A high-temperature graphene flexible heating device and preparation method thereof
By installing reinforcement ribs and anti-oxidation layer made of conductive materials on the surface of the graphene layer of the high-temperature graphene flexible heating device, the problem of cracks or defects during the deformation of the electrode is solved, the conductivity and stability are improved, and high efficiency is achieved , uniform heating effect and extend service life.
Patent Information
- Application Number
- CN202411074663.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The electrodes of the high-temperature graphene flexible heating device are prone to cracks or defects due to deformation during the heating process, resulting in uncertain conductivity and stability, which affects the heating effect.
Reinforcement ribs made of conductive materials are provided on the surface of the graphene layer to form conductive electrode units, and can be covered with an anti-oxidation layer. Reinforcement ribs can be fixed by clamps to ensure their stability and conductivity, so as to achieve smooth current transmission and efficient heating.
It improves the conductivity and stability of the electrode, reduces resistance and energy losses, ensures efficient, uniform and stable heating effects, and extends the service life of the device.
Smart Images

Figure CN118612898B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of graphene heating technology, and in particular to a high-temperature graphene flexible heating device and a preparation method thereof. Background Art
[0002] As a new type of heating product, high-temperature graphene flexible heating devices have attracted widespread attention across various industries in recent years. Glass fiber high-temperature graphene flexible heating devices are a novel heating material created through a special process by organically combining glass fiber and graphene, then forming electrodes on the graphene. This material maintains a uniform and stable temperature distribution during heating, combining the excellent mechanical properties of glass fiber with the high thermal conductivity of graphene to provide efficient, uniform, and stable heating. However, due to the flexibility and deformability of flexible glass fiber cloth, the electrodes can deform after being fabricated on the heating plate due to the influence of the substrate, resulting in cracks or defects in the electrode layer. This leads to uncertainty in the conductivity and stability of the product electrodes, significantly affecting the quality of the heating plate. Summary of the Invention
[0003] In order to solve the above-mentioned problems, improve the conductivity and stability of the electrode, and ensure the quality of the high-temperature graphene flexible heating device, the present application provides a high-temperature graphene flexible heating device and a preparation method thereof.
[0004] The present application provides a high-temperature graphene flexible heating device and a preparation method thereof, which adopt the following technical solutions.
[0005] A high-temperature graphene flexible heating device comprises a substrate, a graphene layer is provided on the substrate, electrodes are provided on the surface of the graphene layer, and reinforcing ribs made of conductive material are provided inside the electrodes.
[0006] By adopting the above technical solution, by setting up reinforcing ribs and electrodes on the surface of the graphene layer, the conductivity and stability of the electrode can be guaranteed. Even if the heating device is bent and deformed, or cracks or defects occur in the electrode, the smooth transmission of current between the electrode and the graphene layer heating material can be ensured, thereby reducing resistance and energy loss, improving the overall conductive efficiency, and ensuring an efficient, uniform and stable heating effect.
[0007] Optionally, an anti-oxidation layer covers the graphene layer and the electrode.
[0008] By adopting the above technical solution and providing an anti-oxidation layer, the package is completed with a smooth surface, so that the electrode has higher durability and stability, thereby extending the service life of the heating device.
[0009] Optionally, graphene layers are provided on both the upper surface and the lower surface of the substrate, and there are two electrodes corresponding to the graphene layers.
[0010] By adopting the above technical solution, a double-layer heating structure of the upper and lower layers of the substrate is realized, thereby improving the heating efficiency of the heating device.
[0011] Optionally, the reinforcing ribs are in a linear or grid shape.
[0012] By adopting the above technical solution, the linear reinforcement rib structure is added to the electrode, which can significantly improve the overall rigidity and stability of the electrode. The linear reinforcement ribs can clearly define the flow path of the current, helping to optimize the current distribution and reduce the current concentration and local overheating. The unique geometry of the reinforcement rib structure, with its mesh-like shape, exhibits excellent performance in the electrode. It can effectively disperse the current, achieve a more uniform current distribution, reduce the current density, and reduce the hot spots and local damage caused by current concentration. It can also increase the active area by changing the morphology of the electrode surface, thereby improving the efficiency of the electrochemical reaction.
