A surface selenium-rich Sb2(S,Se)3 film and preparation method thereof and solar cell
The microfluidic peristaltic pump assisted chemical water bath method regulates the gradient distribution of S-Se elements in Sb2(S,Se)3 film, solves the problem of energy band mismatch, improves the photoelectric conversion efficiency of solar cells and the density of the film, and realizes the Efficient preparation of Sb2(S,Se)3 films.
Patent Information
- Application Number
- CN202411059376.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-03
AI Technical Summary
The confusion of S-Se element distribution in existing Sb2(S,Se)3 solar cell thin films leads to mismatch in energy bands, limiting the improvement of photoelectric conversion efficiency.
The microfluidic peristaltic pump assisted chemical water bath method is used to control the concentration and pumping speed of the Se source, and the gradient distribution of the S-Se element is controlled, forming a gradually narrowing energy level distribution from the bottom of the film to the surface, reducing carrier recombination.
The preparation of Sb2(S,Se)3 films with uniform and dense surfaces and few body phase defects was achieved, which improved the photoelectric conversion efficiency to 9.5%, and reduced the raw material cost and reaction temperature.
Smart Images

Figure CN118600400B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor photovoltaic materials and devices, and in particular to a surface selenium-rich Sb2(S,Se)3 film, a preparation method thereof, and a solar cell. Background Art
[0002] Energy is closely related to human survival and development, and is the cornerstone supporting the normal operation of human society. With the development of society and the advancement of science and technology, human demand for energy is growing, and traditional fossil energy is likely to be exhausted, so people turn their attention to new renewable energy technologies. Solar energy, as an inexhaustible clean energy, is considered to be the most promising renewable energy. In recent years, antimony selenide (Sb2(S,Se)3) has been widely used due to its adjustable band gap (1.1–1.7eV), high absorption coefficient (>105cm -1 ), excellent phase, low toxicity of raw materials, rich storage, simple composition, excellent photoelectric performance, etc., showing great development prospects in the photovoltaic field and attracting extensive attention from researchers at home and abroad. However, the current photoelectric conversion efficiency of Sb2(S,Se)3 solar cells is generally below 10%, and it is urgent to explore key technologies to further improve device performance.
[0003] At present, researchers at home and abroad have conducted in-depth exploration on how to improve the efficiency of Sb2(S,Se)3 thin film solar cells, including Sb2(S,Se)3 thin film preparation methods, crystal growth orientation and device structure. Among them, the special quasi-one-dimensional crystal structure of Sb2(S,Se)3 materials causes the photoelectric anisotropy of the material and the complex defect properties. Exploring suitable preparation methods has become the most important link in the process of building high-efficiency Sb2(S,Se)3 devices. One of the main problems of Sb2(S,Se)3 thin film solar cells at present is the band mismatch caused by the chaotic distribution of S-Se elements. So far, researchers at home and abroad have developed vacuum and non-vacuum methods. Common vacuum methods include vapor transport deposition (VTD), thermal evaporation, magnetron sputtering, etc. However, the vacuum method has high requirements for experimental equipment and the film is prone to holes, which seriously affects the performance of the final device. To this end, researchers have explored a series of non-vacuum methods, including hydrothermal method, solution spin coating and chemical bath deposition (CBD), etc. The hydrothermal method for preparing thin films is a closed process, and it is impossible to directly and conveniently control the element distribution; the spin coating method for preparing thin films is prone to holes; although chemical bath deposition (CBD) is a relatively open reaction system, it is still difficult to control the doping amount and doping time node in real time during the reaction.
[0004] The Sb2(S,Se)3 thin film is prepared by a one-step solution method, especially the chemical water bath deposition technology. Due to the difference in solubility products between Sb2Se3 and Sb2S3, a large amount of Se element is consumed in the early stage of the reaction, and the S element is relatively increased, resulting in a sharp increase in the S / Se gradient from the bottom to the surface of the film, and then a gradually widening energy level distribution. This energy level distribution seriously hinders hole transport and aggravates carrier recombination, thereby limiting the further improvement of device efficiency. In order to reduce non-radiative recombination of carriers and effectively improve the photoelectric conversion efficiency, the current problem of energy band mismatch caused by the chaotic distribution of S-Se elements needs to be solved urgently. Summary of the invention
[0005] In view of this, the present invention proposes a surface selenium-rich Sb2(S,Se)3 film, a preparation method thereof and a solar cell, so as to solve the problem that it is difficult to regulate the distribution of S-Se elements in the existing Sb2(S,Se)3 film preparation, thereby promoting the band mismatch problem caused by the chaotic distribution of S-Se elements in the Sb2(S,Se)3 film.
[0006] The technical solution of the present invention is achieved in this way:
[0007] In a first aspect, the present invention provides a method for preparing a surface selenium-rich Sb2(S,Se)3 thin film, comprising the following steps:
[0008] S1, mixing potassium antimony tartrate with a sulfur source to obtain a Sb2S3 precursor solution;
[0009] S2. After depositing the Sb2S3 film to a preset thickness by a chemical water bath method, the Se source is pumped into the Sb2S3 precursor solution through a peristaltic pump, and the S-Se element gradient distribution of the deposited film is regulated. After the reaction is completed, the film is dried to obtain a Sb2(S,Se)3 precursor film;
[0010] S3. Annealing the Sb2(S,Se)3 precursor film to obtain a Sb2(S,Se)3 thin film with a selenium-rich surface. The surface of the Sb2(S,Se)3 thin film is rich in Se elements, and the bottom is rich in S elements.
