Aerogel with multi-oriented pores and preparation method and application thereof
By treating the fiber suspension at high speed shear and high supercooling, multi-oriented aerogel is prepared, which solves the problem of singleness in traditional aerogel channel structure, and achieves better performance and versatility. It is suitable for Lightweight high-strength composite materials, electrode materials, energy storage, wave absorption and wave-transmissive materials and other fields.
Patent Information
- Application Number
- CN202410806038.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-21
AI Technical Summary
The traditional aerogel's pore structure lacks a clear and consistent orientation, which limits its performance in fluid transmission, material adsorption and energy storage, and the single-oriented pore structure in the prior art cannot fully utilize its performance in complex application environments. Advantages.
Gas with multi-oriented mesh or anisotropic step pores are prepared by shearing the hydrophilic fiber material and hydrophobic fiber material into fiber suspensions in water and freeze-dried at high speed shear and high supercooling. gel.
It has achieved better performance of aerogel in matter transmission, energy storage and conversion, adsorption and separation, etc., broadened its application areas, and showed versatility and efficiency in different scenarios.
Smart Images

Figure CN118599175B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of aerogels, and relates to an aerogel with multi-oriented pores, a preparation method and an application thereof. Background Art
[0002] As a material with unique structure and properties, aerogel has shown broad application prospects and great research value in many fields. In-depth research on aerogel preparation technology, pore structure regulation, and performance optimization will not only help promote the progress of materials science, but also provide new solutions and breakthroughs in energy, environmental protection, biomedicine and other fields. Therefore, the research on aerogel has important practical significance and scientific value, and it is worth our continued investment of more energy and resources for in-depth exploration.
[0003] The pores of traditional aerogels are often disordered or short-range ordered, lacking a clear and consistent orientation. This pore structure limits the performance of aerogels in fluid transport, material adsorption, and energy storage. For example, in capacitive deionization technology, the disordered pore structure may hinder the migration of charged substances in the electrode, thereby affecting the adsorption rate and processing efficiency.
[0004] To solve the above problems, patent application CN109485906B discloses a highly oriented cellulose aerogel and a preparation method thereof, in which an aerogel with an oriented pore structure is prepared by a directional freezing method. However, the aerogel prepared by this method has a single pore orientation, which greatly limits its further application and development. This single oriented pore structure causes the aerogel to often fail to fully exert its performance advantages when facing complex and changeable actual application environments, and even shows obvious deficiencies in certain specific scenarios.
[0005] Therefore, in order to expand the application areas of aerogels and improve their performance, it is urgent to break the limitation of single pore orientation and develop new aerogel materials with more complex and diversified pore structures. Summary of the invention
[0006] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for preparing an aerogel with multi-oriented pores.
[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing an aerogel with multi-oriented pores, comprising dispersing a hydrophilic fiber material and a hydrophobic fiber material in water, shearing the fiber suspension with a shearing machine, freezing the fiber suspension until it is completely frozen, and freeze-drying the aerogel;
[0009] The multi-oriented channels are grid channels or anisotropic step channels; the water contact angle of the hydrophilic fiber material is 0°~20°, the shear stiffness is 10~20, and the aspect ratio is ≤10; the water contact angle of the hydrophobic fiber material is 130°~150°, the shear stiffness is 0.1~0.5, and the aspect ratio is ≥40; the mass ratio of the hydrophilic fiber material to the hydrophobic fiber material is ≥1; the shear rate of the shearing machine is 20000~25000rpm; the supercooling degree during freezing (supercooling degree is the difference between the theoretical crystallization temperature of the crystal and the actual given crystallization field temperature, and the magnitude of supercooling degree is closely related to the cooling rate. The faster the cooling rate, the lower the actual crystallization temperature and the greater the supercooling degree; conversely, the slower the cooling rate, the smaller the supercooling degree and the closer the actual crystallization temperature is to the theoretical crystallization temperature) is ≥5.5℃.
[0010] As the preferred technical solution:
[0011] In the method for preparing an aerogel with multi-oriented pores as described above, the aspect ratio of the hydrophilic fiber material is 1-10, and the aspect ratio of the hydrophobic fiber material is 40-80.