[0013] Optionally, the reinforcing ribs and the electrodes form a conductive electrode unit, the filling rate of the reinforcing ribs accounts for 10% to 50% of the entire conductive electrode unit, the electrode thickness is 1 to 500 um, and the width is 2 mm to 12 mm.
[0014] By adopting the above technical solution, the filling rate of the reinforcing ribs is between 10% and 50%. If the ratio is too small, the effect of the reinforcing ribs is not obvious, and if the ratio is too high, it will affect the stability of the electrode after spraying.
[0015] A method for preparing the high-temperature graphene flexible heating device as described above comprises the following steps:
[0016] Step 1: using a vacuum magnetron sputtering device to deposit graphene on a substrate to form a graphene layer;
[0017] Step 2: Fix the reinforcing ribs to the electrode area of the graphene layer;
[0018] Step 3: Prepare electrodes in the electrode area of the graphene layer and form a conductive electrode unit with the reinforcing ribs to complete the production of the heating device.
[0019] Optionally, the substrate is pretreated before step 1, including cleaning and surface activation.
[0020] By adopting the above technical solution, the substrate is cleaned and the surface is activated to ensure the cleanliness and activity of the substrate surface, thereby enhancing the bonding between the graphene and the substrate.
[0021] Optionally, the specific process of the step 2, fixing the reinforcing rib to the electrode region of the graphene layer by a clamp, includes the following steps:
[0022] S1, placing the substrate on which the graphene layer is formed by depositing graphene in step 1 in the groove position of the lower fixture;
[0023] S2. Fix the reinforcing ribs on the fixing column of the lower fixture;
[0024] S3. Use the upper clamp to press and fix the base and the reinforcement to complete the reinforcement fixation;
[0025] The specific process of step three, preparing the electrode in the electrode area of the graphene layer, is as follows: spraying the electrode material on the hollow position of the upper fixture, covering and fixing the reinforcing ribs; and completing the production of the heating device.
[0026] Optionally, in step 4, an anti-oxidation layer is deposited on the heating device using a vacuum magnetron sputtering or magnetron sputtering evaporation integrated machine.
[0027] By adopting the above technical solution and providing the anti-oxidation layer, the anti-oxidation performance of the heating device is improved, especially preventing oxidation and decay failure during high-temperature use.
[0028] Optionally, the clamp includes a lower clamp and an upper clamp close to each other, a plurality of positioning columns are provided on the lower clamp, and a plurality of positioning holes cooperating with the positioning columns are provided on the upper clamp; a groove is provided on the lower clamp, the groove is used to place the base, and fixing columns are provided on the lower clamp on opposite sides of the groove, and the fixing columns are used to fix the reinforcing ribs; avoidance holes are provided on the upper clamp at positions corresponding to the fixing columns, and electrode covering holes are provided in the area where the fixing columns on both sides of the base are connected on the upper clamp.
[0029] By adopting the above technical solution and using a clamp, the reinforcing ribs and the base can be quickly clamped and fixed so that the two positions are relatively fixed, which is conducive to the preparation of the electrode. In addition, the clamp has a simple structure and is easy to operate, which is conducive to improving production efficiency and quality.
[0030] In summary, this application has at least the following beneficial effects:
[0031] 1. The present application adopts the above-mentioned technical solution and arranges reinforcing ribs and electrodes on the surface of the graphene layer to ensure the conductivity and stability of the electrode. Even if the heating device is bent and deformed, or cracks or defects occur in the electrode, it can ensure smooth transmission of current between the electrode and the graphene layer heating material, reduce resistance and energy loss, improve the overall conductive efficiency, and ensure efficient, uniform and stable heating effect.