[0011] The present invention introduces a microfluidic peristaltic pump into a reaction system, and adopts a microfluidic peristaltic pump-assisted chemical water bath method to controllably adjust the S / Se gradient from the bottom to the surface of the film, so as to obtain an ideal flat gradient or a gradually narrowing gradient, effectively strengthen hole transport, and reduce carrier recombination. The method can be implemented by adding a Se source to the reaction in the late reaction stage through a peristaltic pump when depositing an Sb2S3 film, and after a certain thickness of an Sb2S3 film has been deposited on a substrate, the film surface is Se-treated by the introduction of Se to obtain an Sb2(S,Se)3 film. By adding a Se source through a peristaltic pump, the Se element content added to the reaction system can be determined by changing the concentration of the Se source pumped in, the speed of the Se source pumped in per unit time, or the reaction time, and at the same time, a flexible, continuous and stable addition effect can be achieved, forming a gradually narrowing or flattening energy level distribution, which is conducive to the transmission of holes, thereby solving the problem of energy band mismatch caused by the chaotic distribution of S-Se elements. The above technical solution can achieve a slowdown or change in the S / Se gradient from the bottom to the surface of the film, thereby obtaining a gradually narrowing energy level distribution, increasing the hole transport capacity, reducing non-radiative recombination, and further developing a Sb2(S,Se)3 thin film preparation technology with an adjustable gradient bandgap structure, a uniform and dense surface, and few bulk defects.
[0012] On the basis of the above technical solution, preferably, in step S2, the preset thickness is 100-200 nm.
[0013] On the basis of the above technical scheme, preferably, in step S2, the Se source is pumped into the Sb2S3 precursor solution through a peristaltic pump, and the S-Se element gradient distribution of the deposited film is regulated, specifically including: adjusting the Se source concentration, and pumping the Se source into the Sb2S3 precursor solution at a speed of 0.001-0.5ml / min through a peristaltic pump for 1-3h to achieve the S-Se element gradient distribution of the deposited film.
[0014] On the basis of the above technical solution, preferably, in step S2, the Se source includes Na2SeSO3 solution and / or CH4N2Se solution, the concentration of the Na2SeSO3 solution is 0.1-0.3 mol / L, the concentration of the CH4N2Se solution is 2×10 -3 ~2×10 -2 mol / L.
[0015] On the basis of the above technical scheme, preferably, the preparation method of the Na2SeSO3 solution comprises: the molar ratio of Se particles to Na2SO3 is 1-5:8-15, placed in 30-100 ml of deionized water for hydrothermal reaction, the hydrothermal temperature is 110-150°C, the hydrothermal time is 4-10 hours, and the Na2SeSO3 solution is obtained. The preparation method of the CH4N2Se solution comprises: 8×10-5 ~5×10 -4 mol of CH4N2Se is placed in 30~100ml of deionized water and stirred at room temperature and a stirring rate of 300~900 r / min to obtain a CH4N2Se solution.
[0016] Specifically, Na2SeSO3 is an inorganic Se source that can provide a large amount of Se ions, and CH4N2Se is an organic Se source that can slowly release Se ions at a lower concentration. By regulating the concentrations of these two Se sources, the amount of Se added to the film can be finely adjusted. The Se source pumping speed and time are controlled by a peristaltic pump. The slow addition speed allows Se ions to have enough time (1-3h) to diffuse into the deposited Sb2S3 film, thereby achieving the gradual penetration of Se from the surface to the bottom of the film, forming an S-Se gradient distribution. With the introduction of Se, the density of the film will increase, but too high a Se content will produce holes in the Sb2(S,Se)3 film.
[0017] On the basis of the above technical scheme, preferably, step S1 specifically includes: dissolving KSbC4H4O7•0.5H2O, Na2S2O3·5H2O and C2H5NS in water at 25-27°C, with a stirring rate of 300-900 r / min and a stirring time of 5-10 min to obtain a Sb2S3 precursor solution, wherein the molar ratio of KSbC4H4O7•0.5H2O, Na2S2O3·5H2O and C2H5NS is 2~5:10~20:1~5.
[0018] Based on the above technical solution, preferably, in step S2, the temperature of the chemical water bath reaction is 60-95°C and the time is 2-6 hours; in step S3, the annealing temperature is 300-500°C and the annealing time is 5-15 minutes. More preferably, the annealing temperature is 300-375°C.
[0019] Specifically, a chemical water bath method is used to first deposit an Sb2S3 thin film for a period of time. After the Sb2S3 thin film is deposited to a preset thickness, a Se source is pumped into the Sb2S3 precursor solution through a peristaltic pump while reacting in the chemical water bath. The S-Se element gradient distribution of the deposited Sb2(S,Se)3 thin film is regulated by changing the concentration of the pumped Se source, the speed of the pumped Se source per unit time, or the reaction time. The sample is then annealed in a N2 atmosphere. Annealing can promote the diffusion of Se in the film to form an S-Se gradient distribution, which is also beneficial to the crystallization and performance improvement of the film.
[0020] The water bath temperature is 80~95℃, and the reaction time is 3~6h. If the water bath temperature is higher than 95℃, it is not conducive to carrier transport, and the growth of the film is difficult to control at high temperature. If the reaction time is less than 3h, the thickness of the film is not enough to fully absorb sunlight, and it is not enough to support the doping and diffusion of Se source in the later stage of the reaction. If the reaction time exceeds 6h, the film morphology will deteriorate, affecting carrier transport.
[0021] In a second aspect, the present invention provides a Sb2(S,Se)3 thin film with a selenium-rich surface, wherein the Sb2(S,Se)3 thin film is prepared by a preparation method as described in any of the above items, and the S element content of the Sb2(S,Se)3 thin film shows a gradient decreasing trend from the bottom to the surface, and the Se element content shows a gradient increasing trend.
