A high-low temperature resistant and highly elastic ultra-thin cover material and a preparation method thereof

Through the combination of modified asphalt and modified basalt fibers, the high and low temperature stability and crack resistance of ultra-thin mask materials are improved, and the problems of insufficient performance and durability in the existing technology are solved, and high-temperature rut resistance and low temperature resistance are met. The crack resistance and durability requirements extend the service life of asphalt pavement.

CN118619592BActive Publication Date: 2024-11-12THE FOURTH ENG CO LTD OF CCCC FIRST HIGHWAY ENG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410790013.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-11-12
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

The existing ultra-thin cover repair materials cannot meet the requirements of high-temperature rutting resistance, low-temperature crack resistance and durability. The conventional thin-layer cover materials lack the performance and durability, which cannot meet the improvement of my country's road transportation needs.

Method used

Components based on weight include 90-95 parts of aggregate, 10-14 parts of modified asphalt, 3-5 parts of ore powder, 2-3 parts of modified basalt fibers, and modified molybdenum disulfide and modified basalt fibers. The preparation method of the material can improve the high and low temperature stability and mechanical properties, build a stable interpenetrating network system, and enhance the toughness and crack resistance of the material.

Benefits of technology

It has achieved the improvement of the high and low temperature stability and crack resistance of the material, significantly improved the service life of asphalt pavement and road traffic capacity, and met the requirements of high-temperature rutting resistance, low-temperature crack resistance and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004899734520000131
    Figure BDA0004899734520000131
Patent Text Reader

Abstract

This invention discloses a high- and low-temperature resistant, high-elasticity, ultra-thin overlay material and its preparation method. The invention first pretreats molybdenum disulfide with an aminosilane coupling agent to introduce amino groups onto the surface of molybdenum disulfide. Then, through a chemical reaction between amino and aldehyde groups, polyethyleneimine is grafted onto the surface of molybdenum disulfide to obtain modified molybdenum disulfide. Molybdenum disulfide exhibits high and low-temperature stability. Modification of molybdenum disulfide improves its dispersibility and compatibility in the organic phase of asphalt, thereby enhancing the high and low-temperature stability of the overlay material. Modified molybdenum disulfide can construct a stable interpenetrating network system in the asphalt system. Polyethyleneimine contains alkyl long-chain structures, which enhance the toughness of the material. Simultaneously, the unreacted amino groups in polyethyleneimine undergo cross-linking reactions with epoxy resin, further improving the overall mechanical properties of the asphalt, especially its toughness and low-temperature crack resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of asphalt overlay material preparation technology, specifically to a high- and low-temperature resistant, high-elasticity, ultra-thin overlay material and its preparation method. Background Technology

[0002] After asphalt pavement is built, even if the base layer has not suffered structural damage, the surface layer will often exhibit early defects of varying degrees, such as surface aging, loss of fine aggregate, spalling of coarse aggregate, potholes, and minor cracks, due to the combined influence of external factors such as vehicle load, temperature, and precipitation, as well as internal factors such as material properties and quality defects. These defects not only affect the road's traffic capacity, but more importantly, they greatly shorten the road's service life.

[0003] Asphalt overlay technology is an important road maintenance technique, primarily used to improve the quality of asphalt pavements, enhancing their waterproofing, skid resistance, and smoothness. After years of research and practice, ultra-thin overlay technology has gradually become a popular choice for asphalt pavement maintenance. This technology uses special asphalt materials and construction processes to reduce the asphalt layer thickness to one-third or even less of traditional asphalt pavements, while maintaining excellent road performance. Ultra-thin overlay technology uses high-performance asphalt and mineral aggregates, exhibiting excellent compressive strength, impermeability, and aging resistance, thus extending the service life of roads.

[0004] With the continuous growth of highway transportation demand in my country, the requirements for the performance of ultra-thin overlays, such as high-temperature rutting resistance, low-temperature crack resistance, water damage resistance and durability, are gradually increasing. Conventional thin-layer overlay repair materials cannot meet the requirements, and it is necessary to develop ultra-thin overlay repair materials with better performance and durability. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a high- and low-temperature resistant, high-elasticity, ultra-thin cover material and its preparation method.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] A high- and low-temperature resistant, high-elasticity, ultra-thin overlay material, comprising the following raw materials by weight: 90-95 parts aggregate, 10-14 parts modified bitumen, 3-5 parts mineral powder, and 2-3 parts modified basalt fiber.

[0008] Preferably, in some embodiments of the present invention, the aggregate can be selected as 90 parts, 91 parts, 92 parts, 93 parts, 94 parts, or 95 parts, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0009] More preferably, the aggregate comprises a first aggregate with a continuous gradation of 3-5 mm and a second aggregate with a continuous gradation of 0-3 mm, wherein the mass ratio of the first aggregate to the second aggregate is 6:4.

[0010] In this invention, the aggregate is selected from mineral aggregates, including basalt, granite, river pebbles or sea gravel.

[0011] Preferably, in some embodiments of the present invention, the modified bitumen can be selected as 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, or 15 parts, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0012] The method for preparing the modified asphalt is as follows:

[0013] S1. Molybdenum disulfide is ultrasonically dispersed in an aqueous ethanol solution, then an aminosilane coupling agent is added, the mixture is stirred and reacted, and then filtered, washed and dried to obtain pretreated molybdenum disulfide.

[0014] S2. Pretreated molybdenum disulfide is ultrasonically dispersed in deionized water, the pH of the solution is adjusted to 10-12, then polyethyleneimine and glutaraldehyde are added, the mixture is heated and stirred to react, and after the reaction is completed, it is filtered, washed and dried to obtain modified molybdenum disulfide.