[0032] 2. The reinforcing ribs of the present application are linear in shape. By adding a linear reinforcing rib structure to the electrode, the overall rigidity and stability of the electrode can be significantly improved; the linear reinforcing ribs can clearly define the flow path of the current, help optimize the current distribution, and reduce the current concentration and local overheating.
[0033] 3. The reinforcing ribs of the present application are in a grid shape. The reinforcing rib structure exhibits excellent performance effects in the electrode due to its unique geometric shape; it can effectively disperse the current, achieve a more uniform current distribution, reduce the current density, and reduce hot spots and local damage caused by current concentration. It can increase its active area by changing the morphology of the electrode surface, thereby improving the efficiency of the electrochemical reaction.
[0034] 4. This application provides an anti-oxidation layer and a flat surface for the package, which makes the electrode more durable and stable, especially preventing oxidation and decay failure during high-temperature use, thereby extending the service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0036] Figure 1 This is a schematic diagram of the cross-sectional structure of a high-temperature graphene flexible heating device in Example 1.
[0037] Figure 2 This is a structural schematic diagram of a high-temperature graphene flexible heating device (excluding the anti-oxidation layer) in Example 1.
[0038] Figure 3 This is a schematic diagram of the end face structure of a high-temperature graphene flexible heating device (excluding the anti-oxidation layer) in Example 1.
[0039] Figure 4 yes Figure 3 Schematic diagram of the cross-sectional structure along the section line AA.
[0040] Figure 5 This is a schematic structural diagram of a high-temperature graphene flexible heating device (excluding the anti-oxidation layer) in Example 2.
[0041] Figure 6 This is a schematic diagram of the end face structure of a high-temperature graphene flexible heating device (excluding the anti-oxidation layer) in Example 2.
[0042] Figure 7 yes Figure 6 Schematic diagram of the cross-sectional structure along section line BB.
[0043] Figure 8 This is a schematic structural diagram of a high-temperature graphene flexible heating device (excluding the anti-oxidation layer) in Example 3.
[0044] Figure 9 This is a schematic diagram of the end face structure of a high-temperature graphene flexible heating device (excluding the anti-oxidation layer) in Example 3.
[0045] Figure 10 yes Figure 9 Schematic diagram of the cross-sectional structure along the section line CC.
[0046] Figure 11 This is a schematic structural diagram of a high-temperature graphene flexible heating device (excluding the anti-oxidation layer) in Example 4.
[0047] Figure 12 This is a schematic diagram of the end face structure of a high-temperature graphene flexible heating device (excluding the anti-oxidation layer) in Example 4.
[0048] Figure 13 yes Figure 12 Schematic diagram of the cross-sectional structure along the section line DD.
[0049] Figure 14 This is a process flow chart of a method for preparing a high-temperature graphene flexible heating device in Example 1, Example 2, Example 3, and Example 4.
[0050] Figure 15 It is a schematic diagram of the fixture structure in Example 5.
[0051] Figure 16 It is a schematic diagram of the lower clamp structure in Example 5.
[0052] Figure 17 It is a schematic diagram of the upper clamp structure in Example 5.
[0053] Figure 18 This is a structural diagram of the base and reinforcing ribs fixed on the lower fixture in Example 5.
[0054] Figure 19 This is a schematic diagram of the structure of the clamp after clamping in Example 5.
[0055] Explanation of the accompanying symbols: 1. substrate; 2. graphene layer; 3. reinforcing rib; 4. electrode; 5. anti-oxidation layer; 6. lower clamp; 7. upper clamp; 8. positioning column; 9. positioning hole; 10. groove; 11. fixing column; 12. avoidance hole; 13. electrode covering hole. DETAILED DESCRIPTION
[0056] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0057] The following is combined with Figures 1 to 19 This application is described in further detail.
[0058] The embodiments of the present application disclose a high-temperature graphene flexible heating device and a preparation method thereof.