[0022] Specifically, the thin film structure with Se-rich surface and S-rich bottom mainly improves the transmission of electrons and holes, reduces non-radiative recombination, and forms a more suitable energy level structure. This S-Se gradient distribution Sb2(S,Se)3 thin film structure can better meet the various requirements of solar cells for the light absorption layer.
[0023] In a third aspect, the present invention provides a solar cell, comprising, from bottom to top, a substrate, an electron transport layer, a light absorption layer, a hole transport layer and an anode, wherein the light absorption layer is a surface selenium-rich Sb2(S,Se)3 film as described above.
[0024] Specifically, in the solar cell device, the cathode, electron transport layer, hole transport layer, and anode are all well known to those skilled in the art, and there is no particular limitation in the present application.
[0025] On the basis of the above technical solution, preferably, the S-rich side of the Sb2(S,Se)3 film is close to the electron transport layer, and the Se-rich side is close to the hole transport layer.
[0026] In the present invention, surface Se-enrichment is beneficial to improving carrier transport efficiency, the valence electron structure of Se atoms is beneficial to the separation and transport of carriers (electrons and holes), and surface Se-enrichment helps in the rapid separation and collection of photogenerated carriers, thereby improving the photoelectric conversion efficiency of the device; bottom S-enrichment can improve the interface characteristics with the bottom electrode, and good interface contact and energy level matching are formed between S atoms and the electron transport layer.
[0027] On the basis of the above technical solution, preferably, the method for preparing the solar cell includes:
[0028] (1) Cd(NO3)2 and CH4N2S are dissolved in water, mixed with ammonia water and stirred at 25-27°C, and an electron transport layer is prepared on the substrate surface by a chemical water bath method;
[0029] (2) using an anhydrous methanol solution of CdCl2 to spin-coat the surface of the electron transport layer, and then performing high-temperature annealing in an air atmosphere;
[0030] (3) depositing a surface selenium-rich Sb2(S,Se)3 film as a light absorption layer on a substrate having an electron transport layer deposited thereon;
[0031] (4) preparing a hole transport layer by spin coating on the surface of the light absorption layer;
[0032] (5) The Au electrode is deposited on the surface of the hole transport layer by thermal evaporation to obtain the solar cell.
[0033] Based on the above technical solution, preferably, in step (1), the molar ratio of Cd(NO3)2, CH4N2S and ammonia water is 1-3:50-100:300-500, the temperature of the chemical water bath is 50-80°C, and the time is 10-30 min.
[0034] On the basis of the above technical scheme, preferably, in step (2), the concentration of the anhydrous methanol solution of CdCl2 is 10-50 mg / ml, and when the spin coating is performed, the spin coating speed is 2000-5000 r / s, the spin coating time is 20-50 s, and the annealing temperature after the spin coating is completed is 200-500°C, and the annealing time is 5-30 min.
[0035] Based on the above technical solution, preferably, in step (4), Sprio-OMeTAD is spin-coated on the Sb2(S,Se)3 film, the spin-coating speed is 2000~5000r / s, the spin-coating time is 20~50s, and after the spin-coating is completed, the annealing temperature is 50~150℃, and the annealing time is 5~20min.
[0036] Based on the above technical solution, preferably, in step (5), the Au electrode is deposited by thermal evaporation, and the thickness of the Au electrode is 50-100 nm.
[0037] The surface selenium-rich Sb2(S,Se)3 thin film and its preparation method and solar cell of the present invention have the following beneficial effects compared with the prior art:
[0038] (1) By preparing a Sb2(S,Se)3 thin film with a selenium-rich surface, the S element content of the film decreases gradually from the bottom to the surface, and the Se element content increases gradually, which is conducive to obtaining a gradually narrowing energy level distribution, increasing the hole transport capacity, and reducing non-radiative recombination. This S-Se gradient distribution Sb2(S,Se)3 thin film structure is applied to solar cells to better improve the photoelectric conversion efficiency of solar cells. The photoelectric conversion efficiency of the Sb2(S,Se)3 thin film prepared by the present invention is 9.5%;
[0039] (2) The S / Se gradient from the bottom to the surface of the film can be controlled by using a microfluidic peristaltic pump-assisted chemical water bath method. The Se content added to the reaction system can be determined by changing the concentration of the Se source pumped in, the speed of the Se source pumped in per unit time, or the reaction time. At the same time, flexible, continuous, and stable addition effects can be achieved, forming a gradually narrowing or flattening energy level distribution, which is beneficial to the transmission of holes, thereby solving the problem of energy band mismatch caused by the chaotic distribution of S-Se elements.
[0040] (3) The surface selenium-rich gradient component Sb2(S,Se)3 film synthesized by microfluidic peristaltic pump-assisted chemical water bath method has a uniform and dense surface, few bulk defects, low cost of raw materials, low reaction temperature, no need for organic solvents, and a simple and environmentally friendly preparation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 XRD diagrams of Sb2(S,Se)3 thin films, Sb2S3 thin films and Sb2Se3 thin films prepared in Example 1 of the present invention, where the abscissa 2θ indicates the diffraction angle of X-rays;
[0043] Figure 2 SEM images of Sb2(S,Se)3 thin film, Sb2S3 thin film and Sb2Se3 thin film prepared in Example 1 of the present invention;
[0044] Figure 3 This is a TOF-SIMS (time-of-flight secondary ion mass spectrometry) image of the Sb2(S,Se)3 thin film prepared in Example 1 of the present invention;
[0045] Figure 4EQE diagrams of Sb2(S,Se)3 thin films, Sb2S3 thin films and Sb2Se3 thin films prepared in Example 1 of the present invention;
[0046] Figure 5 The ultraviolet absorption spectra of the Sb2(S,Se)3 thin film, Sb2S3 thin film and Sb2Se3 thin film prepared in Example 1 of the present invention;
[0047] Figure 6 Photovoltaic parameter diagram of Sb2(S,Se)3 thin film, Sb2S3 thin film and Sb2Se3 thin film prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0048] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.
