-retardant low-dielectric polyolefin elastomer sample for Ethernet in Application Comparative Example 3 is 2.40, the dielectric loss is below 0.038, and the oxygen index is 21.1%.
[0111] The dielectric constant of the flame-retardant low-dielectric polyolefin elastomer sample for Ethernet in Application Comparative Example 4 is 2.20, the dielectric loss is below 0.030, and the oxygen index is 22.5%.
[0112] Figure 3 The dielectric constant and dielectric loss of the flame-retardant low-dielectric polyolefin elastomer for Ethernet in Application Examples 1 to 4 and Application Comparative Example 1 vary with frequency; it can be seen that the dielectric constant is lowest, which is 2.17, when the addition amount of the ZIF-8 nano flame retardant material modified by the phosphorus and nitrogen groups is 2wt%; and the dielectric constants in Application Examples 1 to 4 are all lower than the dielectric constant when the ZIF-8 nano flame retardant material modified by the phosphorus and nitrogen groups is not added in Application Comparative Example 1; in addition, the dielectric losses of Application Examples 1 to 4 are all maintained below 0.050.
[0113] Figure 4The oxygen index of the flame-retardant low-dielectric polyolefin elastomer for Ethernet when the addition amount of the ZIF-8 nano flame-retardant material modified with different phosphorus and nitrogen groups in Examples 1 to 4 and Comparative Example 1 is applied; it can be seen that within a certain range, as the addition amount of the ZIF-8 nano flame-retardant material modified with phosphorus and nitrogen groups increases, the dielectric constant of the flame-retardant low-dielectric polyolefin elastomer for Ethernet first decreases and then increases;
[0114] Within a certain range, the oxygen index increases with the increase in the addition amount of ZIF-8 nano flame retardant material modified with phosphorus and nitrogen groups.
[0115] In summary, the present invention adds phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material into polyolefin elastomer, and the flame retardant low-dielectric polyolefin elastomer for Ethernet prepared has excellent flame retardant properties and reduces the dielectric constant of the material.
[0116] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. A flame retardant low dielectric polyolefin elastomer for Ethernet, characterized in that: It includes 0.5-10wt% of phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material; The preparation method of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material comprises: (1) dissolving 2-methylimidazole and zinc nitrate hexahydrate in solvents respectively and mixing them to obtain a mixed solution, and then subjecting the mixed solution to a first heating reaction and centrifugal washing to obtain ZIF-8; (2) Mixing ZIF-8 and ethylenediamine and subjecting them to a second heating reaction to obtain amine-functionalized ZIF-8; (3) The amine-functionalized ZIF-8 is mixed with a mixed solvent of formaldehyde and water and subjected to a third heating reaction, wherein the mass volume ratio of the amine-functionalized ZIF-8 to formaldehyde is 1 g: (0.8-5) ml; phosphorous acid solution is then added, and a fourth heating reaction and reduced pressure rotary evaporation are performed to obtain a phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material.
2. The flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 1, characterized in that: The average size of the phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material is 200-500 nm.
3. The flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 1, characterized in that: The mass volume ratio of the total mass of 2-methylimidazole and zinc nitrate hexahydrate to the solvent in the mixed solution (1) is (20-50) g: (50-200) ml.
4. The flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 1, characterized in that: The first heating reaction temperature in (1) is 30-60° C. and the time is 10-60 min.
5. The flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 1, characterized in that: The mass volume ratio of ZIF-8 and ethylenediamine in (2) is (5-12) g: (80-200) ml.
6. The flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 1, characterized in that: The second heating reaction temperature in (2) is 90-150° C. and the reaction time is 12-48 hours.
7. The flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 1, characterized in that: The mass volume ratio of the amine-functionalized ZIF-8 and the mixed solvent in (3) is (5-12) g: (20-80) ml.
8. The flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 1, characterized in that: The concentration of the phosphorous acid solution in (3) is 0.1-1.6 g / mL; the mass ratio of the amine-functionalized ZIF-8 to the phosphorous acid in the phosphorous acid solution in (3) is 1:(0.5-10).
9. The flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 1, characterized in that: The third heating reaction temperature in (3) is 30-60°C, and the time is 30-90 min; the fourth heating reaction temperature in (3) is 40-90°C, and the time is 8-24 h.
10. The flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 1, characterized in that: The flame-retardant low-dielectric polyolefin elastomer for Ethernet includes 1-5 wt % of phosphorus-nitrogen group-modified ZIF-8 nano flame-retardant material.
11. A method for preparing the flame-retardant low-dielectric polyolefin elastomer for Ethernet as claimed in claim 1, characterized in that: The preparation method comprises: (1) Mixing polyolefin elastomer SEBS, phosphorus-nitrogen group-modified ZIF-8 nano flame retardant material and organic solvent to obtain a pre-curing solution; (2) After the pre-curing solution is poured, it is dried and cured to obtain a flame-retardant low-dielectric polyolefin elastomer for Ethernet.
12. The method for preparing a flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 11, characterized in that: The concentration of the polyolefin elastomer SEBS in the pre-curing solution in (1) is 0.1-0.5 g / mL.
13. The method for preparing a flame-retardant low-dielectric polyolefin elastomer for Ethernet according to claim 11, characterized in that: The drying and curing temperature in (2) is 60-100° C. and the time is 1-30 hours.
Citation Information
Patent Citations
Flame-retardant polymer containing phosphorus and nitrogen and preparation method thereof
CN102391403A
Preparation method of phosphate or phosphite flame retardant with low acid value and high stability
CN105440071A