[0059] Example 1: Reference Figure 1 、 2 , 3, 4, 14, a high-temperature graphene flexible heating device, comprising:
[0060] The substrate 1 includes a glass fiber cloth material. The glass fiber cloth has a certain flexibility and deformation ability, which makes the heating device have excellent local mechanical properties, can resist external stress and deformation, and improves the durability and stability of the heating device. Other fiber cloth materials can also be used.
[0061] A graphene layer 2 is provided on the substrate 1, and the graphene layer 2 is provided on both the upper and lower surfaces of the substrate 1, realizing an upper and lower double-layer heating structure of the substrate 1, thereby improving the heating efficiency of the heating device.
[0062] Two electrodes 4 are disposed on the outer edges of the graphene layer 2, each having a rectangular cross-section. Ribs 3 made of conductive material are disposed within the electrodes 4, forming a conductive electrode unit. The ribs 3 are linear and include multiple ribs. Adding linear ribs to the electrode significantly improves its overall rigidity and stability. These ribs clearly define the current flow path, helping to optimize current distribution and reduce current concentration and localized overheating. Both the ribs 3 and electrodes 4 are made of materials such as tungsten, molybdenum, copper, zirconium, titanium, rhenium, iron-chromium-aluminum, or alloys of two of these materials. The ribs 3 are present in an amount between 10% and 50% of the total conductive electrode unit. A smaller percentage results in insignificant reinforcement effects, while a higher percentage can compromise stability after electrode sputtering. The electrodes are 1 to 500 μm thick and 2 to 12 mm wide.
[0063] The anti-oxidation layer 5 covers the graphene layer 2 and the electrode 4. Through the provision of the anti-oxidation layer 5, the surface of the package is flattened, so that the electrode has higher durability and stability, and the service life of the heating device is extended.
[0064] Reference Figure 1 、 2, 3, 4, 14, a method for preparing a high-temperature graphene flexible heating device, comprising the following steps:
[0065] Step 1: using a vacuum magnetron sputtering device to deposit graphene on a substrate 1 to form a graphene layer 2;
[0066] First, the substrate 1 is pretreated, including cleaning and surface activation, to ensure the cleanliness and activity of the substrate 1 surface, thereby enhancing the bonding between the graphene and the substrate 1. Then, the pretreated substrate 1 is deposited on the substrate 1 using a vacuum magnetron sputtering device in a roll-to-roll manner to form a graphene layer 2. By precisely controlling the sputtering parameters, the graphene layer 2 is ensured to be evenly and tightly covered on the surface of the base layer. The vacuum degree is controlled at 1.0x10 -2 pa to 4.0x10 -4 The sputtering power is controlled within 10 to 20 kW (adjustable according to required deposition thickness).
[0067] Step 2: Fix the reinforcing rib 3 to the electrode area of the graphene layer 2;
[0068] A special fixing fixture is used to fix and flatten the wire-shaped reinforcement rib 3 material in the electrode area of the base layer. The size of the wire can be set according to the product's overcurrent, power, and temperature requirements.
[0069] The fixing of the reinforcement rib 3 specifically includes the following steps:
[0070] S1, placing the substrate 1 on which the graphene layer 2 is formed by depositing graphene in step 1, at the position of the groove 10 of the lower fixture 6;
[0071] S2. Fix the two ends of the reinforcing rib 3 to the fixing columns 11 of the lower fixture 6;
[0072] S3. Use the upper clamp 7 to press and fix the base 1 and the reinforcing rib 3 to complete the fixation of the reinforcing rib 3.
[0073] Step 3: preparing an electrode 4 in the electrode region of the graphene layer 2;
[0074] Electrode material is sprayed on the hollowed position of the upper fixture 7 to cover and fix the reinforcing rib 3; and the heating device is completed.
[0075] Electrode material is prepared in the electrode area of the base layer by spraying or brazing to form electrode 4. The electrode is fully combined and fixed with graphene through the spraying / brazing process to form an electrode. The electrode specifications can be set according to the product overcurrent, power, and temperature requirements.