[0050] Example 1
[0051] This embodiment provides a surface selenium-rich Sb2(S,Se)3 thin film and a preparation method thereof and a solar cell, and the specific operations are as follows:
[0052] (1) Take 15 ml of 0.03 mol / L Cd(NO3)2 solution, 5 ml of 2 mol / L CH4N2S solution, 20 ml of ammonia (25-28%) and 60 ml of deionized water, and stir at room temperature at a stirring rate of 400 r / min for 3 min. Place FTO on the substrate, then put it into the sample bottle and pour in the precursor solution. Using the chemical water bath method, put the sample bottle into a water bath pot and bathe it at a water bath temperature of 50°C for 20 min. Then take out the FTO, rinse it clean, and obtain a light yellow CdS film as the electron transport layer.
[0053] (2) Place the CdS-deposited FTO obtained in step (1) on a coating machine, and use an anhydrous methanol solution of CdCl2 with a concentration of 10 mg / ml to spin coat the surface of CdS. Use a pipette to draw 50 μl of the solution for spin coating, the spin coating speed is 4000 r / s, and the spin coating time is 30 s. After spin coating, place it on a heating table for annealing in an air atmosphere, the annealing temperature is 300°C, the annealing time is 20 min, and then cool to 150°C and remove it for use.
[0054] (3) Weigh KSbC4H4O7·0.5H2O (1 g, 2.57 mmol), Na2S2O3·5H2O (3 g, 12.09 mmol) and (0.01 g, 0.13 mmol) was placed in 40 ml of deionized water and stirred at room temperature at a stirring rate of 700 r / min. After it was completely dissolved, a Sb2S3 precursor solution was obtained.
[0055] (4) Pour the Sb2S3 precursor solution into the sample bottle containing the FTO with CdS deposited in step (2), and use the chemical water bath method to deposit the thin film. The water bath temperature is 90°C. After the water bath reaction for 2 hours, the Sb2S3 film is made to a preset thickness (150nm). Se particles (0.7g, 8.87mol), Na2SO3 (5g, 39.67mmol) and 40ml of deionized water are weighed and placed in the reactor lining. The mixture is hydrothermaled at 140°C for 5 hours to obtain a Na2SeSO3 solution. 8ml of the Na2SeSO3 solution (0.2mol / L) is mixed with 22ml of deionized water. Use a peristaltic pump to pump the Se source solution into the Sb2S3 precursor solution in step (3) at a rate of 0.2 ml / min when the reaction lasts for 2 hours, and continue the water bath reaction for 1 hour (the Se source pumping time is the same) to achieve Se element doping. After the reaction is completed, the Sb2(S,Se)3 precursor film is rinsed clean and annealed in a N2 atmosphere at a temperature of 350°C and a time of 10 minutes to obtain a gradient band gap Sb2(S,Se)3 thin film sample.
[0056] (5) Weigh 1g of Spiro powder and place it in a sample bottle. Then add 2ml of chlorobenzene with a syringe. After shaking until completely dissolved, add 20μl of tetra-tert-butylpyridine and 20μl of lithium salt. Spin-coat Spiro-OMeTAD on the surface of the FTO / CdS / Sb2(S,Se)3 sample obtained in step (4). Use a pipette to draw 20μl of solution for spin coating. The spin coating speed is 4000r / s and the spin coating time is 30s. After spin coating, place it on a heating table for annealing in an air atmosphere. The annealing temperature is 150℃ and the annealing time is 20min.
[0057] (6) Deposit Au electrode by thermal evaporation. Fix the sample in the template and place it in the evaporation chamber. -4 About 60 nm of Au was deposited under high vacuum conditions of Pa to obtain a complete device.
[0058] Example 2
[0059] This embodiment provides a surface selenium-rich Sb2(S,Se)3 thin film and a preparation method thereof and a solar cell, and the specific operations are as follows:
[0060] (1) Take 15 ml of 0.03 mol / L Cd(NO3)2 solution, 12 ml of 2 mol / L CH4N2S solution, 8.5 ml of ammonia (25-28%) and 60 ml of deionized water, and stir at room temperature at a stirring rate of 400 r / min for 3 min. Place FTO on the substrate, then put it into the sample bottle and pour in the precursor solution. Using the chemical water bath method, put the sample bottle into a water bath pot and bathe it at a water bath temperature of 65°C for 10 min. Then take out the FTO, rinse it clean, and obtain a light yellow CdS film as the electron transport layer.
[0061] (2) Place the CdS-deposited FTO obtained in step (1) on a coating machine, and use an anhydrous methanol solution of CdCl2 with a concentration of 25 mg / ml to spin coat the surface of CdS. Use a pipette to draw 50 μl of the solution for spin coating, the spin coating speed is 2000 r / s, and the spin coating time is 20 s. After spin coating, place it on a heating table for annealing in an air atmosphere, the annealing temperature is 200°C, the annealing time is 5 min, and then cool to 150°C and remove it for use.
[0062] (3) Weigh KSbC4H4O7·0.5H2O (1 g, 2.57 mmol), Na2S2O3·5H2O (6.38 g, 25.7 mmol) and (0.096 g, 1.285 mmol) was placed in 80 ml of deionized water and stirred at room temperature at a stirring rate of 300 r / min for 5 min. After it was completely dissolved, a Sb2S3 precursor solution was obtained.