[0012] In the method for preparing an aerogel with multi-oriented pores as described above, the hydrophilic fiber material is cellulose fiber or cellulose derivative fiber (such as carboxymethyl cellulose fiber, hydroxypropyl cellulose fiber).
[0013] In the method for preparing an aerogel with multi-oriented pores as described above, the hydrophobic fiber material is thermoplastic polyurethane fiber, polylactic acid fiber or polycaprolactone fiber.
[0014] In the method for preparing an aerogel with multi-oriented pores as described above, the content of the hydrophilic fiber material in the fiber suspension is 0.5-0.75wt%.
[0015] In the method for preparing an aerogel with multi-oriented pores as described above, the fiber suspension also contains 0.25-2wt% of a surfactant, so that the surface energy can be adjusted, and the size of the pore structure can be controlled.
[0016] In the method for preparing an aerogel with multi-oriented pores as described above, freezing the fiber suspension until it is completely frozen means leaving the fiber suspension at -50 to -196°C for 0.2 to 8 hours.
[0017] The present invention also provides an aerogel with multi-oriented pores, which is prepared by using the preparation method of the aerogel with multi-oriented pores as described in any one of the above items.
[0018] The present invention also provides an application of the aerogel having multi-oriented pores as described above, which is used as a lightweight and high-strength composite material, an aerogel-based electrode material, an energy storage and conversion material, an absorbing and transmitting wave material, a fireproof and heat-insulating material for buildings, a sewage treatment and seawater desalination material, a one-way moisture-conducting material, microelectronics or a water-retaining agent;
[0019] When used as a lightweight and high-strength composite material, an aerogel-based electrode material, or an energy storage and conversion material, an aerogel with grid pores can be selected because the arrangement direction of such pores is orderly and the stability is good, which enables the material to disperse and transfer stress more effectively when subjected to external forces, thereby giving the material the characteristics of lightness and high strength, and can be applied to aerospace, automobile manufacturing and other fields; the grid pore structure can achieve a variety of pore size combinations from micropores to mesopores and even macropores, providing possibilities for material transport and chemical reactions at different scales, and can promote the rapid migration of ions in electrode materials, thereby improving the energy density and charge and discharge rate of the battery;
[0020] When used as wave-absorbing and wave-transmitting materials, building fireproof and heat-insulating materials, sewage treatment and seawater desalination materials, unidirectional moisture-conducting materials, microelectronics, and water-retaining agents, aerogels with anisotropic stepped pores can be selected. This is because the anisotropic stepped pore structure can be multifunctional by introducing different fillers or functional components, such as electrical conductivity, thermal conductivity, wave absorption, and wave transmission. Different oriented channels can respond to electromagnetic waves of different frequencies, thereby having a high absorption rate (wave absorption) for electromagnetic waves in a specific frequency band, and having good transmittance (wave transmission) for electromagnetic waves in other frequency bands, and can be used in the field of concealed camouflage and military defense; the anisotropic stepped pore structure is also used because it can simultaneously have heat insulation and flame retardancy. It is used in building materials and fireproof materials to provide additional safety protection. This structure can be used in sewage treatment and seawater desalination. The direction of the hydrophilic layer helps the adsorption and transmission of water molecules, while the direction of the hydrophobic layer can effectively block the penetration of pollutants and salts, providing higher molecular transmission efficiency and better selectivity, and helping to more effectively separate salt and other impurities. This structure can be used in the design of microfluidic chips. The hydrophilic layer helps the flow and mixing of liquids, while the hydrophobic layer can be used to separate different reaction zones to realize complex chemical reaction processes. In the agricultural field, this structure can be used to develop new water-retaining agents. The hydrophilic layer helps the absorption and retention of water, while the hydrophobic layer prevents the evaporation of water too quickly.
[0021] Principle of the invention:
[0022] Under high-speed shearing, the fiber material is distributed parallel or perpendicular to the Z axis. The hydrophilic fiber material with large shear stiffness is more hydrophilic, and the angle with the Z axis is closer to 0°. The hydrophobic fiber material with small shear stiffness is more hydrophobic, and the angle with the Z axis is closer to 90°. Under high supercooling, ice crystals grow perpendicular to the surface of the fiber material, thus forming columnar ice crystals. After freeze-drying, a grid of pores (such asFigure 1 In extreme cases, the highly hydrophobic fiber material with extremely low shear stiffness completely sinks to the bottom, and the extremely hydrophilic fiber material with large shear stiffness is dispersed on the top, which can form anisotropic stepped channels (such as Figure 2 shown).