[0076] Step 4: Use vacuum magnetron sputtering or magnetron sputtering evaporation machine to coat the anti-oxidation layer 5 on the heating device made in step 3 to complete the heating device. The vacuum degree is controlled at 1.0x10 -2 pa to 4.0x10-4 pa, the sputtering power supply is controlled at 10 to 20KW (the deposition thickness can be adjusted according to the requirements), the anti-oxidation layer 5 is made of aluminum oxide, hexagonal boron nitride, and aluminum silicate. Aluminum oxide, hexagonal boron nitride, and aluminum silicate materials have the advantages of good high temperature resistance, high thermal conductivity, insulation, and high mechanical strength. They can protect the graphene layer 2 from oxidation and decay failure during high-temperature use; the thickness of the anti-oxidation layer 5 is 28nm to 1000nm.
[0077] After the device is completed, it needs to be tested. The test of the heating device:
[0078] (1) Conductivity test:
[0079] DC resistance: Use a DC resistance instrument to test, the test data is 100 to 500mΩ
[0080] Sheet resistance: Tested using an ST2253 four-probe square resistance meter, the test data is <20mΩ
[0081] (2) Oxidation resistance test: The device can maintain effective use time of more than 5000 hours in an environment with a high temperature of less than 1000℃.
[0082] (3) High temperature resistance test: Use a high temperature resistance tester to test, the temperature resistance is within 1000℃.
[0083] (4) Insulation test: Use insulation withstand voltage tester to test, the insulation data is 3 to 3.6KV.
[0084] After preparation, qualified products undergo necessary post-processing, such as vacuum packaging, to ensure the product is safe for transportation and storage.
[0085] The high-temperature graphene flexible heating device produced by the technical solution of the present application includes a linear reinforcing rib 3 material in the electrode 4, which improves the problem that the electrode 4 is deformed by the influence of the substrate after being prepared on the heating plate, and cracks or defects appear in the electrode layer; a good conductive connection is formed between the pre-embedded linear reinforcing rib 3 conductive material and the electrode 4, and this connection ensures the smooth transmission of current between the electrode 4 and the heating material, reduces resistance and energy loss, and improves the overall conductive efficiency; the internal pre-embedded reinforcing rib 3 and the electrode 4 form a combination of pre-embedded conductive material and electrode, which increases the strength of the entire conductive electrode unit structure. The reinforced structure can resist external stress and deformation, ensure efficient, uniform and stable heating effect, and improve the durability and stability of the product.
[0086] Example 2: Reference Figure 5 、 6 7.14. A high-temperature graphene flexible heating device comprising:
[0087] The substrate 1 includes a glass fiber cloth material. The glass fiber cloth has a certain flexibility and deformation ability, which makes the heating device have excellent local mechanical properties, can resist external stress and deformation, and improves the durability and stability of the heating device. Other fiber cloth materials can also be used.
[0088] A graphene layer 2 is provided on the substrate 1, and the graphene layer 2 is provided on both the upper and lower surfaces of the substrate 1, realizing an upper and lower double-layer heating structure of the substrate 1, thereby improving the heating efficiency of the heating device.
[0089] Two electrodes 4 are provided at the edges of the outer surface of the graphene layer 2, and the cross-section of the electrodes 4 is rectangular. Ribs 3 made of conductive material are provided within the electrodes 4, and the ribs 3 and the electrodes 4 form a conductive electrode unit. The ribs 3 are in a grid-like shape, forming a circular hole-type grid electrode sheet. The circular hole-type rib structure added to the electrode has a unique geometric shape that can increase the active area by changing the morphology of the electrode surface, thereby improving the efficiency of the electrochemical reaction and exhibiting excellent performance in the electrode. The circular holes can effectively disperse the current, achieving a more uniform current distribution, reducing the current density, and reducing hot spots and local damage caused by current concentration. The materials of the ribs 3 and electrodes 4 both include tungsten, molybdenum, copper, zirconium, titanium, rhenium, iron, chromium, and aluminum, or alloys of two of these materials. The filling rate of the ribs 3 accounts for 10% to 50% of the total conductive electrode material. If the proportion is too small, the rib effect is not obvious, and if the proportion is too high, the stability of the electrode after spraying will be affected. The electrode thickness is 1 to 500 μm and the width is 2 mm to 12 mm.