[0063] (4) Pour the Sb2S3 precursor solution into the sample bottle containing the FTO with CdS deposited in step (2), and use the chemical water bath method to deposit the thin film. The water bath temperature is 60°C. After the water bath reacts for 1 hour, the Sb2S3 film reaches the preset thickness (100nm). Se particles (0.7g, 8.87mol), Na2SO3 (5g, 39.67mmol) and 40ml of deionized water are weighed and placed in the reactor lining. Hydrothermal treatment is performed at 140°C for 5 hours to obtain Na2SeSO3 solution. 8ml of Na2SeSO3 solution (0.1mol / L) is mixed with 22ml of deionized water. Use a peristaltic pump to pump the Se source solution into the Sb2S3 precursor solution in step (3) at a rate of 0.001 ml / min when the reaction lasts for 1 hour, and continue the water bath reaction for 1 hour (the Se source pumping time is the same) to achieve Se element doping. After the reaction is completed, the Sb2(S,Se)3 precursor film is rinsed clean and annealed in a N2 atmosphere at a temperature of 300°C and a time of 5 minutes to obtain a gradient band gap Sb2(S,Se)3 thin film sample.
[0064] (5) Weigh 1g of Spiro powder and place it in a sample bottle. Then add 2ml of chlorobenzene with a syringe, shake until completely dissolved, then add 20μl of tetra-tert-butylpyridine and 20μl of lithium salt to obtain Spiro-OMeTAD. Spin-coat Spiro-OMeTAD on the surface of the FTO / CdS / Sb2(S,Se)3 sample obtained in step (4). Use a pipette to draw 20μl of solution for spin coating. The spin coating speed is 2000r / s and the spin coating time is 20s. After spin coating, place it on a heating table for annealing in an air atmosphere. The annealing temperature is 50℃ and the annealing time is 5min.
[0065] (6) Deposit Au electrode by thermal evaporation. Fix the sample in the template and place it in the evaporation chamber. -4 About 50 nm of Au was deposited under high vacuum conditions of Pa to obtain a complete device.
[0066] Example 3
[0067] This embodiment provides a surface selenium-rich Sb2(S,Se)3 thin film and a preparation method thereof and a solar cell, and the specific operations are as follows:
[0068] (1) Take 15 ml of 0.03 mol / L Cd(NO3)2 solution, 7.5 ml of 2 mol / L CH4N2S solution, 4.75 ml of ammonia (25-28%) and 60 ml of deionized water, and stir at room temperature at a stirring rate of 400 r / min for 3 min. Place FTO on the substrate, then put it into the sample bottle and pour in the precursor solution. Using the chemical water bath method, put the sample bottle into a water bath pot and bathe it at a water bath temperature of 80°C for 30 min. Then take out the FTO, rinse it clean, and obtain a light yellow CdS film as the electron transport layer.
[0069] (2) Place the CdS-deposited FTO obtained in step (1) on a coating machine, and use an anhydrous methanol solution of CdCl2 with a concentration of 50 mg / ml to spin coat the surface of CdS. Use a pipette to draw 50 μl of the solution for spin coating, the spin coating speed is 5000 r / s, and the spin coating time is 50 s. After the spin coating is completed, place it on a heating table for annealing in an air atmosphere, the annealing temperature is 500°C, the annealing time is 30 min, and then cool to 150°C and remove it for use.
[0070] (3) Weigh KSbC4H4O7·0.5H2O (1 g, 2.57 mmol), Na2S2O3·5H2O (1.28 g, 5.14 mmol) and (0.19 g, 2.57 mmol) was placed in 40 ml of deionized water and stirred at room temperature at a stirring rate of 700 r / min. After it was completely dissolved, a Sb2S3 precursor solution was obtained.
[0071] (4) Pour the Sb2S3 precursor solution into the sample bottle containing the FTO with CdS deposited in step (2), and use the chemical water bath method to deposit the thin film. The water bath temperature is 95°C. After the water bath reaction for 3 hours, the Sb2S3 film is made to a preset thickness (200nm). Se particles (0.7g, 8.87mol), Na2SO3 (5g, 39.67mmol) and 40ml of deionized water are weighed and placed in the reactor lining. The mixture is hydrothermaled at 140°C for 5 hours to obtain a Na2SeSO3 solution. 8ml of the Na2SeSO3 solution (0.3mol / L) is mixed with 22ml of deionized water. Use a peristaltic pump to pump the Se source solution into the Sb2S3 precursor solution in step (3) at a rate of 0.5 ml / min when the reaction lasts for 3 hours, and continue the water bath reaction for 3 hours (the Se source pumping time is the same) to achieve Se element doping. After the reaction is completed, the Sb2(S,Se)3 precursor film is rinsed clean and annealed in a N2 atmosphere at a temperature of 500°C and a time of 15 minutes to obtain a gradient band gap Sb2(S,Se)3 thin film sample.
[0072] (5) Weigh 1g of Spiro powder and place it in a sample bottle. Then add 2ml of chlorobenzene with a syringe, shake until completely dissolved, then add 20μl of tetra-tert-butylpyridine and 20μl of lithium salt to obtain Spiro-OMeTAD. Spin-coat Spiro-OMeTAD on the surface of the FTO / CdS / Sb2(S,Se)3 sample obtained in step (4). Use a pipette to draw 20μl of solution for spin coating. The spin coating speed is 5000r / s and the spin coating time is 50s. After spin coating, place it on a heating table for annealing in an air atmosphere. The annealing temperature is 100℃ and the annealing time is 10min.