[0023] Beneficial effects:
[0024] The preparation method of the aerogel with multi-oriented pores of the present invention is simple, and the aerogel with multi-oriented pores can show more excellent performance in material transmission, energy storage and conversion, adsorption and separation, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of aerogel with grid pores;
[0026] Figure 2 Schematic diagram of aerogel with anisotropic stepped pores;
[0027] Figure 3 This is a top view of the aerogel with grid pores of Example 1 (the lines in the figure represent the distribution of the grid pores);
[0028] Figure 4 This is a front view of the aerogel with anisotropic stepped pores of Example 2 (the lines in the figure represent the distribution of the anisotropic stepped pores). DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0030] Example 1
[0031] A method for preparing an aerogel with multi-oriented pores, the specific steps are as follows:
[0032] (1) Preparation of raw materials;
[0033] Hydrophilic fiber material: cellulose fiber, water contact angle of 10° to 20°, shear stiffness of 10 to 20, aspect ratio of 1 to 10;
[0034] Hydrophobic fiber material: polylactic acid fiber, water contact angle of 130° to 135°, shear stiffness of 0.1 to 0.5, aspect ratio of 40 to 80;
[0035] Surfactant: potassium lauryl ether phosphate, CAS number 58318-92-6;
[0036] water;
[0037] (2) The hydrophilic fiber material, the hydrophobic fiber material and the surfactant are dispersed in water, and the fiber suspension is obtained by shearing with a shearing machine (shear rate of 20000 rpm), and the fiber suspension is allowed to stand at -50 ° C (supercooling degree of 5.5 ° C) for 8 hours, and freeze-dried (temperature of -45 ° C, pressure of 15 Pa, time of 24 hours) to obtain an aerogel;
[0038] The mass ratio of the hydrophilic fiber material to the hydrophobic fiber material is 1; the content of the hydrophilic fiber material in the fiber suspension is 0.5wt%, and the content of the surfactant is 0.25wt%.
[0039] The aerogel with multi-oriented pores finally obtained is an aerogel with grid pores, such as Figure 3 As shown, it can be used as lightweight and high-strength composite materials, aerogel-based electrode materials, and energy storage and conversion materials.
[0040] Example 2
[0041] A method for preparing an aerogel with multi-oriented pores, the specific steps are as follows:
[0042] (1) Preparation of raw materials;
[0043] Hydrophilic fiber material: carboxymethyl cellulose fiber, water contact angle of 0° to 20°, shear stiffness of 10 to 20, aspect ratio of 2 to 10;
[0044] Hydrophobic fiber material: thermoplastic polyurethane fiber, water contact angle of 140° to 150°, shear stiffness of 0.1 to 0.3, aspect ratio of 40 to 80;
[0045] Surfactant: blocked water-based isocyanate, manufactured by China Changzhou Houding Chemical Co., Ltd., model number HD-8035;
[0046] water;
[0047] (2) The hydrophilic fiber material, the hydrophobic fiber material and the surfactant are dispersed in water, and the fiber suspension is obtained by shearing with a shearing machine (shear rate of 23000 rpm), and the fiber suspension is allowed to stand at -70°C (supercooling degree of 7°C) for 6 hours, and freeze-dried (temperature of -50°C, pressure of 20 Pa, time of 36 hours) to obtain an aerogel;
[0048] The mass ratio of the hydrophilic fiber material to the hydrophobic fiber material is 2; the content of the hydrophilic fiber material in the fiber suspension is 0.67wt%, and the content of the surfactant is 1wt%.
[0049] The aerogel with multi-oriented pores finally obtained is an aerogel with anisotropic stepped pores, such as Figure 4 As shown, it can be used as wave absorbing and transmitting material, building fireproof and heat-insulating material, sewage treatment and seawater desalination material, one-way moisture-conducting material, microelectronics or water-retaining agent.