[0090] The anti-oxidation layer 5 covers the graphene layer 2 and the electrode 4. Through the provision of the anti-oxidation layer 5, the surface of the package is flattened, so that the electrode has higher durability and stability, and the service life of the heating device is extended.
[0091] Reference Figure 5 、 6 7.14. A method for preparing a high-temperature graphene flexible heating device, comprising the following steps:
[0092] Step 1: using a vacuum magnetron sputtering device to deposit graphene on a substrate 1 to form a graphene layer 2;
[0093] First, the substrate 1 is pretreated, including cleaning and surface activation, to ensure the cleanliness and activity of the substrate 1 surface, thereby enhancing the bonding between the graphene and the substrate 1. Then, the pretreated substrate 1 is deposited on the substrate 1 using a vacuum magnetron sputtering device in a roll-to-roll manner to form a graphene layer 2. By precisely controlling the sputtering parameters, the graphene layer 2 is ensured to be evenly and tightly covered on the surface of the base layer. The vacuum degree is controlled at 1.0x10 -2 pa to 4.0x10 -4The sputtering power is controlled within 10 to 20 kW (adjustable according to required deposition thickness).
[0094] Step 2: Fix the reinforcing rib 3 to the electrode area of the graphene layer 2;
[0095] A special fixing fixture is used to fix and flatten the grid-shaped reinforcement rib 3 material in the electrode area of the base layer. The size of the wire body can be set according to the product's overcurrent, power, and temperature requirements.
[0096] The fixing of the reinforcement rib 3 specifically includes the following steps:
[0097] S1, placing the substrate 1 on which the graphene layer 2 is formed by depositing graphene in step 1, at the position of the groove 10 of the lower fixture 6;
[0098] S2. Fix the two ends of the reinforcing rib 3 to the fixing columns 11 of the lower fixture 6;
[0099] S3. Use the upper clamp 7 to press and fix the base and the reinforcing rib 3 to complete the fixation of the reinforcing rib 3.
[0100] Step 3: preparing an electrode 4 in the electrode region of the graphene layer 2;
[0101] Electrode material is sprayed on the hollowed position of the upper fixture 7 to cover and fix the reinforcing rib 3; and the heating device is completed.
[0102] Electrode material is prepared in the electrode area of the base layer by spraying or brazing to form electrode 4. The electrode is fully combined and fixed with graphene through the spraying / brazing process to form an electrode. The electrode specifications can be set according to the product overcurrent, power, and temperature requirements.
[0103] Step 4: Use vacuum magnetron sputtering or magnetron sputtering evaporation machine to coat the anti-oxidation layer 5 on the heating device made in step 3 to complete the heating device. The vacuum degree is controlled at 1.0x10 -2 pa to 4.0x10 -4 pa, the sputtering power supply is controlled at 10 to 20KW (the deposition thickness can be adjusted according to the requirements), the anti-oxidation layer 5 is made of aluminum oxide, hexagonal boron nitride, and aluminum silicate. Aluminum oxide, hexagonal boron nitride, and aluminum silicate materials have the advantages of good high temperature resistance, high thermal conductivity, insulation, and high mechanical strength. They can protect the graphene layer 2 from oxidation and decay failure during high-temperature use; the thickness of the anti-oxidation layer 5 is 28nm to 1000nm.
[0104] After the device is completed, it needs to be tested. The test of the heating device:
[0105] (1) Conductivity test:
[0106] DC resistance: Use a DC resistance instrument to test, the test data is 100 to 500mΩ
[0107] Sheet resistance: Tested using an ST2253 four-probe square resistance meter, the test data is <20mΩ
[0108] (2) Oxidation resistance test: The product can maintain effective use time of more than 5000 hours in high temperature environment within 1000℃.