[0073] (6) Deposit Au electrode by thermal evaporation. Fix the sample in the template and place it in the evaporation chamber. -4 About 100 nm of Au was deposited under high vacuum conditions of Pa to obtain a complete device.
[0074] Example 4
[0075] This embodiment provides a surface selenium-rich Sb2(S,Se)3 film, a preparation method thereof, and a solar cell. The specific preparation method is the same as that in Example 1, except that: the Se source is a CH4N2Se solution, 50 mg of CH4N2Se is weighed and placed in 30 ml of deionized water, and stirred at room temperature until completely dissolved, with a stirring rate of 800 r / min.
[0076] Example 5
[0077] This embodiment provides a surface selenium-rich Sb2(S,Se)3 film, a preparation method thereof, and a solar cell. The specific preparation method is the same as that in Example 1, except that: in step (4), the concentration of the Na2SeSO3 solution is 0.05 mol / L, and the Se source is pumped into the Sb2S3 precursor solution at a rate of 0.8 ml / min.
[0078] Example 6
[0079] The present embodiment provides a surface selenium-rich Sb2(S,Se)3 film, a preparation method thereof, and a solar cell. The specific preparation method is the same as that in Example 1, except that: in step (4), the concentration of the Na2SeSO3 solution is 0.4 mol / L, and the Se source is pumped into the Sb2S3 precursor solution at a rate of 0.2 ml / min for 0.5 h. After 0.5 h, the pumping is stopped and the water bath reaction is continued for 0.5 h.
[0080] Example 7
[0081] This embodiment provides a surface selenium-rich Sb2(S,Se)3 film and a preparation method thereof and a solar cell. The specific preparation method is the same as that of Embodiment 1, except that:
[0082] (4) Pour the Sb2S3 precursor solution into the sample bottle containing the FTO with CdS deposited in step (2), and use the chemical water bath method to deposit the thin film. The water bath temperature is 100°C. After the water bath reaction for 3 hours, the Sb2S3 film is made to a preset thickness. Se particles (0.7 g, 8.87 mol), Na2SO3 (5 g, 39.67 mmol) and 40 ml of deionized water are weighed and placed in the reactor lining. The mixture is hydrothermaled at 140°C for 5 hours to obtain a Na2SeSO3 solution. 8 ml of the Na2SeSO3 solution (0.2 mol / L) is mixed with 22 ml of deionized water. Use a peristaltic pump to pump the Se source solution into the Sb2S3 precursor solution in step (3) at a rate of 0.2 ml / min when the reaction lasts for 3 hours, and continue the water bath reaction for 4 hours (the Se source pumping time is the same) to achieve Se element doping. After the reaction is completed, the Sb2(S,Se)3 precursor film is rinsed clean and annealed in a N2 atmosphere at a temperature of 350°C and a time of 10 minutes to obtain a gradient band gap Sb2(S,Se)3 thin film sample.
[0083] Example 8
[0084] The present embodiment provides a Sb2(S,Se)3 thin film with a selenium-rich surface, a preparation method thereof, and a solar cell. The specific preparation method is the same as that in Example 1, except that: in step (4), after the reaction is completed, the Sb2(S,Se)3 precursor film is rinsed clean and then directly dried to obtain a Sb2(S,Se)3 thin film sample.
[0085] Comparative Example 1
[0086] This comparative example provides a surface selenium-rich Sb2(S,Se)3 film and a preparation method and a solar cell thereof. The specific preparation method is the same as that of Example 1, except that:
[0087] In step (4), the Sb2S3 precursor solution is poured into the sample bottle containing the FTO deposited with CdS obtained in step (2), and the thin film is deposited by a chemical water bath method. The water bath temperature is 90°C. While the Sb2S3 thin film is being deposited, the Se source solution is pumped into the Se source solution. The water bath reaction time is a total of 3 hours (the Se source pumping time is the same). The remaining operations are the same as in Example 1.
[0088] Comparative Example 2
[0089] This comparative example provides a Sb2(S,Se)3 thin film and a preparation method thereof and a solar cell, and the specific operation steps are as follows:
[0090] (1) Take 15 ml of 0.03 mol / L Cd(NO3)2 solution, 5 ml of 2 mol / L CH4N2S solution, 20 ml of ammonia (25-28%) and 60 ml of deionized water, and stir at room temperature at a stirring rate of 400 r / min for 3 min. Place the FTO on the substrate, then put it into the sample bottle and pour in the precursor solution. Using the chemical water bath method, put the sample bottle into a water bath pot and bathe it at a water bath temperature of 50°C for 20 min. Then take out the FTO substrate, rinse it clean, and obtain a light yellow CdS film as the electron transport layer.
[0091] (2) Place the CdS-deposited FTO obtained in step (1) on a coating machine, and use an anhydrous methanol solution of CdCl2 with a concentration of 10 mg / ml to spin coat the surface of CdS. Use a pipette to draw 50 μl of the solution for spin coating, the spin coating speed is 4000 r / s, and the spin coating time is 30 s. After spin coating, place it on a heating table for annealing in an air atmosphere, the annealing temperature is 300°C, the annealing time is 20 min, and then cool to 150°C and remove it for use.