[0050] Example 3
[0051] A method for preparing an aerogel with multi-oriented pores, the specific steps are as follows:
[0052] (1) Preparation of raw materials;
[0053] Hydrophilic fiber material: Hydroxypropyl methylcellulose fiber, water contact angle of 10° to 20°, shear stiffness of 10 to 20, aspect ratio of 2 to 10;
[0054] Hydrophobic fiber material: polycaprolactone fiber, water contact angle of 130° to 150°, shear stiffness of 0.1 to 0.3, aspect ratio of 40 to 80;
[0055] Surfactant: Lauramidopropyl hydroxysulfobetaine, CAS No. 13197-76-7;
[0056] water;
[0057] (2) The hydrophilic fiber material, the hydrophobic fiber material and the surfactant are dispersed in water, and the fiber suspension is obtained by shearing with a shearing machine (shear rate of 25000 rpm), and the fiber suspension is allowed to stand at -196 ° C (supercooling degree of 8 ° C) for 0.2 h, and freeze-dried (temperature of -60 ° C, pressure of 40 Pa, time of 48 h) to obtain an aerogel;
[0058] The mass ratio of the hydrophilic fiber material to the hydrophobic fiber material is 3; the content of the hydrophilic fiber material in the fiber suspension is 0.75wt%, and the content of the surfactant is 2wt%.
[0059] The aerogel with multi-oriented pores finally obtained is an aerogel with anisotropic stepped pores, which can be used as wave absorbing and transmitting materials, building fireproof and heat-insulating materials, sewage treatment and seawater desalination materials, unidirectional moisture-conducting materials, microelectronics or water-retaining agents.
[0060] Example 4
[0061] A method for preparing an aerogel with multi-oriented pores is basically the same as that of Example 3, except that no surfactant is added in step (2).
[0062] The aerogel with multi-oriented pores finally obtained is an aerogel with anisotropic stepped pores, which can be used as wave absorbing and transmitting materials, building fireproof and heat-insulating materials, sewage treatment and seawater desalination materials, unidirectional moisture-conducting materials, microelectronics or water-retaining agents.
Claims
1. A method for preparing an aerogel having multi-oriented pores, characterized in that: The hydrophilic fiber material and the hydrophobic fiber material are dispersed in water, and after being sheared by a shearing machine to obtain a fiber suspension, the fiber suspension is frozen until completely frozen, and then freeze-dried to obtain an aerogel; The hydrophilic fiber material is cellulose fiber or cellulose derivative fiber; the water contact angle of the hydrophilic fiber material is 0°~20°, the shear stiffness is 10~20, and the aspect ratio is ≤10; the water contact angle of the hydrophobic fiber material is 130°~150°, the shear stiffness is 0.1~0.5, and the aspect ratio is ≥40; the mass ratio of the hydrophilic fiber material to the hydrophobic fiber material is ≥1; the shear rate of the shearing machine is 20000~25000rpm; the supercooling degree during freezing is ≥5.5℃.
2. The method for preparing an aerogel having multi-oriented pores according to claim 1, characterized in that: The aspect ratio of the hydrophilic fiber material is 1-10, and the aspect ratio of the hydrophobic fiber material is 40-80.
3. The method for preparing an aerogel having multi-oriented pores according to claim 1, characterized in that: The hydrophobic fiber material is thermoplastic polyurethane fiber, polylactic acid fiber or polycaprolactone fiber.
4. The method for preparing an aerogel having multi-oriented pores according to claim 1, characterized in that: In the fiber suspension, the content of the hydrophilic fiber material is 0.5-0.75wt%.
5. The method for preparing an aerogel having multi-oriented pores according to claim 1, characterized in that: The fiber suspension also contains 0.25-2 wt% of a surfactant.
6. The method for preparing an aerogel having multi-oriented pores according to claim 1, characterized in that: Freezing the fiber suspension until it is completely frozen means leaving the fiber suspension at -50 to -196°C for 0.2 to 8 hours.
7. An aerogel having multi-oriented pores, characterized in that: The aerogel having multi-oriented pores is prepared by the preparation method of any one of claims 1 to 6.
8. The use of an aerogel with multi-oriented pores as claimed in claim 7, characterized in that: Used as lightweight and high-strength composite materials, aerogel-based electrode materials, energy storage and conversion materials, wave absorbing and transmitting materials, building fireproof and heat-insulating materials, sewage treatment and seawater desalination materials, one-way moisture-conducting materials, microelectronics or water-retaining agents.