[0109] (3) High temperature resistance test: Use a high temperature resistance tester to test, the product can withstand temperatures within 1000℃.
[0110] (4) Insulation test: Use insulation withstand voltage tester to test, the product insulation data is 3 to 3.6KV.
[0111] After preparation, qualified products undergo necessary post-processing, such as vacuum packaging, to ensure the product is safe for transportation and storage.
[0112] The high-temperature graphene flexible heating device produced by the technical solution of the present application includes a linear reinforcing rib 3 material in the electrode 4, which improves the problem that the electrode 4 is deformed by the influence of the substrate after being prepared on the heating plate, and cracks or defects appear in the electrode layer; a good conductive connection is formed between the pre-embedded linear reinforcing rib 3 conductive material and the electrode 4, and this connection ensures the smooth transmission of current between the electrode 4 and the heating material, reduces resistance and energy loss, and improves the overall conductive efficiency; the internal pre-embedded reinforcing rib 3 and the electrode 4 form a combination of pre-embedded conductive material and electrode, which increases the strength of the entire conductive electrode unit structure. The reinforced structure can resist external stress and deformation, ensure efficient, uniform and stable heating effect, and improve the durability and stability of the product.
[0113] Example 3: Refer to Example 2, refer to Figure 8 、 9 , 10, 14, the reinforcement rib 3 is in a grid shape, which is a grid-shaped electrode sheet with hexagonal holes. The hexagonal hole reinforcement rib structure shows excellent performance in the electrode due to its unique geometric shape; the hexagonal holes can effectively disperse the current, achieve a more uniform current distribution, reduce the current density, and reduce hot spots and local damage caused by current concentration.
[0114] Example 4: Refer to Example 2, refer to Figure 11 、 12 , 13, 14, the reinforcing rib 3 is in a grid shape, which is a square-hole grid electrode sheet. Adding a square-hole reinforcing rib structure to the electrode can increase its active area by changing the morphology of the electrode surface, thereby improving the electrochemical reaction efficiency; the square-hole reinforcing rib also helps to optimize the flow path of the current, make the current distribution more uniform, and reduce local damage caused by excessive current density.
[0115] Example 5: Referring to the above embodiment, Figure 15-19 , the special fixing fixtures mentioned above include:
[0116] The lower clamp 6 and the upper clamp 7 are close to each other, and both are rectangular plates. A plurality of positioning posts 8 are provided on the lower clamp 6. Four positioning posts 8 are provided and distributed near the four corners of the lower clamp 6. A plurality of positioning holes 9 cooperating with the positioning posts 8 are provided on the upper clamp 7.
[0117] A groove 10 is provided on the lower clamp 6, and the groove 10 is used to place the base 1. Fixed columns 11 are provided on the lower clamp 6 on opposite sides of the groove 10, and the fixed columns 11 are used to fix the reinforcing rib 3 by binding or the like. The fixed columns 11 on opposite sides of the groove 10 respectively fix the two ends of the reinforcing rib 3 to complete the fixation of the reinforcing rib 3 on the base 1.
[0118] An avoidance hole 12 is opened at the position corresponding to the fixed column 11 on the upper clamp 7, and an electrode covering hole 13 is opened in the area where the fixed columns 11 on both sides of the base 1 are connected, forming a hollow design of the upper clamp 7, that is, the electrode area is formed on the base 1 corresponding to the reinforcement area on the base 1, which is convenient for preparing the electrode 4 in the electrode area, that is, spraying the electrode material on the hollow position of the upper clamp 7.
[0119] By using the clamp, the reinforcing rib 3 and the base 1 can be quickly clamped and fixed so that the two positions are relatively fixed, which is conducive to the preparation of the electrode 4. In addition, the clamp has a simple structure and is easy to operate, which is conducive to improving production efficiency and quality.