[0092] (3) Weigh KSbC4H4O7·0.5H2O (1 g, 2.57 mmol), Na2S2O3·5H2O (3 g, 12.09 mmol) and (0.01g, 0.13mmol) was placed in 40ml deionized water and stirred at room temperature at a stirring rate of 700r / min. After it was completely dissolved, the Sb2S3 precursor solution was obtained. Se particles (0.7g, 8.87mol), Na2SO3 (5g, 39.67mmol) and 40ml deionized water were weighed and placed in the reactor lining. They were hydrothermaled at 140℃ for 5h to obtain Na2SeSO3 solution. 8ml Na2SeSO3 solution (0.2mol / L) was mixed with 22ml deionized water, and then mixed with Sb2S3 precursor solution. The film was deposited by chemical water bath method. The water bath temperature was 90℃ and the water bath reaction was carried out for 3h. After the reaction was completed, the Sb2(S,Se)3 precursor film was rinsed clean and annealed in N2 atmosphere. The annealing temperature was 350℃ and the annealing time was 10min. The gradient band gap Sb2(S,Se)3 film sample was obtained.
[0093] (4) Weigh 1g of Spiro powder and place it in a sample bottle. Then add 2ml of chlorobenzene with a syringe. After shaking until completely dissolved, add 20μl of tetra-tert-butylpyridine and 20μl of lithium salt. Spin-coat Spiro-OMeTAD on the surface of the FTO / CdS / Sb2(S,Se)3 sample obtained in step (3). Use a pipette to draw 20μl of solution for spin coating. The spin coating speed is 4000r / s and the spin coating time is 30s. After spin coating, place it on a heating table for annealing in an air atmosphere. The annealing temperature is 150℃ and the annealing time is 20min.
[0094] (5) Deposit Au electrode by thermal evaporation. Fix the sample in the template and place it in the evaporation chamber. -4 About 60 nm of Au was deposited under high vacuum conditions of Pa to obtain a complete device.
[0095] Performance Testing
[0096] The photoelectric conversion efficiency of the solar cells prepared in the examples and comparative examples was tested, and the thickness of the Sb2(S,Se)3 films prepared in the examples and comparative examples was tested. The test results are shown in Table 1.
[0097] Table 1
[0098]
[0099] Figure 1 The XRD patterns of the Sb2(S,Se)3 film, Sb2S3 film and Sb2Se3 film prepared in Example 1 are shown, with the Sb2S3 film and Sb2Se3 film used as comparison. As can be seen from the figure, the diffraction peak of the XRD of Sb2(S,Se)3 is between that of Sb2S3 and Sb2Se3. From the (120) plane, it can be seen that the diffraction peak of Sb2(S,Se)3 shifts to a small angle. Since the radius of Se atoms is larger than that of S atoms, it can be proved that Se is effectively incorporated.
[0100] Figure 2 The SEM images of the Sb2(S,Se)3 thin film, Sb2S3 thin film and Sb2Se3 thin film prepared in Example 1 are shown. Figure 2 (a) is the surface SEM image of Sb2S3 film. Figure 2 (b) is the surface SEM image of Sb2(S,Se)3 film. Figure 2 (c) is the surface SEM image of Sb2Se3 film. Figure 2 (d) is the cross-sectional SEM image of the Sb2S3 device. Figure 2 (e) is a cross-sectional SEM image of the Sb2(S,Se)3 device. Figure 2(f) is a cross-sectional SEM image of the Sb2Se3 device. As can be seen from the figure, the surface morphology of the Sb2(S,Se)3 film is uniform and dense, no holes appear after selenium is doped, and the film thickness is relatively suitable, about 200nm.
[0101] Figure 3 The TOF-SIMS (time-of-flight secondary ion mass spectrometry) diagram of the Sb2(S,Se)3 film prepared in Example 1 is shown. As can be seen from the figure, starting from the Au electrode on the surface, the surface close to the Au electrode is obviously rich in Se elements, and decreases with the sputtering time until it disappears. The proportion of S element as a source element in the entire Sb2(S,Se)3 film is relatively stable.
[0102] Figure 4 The EQE (external quantum efficiency) diagram of the Sb2(S,Se)3 film, Sb2S3 film and Sb2Se3 film prepared in Example 1 is shown. As can be seen from the figure, Sb2(S,Se)3 has a more suitable band gap and effective light absorption, which reduces the non-radiative recombination of carriers.
[0103] Figure 5 The ultraviolet absorption spectra of the Sb2(S,Se)3 thin film, Sb2S3 thin film and Sb2Se3 thin film prepared in Example 1 are shown. As can be seen from the figure, Sb2(S,Se)3 has a more obvious light absorption effect in the short-wave band of 500-700 nm.
[0104] Figure 6 The photovoltaic parameter diagrams of the Sb2(S,Se)3 thin film, Sb2S3 thin film and Sb2Se3 thin film prepared in Example 1 are shown. Figure 6 (a) in the figure represents PCE (photovoltaic conversion efficiency), Figure 6 (b) in the figure indicates V OC (open circuit voltage), Figure 6 (c) in the figure represents FF (fill factor), Figure 6 The (d) in the figure indicates J SC (short circuit current), Figure 6 The (e) in the formula represents R s (series resistance), Figure 6 (f) in the formula represents R sh(Parallel resistance). As can be seen from the figure, Sb2(S,Se)3 has a better photoelectric conversion efficiency, Sb2S3 has a high open circuit voltage and low short circuit current, Sb2Se3 has a high short circuit current and low open circuit voltage, and Sb2(S,Se)3 has a more suitable combination of open circuit voltage and short circuit current. And the Sb2(S,Se)3 solar cell prepared by this method has a smaller device internal resistance and a higher composite resistance, and has an excellent fill factor, which is also the reason for the high efficiency of the device.