[0120] In the description of the present invention, it should be understood that the terms "upper", "lower", "outer", "both sides", "two ends" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention. In the description of the present invention, unless otherwise specified and limited, it should be noted that the term "connection" should be understood in a broad sense, for example, it can be a mechanical connection or an electrical connection, or it can be the internal communication of two elements, it can be a direct connection, or it can be an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to the specific circumstances.
[0121] The above are only preferred embodiments of the invention and are not intended to limit the invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the invention should be included in the scope of protection of the invention.
Claims
1. A method for preparing a high-temperature graphene flexible heating device, It is characterized in that The high-temperature graphene flexible heating device comprises a substrate (1), a graphene layer (2) is arranged on the substrate (1), an electrode (4) is arranged on the surface of the graphene layer (2), and a reinforcing rib (3) made of a conductive material is arranged inside the electrode (4); The preparation method comprises the following steps: Step 1: using a vacuum magnetron sputtering device to deposit graphene on a substrate (1) to form a graphene layer (2); Step 2: fix the reinforcing rib (3) to the electrode region of the graphene layer (2); Step 3: preparing an electrode (4) in the electrode region of the graphene layer (2) and forming a conductive electrode unit with the reinforcing rib (3), thereby completing the production of the heating device; The specific process of the step 2, fixing the reinforcing rib (3) to the electrode region of the graphene layer (2) by means of a clamp, comprises the following steps: S1, placing the substrate (1) on which the graphene layer (2) is formed by depositing graphene in step 1, in the groove (10) of the lower fixture (6); S2, fixing the reinforcing rib on the fixing column (11) of the lower clamp (6); S3, using the upper clamp (7) to press and fix the base and the reinforcing ribs to complete the fixing of the reinforcing ribs; The specific process of step 3, preparing the electrode (4) in the electrode region of the graphene layer (2) is as follows: spraying the electrode material on the hollowed-out position of the upper fixture (7) to cover and fix the reinforcing ribs; and completing the production of the heating device; The clamp comprises a lower clamp (6) and an upper clamp (7) which are close to each other, a plurality of positioning columns (8) are provided on the lower clamp (6), and a plurality of positioning holes (9) which cooperate with the positioning columns (8) are provided on the upper clamp (7); a groove (10) is provided on the lower clamp (6), and the groove (10) is used to place the substrate (1); fixing columns (11) are provided on the lower clamp (6) on opposite sides of the groove (10), and the fixing columns (11) are used to fix the reinforcing ribs (3); avoidance holes (12) are provided on the upper clamp (7) at positions corresponding to the fixing columns (11), and electrode covering holes (13) are provided in the upper clamp (7) at the position area corresponding to the connection position of the fixing columns (11) on both sides of the substrate (1).
2. A method for preparing a high-temperature graphene flexible heating device according to claim 1, It is characterized in that The anti-oxidation layer (5) covers the graphene layer (2) and the electrode (4).
3. A method for preparing a high-temperature graphene flexible heating device according to claim 1, It is characterized in that The upper surface and the lower surface of the substrate (1) are both provided with a graphene layer (2), and there are two electrodes (4) corresponding to the graphene layer (2).
4. The method for preparing a high-temperature graphene flexible heating device according to claim 1, It is characterized in that The reinforcing ribs (3) are in a linear or grid shape.
5. The method for preparing a high-temperature graphene flexible heating device according to claim 1, It is characterized in that The reinforcing ribs (3) and the electrodes (4) form a conductive electrode unit, the filling rate of the reinforcing ribs (3) accounts for 10% to 50% of the entire conductive electrode unit, the electrode thickness is 1 to 500 um, and the width is 2 mm to 12 mm.
6. The method for preparing a high-temperature graphene flexible heating device according to claim 1, It is characterized in that Prior to step 1, the substrate (1) is pretreated, including cleaning and surface activation.
7. The method for preparing a high-temperature graphene flexible heating device according to claim 1, It is characterized in that Step 4: Use a vacuum magnetron sputtering or magnetron sputtering evaporation machine to coat an anti-oxidation layer (5) on the heating device.