[0105] As can be seen from Table 1, by comparing Examples 1-4, it can be seen that the technical scheme of the present invention can prepare a Sb2(S,Se)3 film with a Se-rich surface, which can be applied to solar cells to improve the photoelectric conversion efficiency; by comparing Example 1 with Examples 5 and 6, it can be seen that the Se source concentration, Se source pumping speed and pumping time will affect the distribution of S-Se in the Sb2(S,Se)3 film, thereby affecting the photoelectric conversion efficiency of the film; by comparing Example 1 with Example 7, it can be seen that the temperature and time of the water bath reaction will affect the quality of the film, thereby affecting the photoelectric conversion efficiency of the film; by comparing Example 1 with Example 8, it can be seen that annealing treatment is beneficial to the gradient diffusion of the Se element, thereby improving the photoelectric conversion efficiency; by comparing Example 1 with Comparative Example 1, it can be seen that pumping Se elements after the Sb2S3 film is deposited to a preset thickness is more conducive to forming an ideal Sb2(S,Se)3 film with Se-rich surface and S-rich bottom, thereby improving the photoelectric conversion efficiency; by comparing Example 1 with Comparative Example 2, it can be seen that a Sb2(S,Se)3 film with Se-rich surface can be obtained by the coordinated control of a peristaltic pump and Se source pumping.
[0106] In an embodiment of the present invention, the solar cell device described in the present invention uses the Sb2(S,Se)3 thin film prepared by the above-mentioned preparation method as the light absorption layer, fluorine-doped SnO2 transparent conductive glass (FTO), cadmium sulfide (CdS), Spiro-OMeTAD and Au as the cathode, electron transport layer, hole transport layer and anode, respectively, to assemble into a complete battery device, wherein there is no restriction on the materials of the cathode, electron transport layer, hole transport layer and anode of the present invention.
[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a surface selenium-rich Sb2(S,Se)3 thin film, characterized in that: The following steps are involved: S1, mixing potassium antimony tartrate with a sulfur source to obtain a Sb2S3 precursor solution; S2. After depositing the Sb2S3 film to a preset thickness by a chemical water bath method, the Se source is pumped into the Sb2S3 precursor solution through a peristaltic pump, and the S-Se element gradient distribution of the deposited film is regulated. After the reaction is completed, the film is dried to obtain a Sb2(S,Se)3 precursor film; S3, annealing the Sb2(S,Se)3 precursor film to obtain a Sb2(S,Se)3 thin film with a selenium-rich surface, wherein the surface of the Sb2(S,Se)3 thin film is rich in Se elements and the bottom is rich in S elements; In step S2, the Se source is pumped into the Sb2S3 precursor solution through a peristaltic pump, and the S-Se element gradient distribution of the deposited film is regulated. Specifically, the Se source concentration is adjusted, and the Se source is pumped into the Sb2S3 precursor solution at a speed of 0.001-0.5 ml / min through a peristaltic pump for 1-3 hours to achieve the S-Se element gradient distribution of the deposited film; In step S2, the Se source includes Na2SeSO3 solution and / or CH4N2Se solution, the concentration of the Na2SeSO3 solution is 0.1-0.3 mol / L, and the concentration of the CH4N2Se solution is 2×10 -3 ~2×10 -2 mol / L; In step S2, the temperature of the chemical water bath reaction is 60-95° C. and the reaction time is 2-6 hours.
2. The method for preparing a surface selenium-rich Sb2(S,Se)3 thin film according to claim 1, characterized in that: Step S1 specifically includes: dissolving KSbC4H4O7•0.5H2O, Na2S2O3·5H2O and C2H5NS in water at 25-27°C, with a stirring rate of 300-900r / min and a stirring time of 5-10min to obtain a Sb2S3 precursor solution, wherein the molar ratio of KSbC4H4O7•0.5H2O, Na2S2O3·5H2O and C2H5NS is 2~5:10~20:1~5.
3. The method for preparing a surface selenium-rich Sb2(S,Se)3 thin film according to claim 1, characterized in that: In step S3, the annealing temperature is 300-500° C. and the annealing time is 5-15 min.
4. A surface selenium-rich Sb2(S,Se)3 film, characterized in that: The Sb2(S,Se)3 film is prepared by the preparation method described in any one of claims 1 to 3. The S element content of the Sb2(S,Se)3 film decreases gradually from the bottom to the surface, and the Se element content increases gradually.
5. A solar cell, characterized in that: From bottom to top, it includes a substrate, an electron transport layer, a light absorption layer, a hole transport layer and an anode, and the light absorption layer is a surface selenium-rich Sb2(S,Se)3 film as described in claim 4.
6. A solar cell according to claim 5, characterized in that: The S-rich side of the Sb2(S,Se)3 film is close to the electron transport layer, and the Se-rich side is close to the hole transport layer.
7. A solar cell according to claim 5, characterized in that: The method for preparing the solar cell comprises: (1) Cd(NO3)2 and CH4N2S are dissolved in water, mixed with ammonia water and stirred at 25-27°C, and an electron transport layer is prepared on the substrate surface by a chemical water bath method; (2) using an anhydrous methanol solution of CdCl2 to spin-coat the surface of the electron transport layer, and then performing high-temperature annealing in an air atmosphere; (3) depositing a surface selenium-rich Sb2(S,Se)3 film as a light absorption layer on a substrate having an electron transport layer deposited thereon; (4) preparing a hole transport layer by spin coating on the surface of the light absorption layer; (5) The Au electrode is deposited on the surface of the hole transport layer by thermal evaporation to obtain the solar cell.
8. A solar cell according to claim 7, characterized in that: In step (1), the molar ratio of Cd(NO3)2, CH4N2S and ammonia water is 1-3:50-100:300-500, the temperature of the chemical water bath is 50-80°C, and the time is 10-30 min.