[0015] S3. Heat the base asphalt to melt, then add modified molybdenum disulfide and epoxy resin, and shear and disperse evenly in a dispersing emulsifier to obtain modified asphalt.

[0016] Preferably, in step S1, the mass ratio of molybdenum disulfide to aminosilane coupling agent is 8-12:1-3. In some embodiments of the present invention, for example, 8:1, 8:2, 8:3, 10:1, 10:2, 10:3, 12:1, 12:2, 12:3 can be selected, but it is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0017] Preferably, the aminosilane coupling agent can be selected from KH550, Shin-Etsu KBM-573, or Dow Corning Z-6121.

[0018] Preferably, the mass fraction of the ethanol aqueous solution is 60-80%, such as 60%, 65%, 70%, 75%, 80%, but not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0019] Preferably, the stirring reaction time is 1-3 hours, for example, 1 hour, 2 hours, or 3 hours can be selected, but it is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0020] Preferably, in step S2, the mass ratio of pretreated molybdenum disulfide, polyethyleneimine, and glutaraldehyde is 5-10:4-8:6-8. In some embodiments of the present invention, for example, 5:4:6, 5:4:8, 5:8:8, 8:4:6, 8:8:8, 10:5:6, 10:5:8, and 10:8:8 can be selected, but the values ​​are not limited to those listed. Other unlisted values ​​within the range are also applicable.

[0021] Preferably, in step S2, the temperature of the heating and stirring reaction is 65-80℃, for example, 65℃, 70℃, 75℃, or 80℃ can be selected; the heating and stirring reaction time is 3-5h, for example, 3h, 4h, or 5h can be selected, but it is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0022] Preferably, in step S3, the mass ratio of the base asphalt, modified molybdenum disulfide, and epoxy resin is 80-90:4-8:10-15. In some embodiments of the present invention, for example, 80:4:10, 80:5:15, 85:5:10, 85:5:15, 90:4:10, 90:5:10, and 90:8:15 can be selected, but the values ​​are not limited to those listed. Other unlisted values ​​within the range are also applicable.

[0023] Preferably, in step S3, the melting temperature is 150-180℃.

[0024] Preferably, in step S3, the shearing speed is 4000-5000 r / min, and the shearing time is 1-3 h.

[0025] Preferably, in some embodiments of the present invention, the mineral powder can be selected as 3 parts, 3.5 parts, 4 parts, 4.5 parts, or 5 parts, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0026] Preferably, the mineral powder can be selected from quartz powder or limestone powder.

[0027] In this embodiment of the invention, the selected mineral powder is limestone powder with a particle size of 2-10 μm.

[0028] Preferably, in some embodiments of the present invention, the modified basalt fiber can be selected in the form of 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts, or 3 parts, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0029] The method for preparing the modified basalt fiber is as follows:

[0030] (1) Basalt fibers were ultrasonically dispersed in an ethanol aqueous solution, and then a vinyl silane coupling agent was added to it. The mixture was stirred for 1-3 hours, and then filtered, washed and dried to obtain pretreated basalt fibers.

[0031] (2) Disperse the pretreated basalt fiber in toluene solvent, then add octadeceneamine, N,N'-methylenebisacrylamide and benzoyl peroxide to it, stir and react at 60-80℃ for 2-4h, and after the reaction is completed, filter, wash and dry to obtain modified basalt fiber.

[0032] Preferably, in step (1), the mass ratio of basalt fiber to vinyl silane coupling agent is 5-10:1-3. For example, 5:1, 5:2, 5:3, 8:1, 8:2, 8:3, 10:1, 10:2, 10:3 can be selected, but not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0033] Preferably, the vinyl silane coupling agent can be vinyltrimethoxysilane or vinyltriethoxysilane.

[0034] Preferably, in step (1), the mass fraction of the ethanol aqueous solution is 60-80%.

[0035] Preferably, in step (2), the mass ratio of pretreated basalt fiber, octadeceneamine, N,N'-methylenebisacrylamide and benzoyl peroxide is 8-10:4-6:0.8-1:0.2-0.5.

[0036] The present invention also provides a method for preparing the above-mentioned high and low temperature resistant, high ductility and elasticity ultrathin cover material, comprising the following steps: weighing each raw material according to the weight parts, mixing the aggregate and mineral powder evenly and heating to 150-180℃, then adding modified basalt fiber and stirring for 30-60s, then adding modified asphalt and stirring at 150-180℃ for 3-5min, and molding the specimen at this temperature to obtain the high and low temperature resistant, high ductility and elasticity ultrathin cover material.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) In this invention, molybdenum disulfide is first pretreated with an aminosilane coupling agent to introduce amino groups on the surface of molybdenum disulfide. Then, through the chemical reaction of amino groups and aldehyde groups, polyethyleneimine is grafted onto the surface of molybdenum disulfide to obtain modified molybdenum disulfide. Molybdenum disulfide has high and low temperature stability. By modifying molybdenum disulfide, the dispersibility and compatibility of molybdenum disulfide in the organic phase of asphalt are improved, thereby improving the high and low temperature stability of the overlay material. Modified molybdenum disulfide can construct a stable interpenetrating network system in the asphalt system. Polyethyleneimine contains alkyl long-chain structures, which can enhance the toughness of the material. At the same time, the unreacted amino groups in polyethyleneimine undergo cross-linking reaction with epoxy resin, further improving the overall mechanical properties of asphalt, especially toughness and low temperature crack resistance.

[0039] (2) In this invention, octadeceneamine is used to modify basalt fibers. The modified basalt fibers contain amino groups, which can adsorb modified asphalt through hydrogen bonding. The modified basalt fibers act as a stabilizer, which improves the bonding force between the modified asphalt and aggregates and mineral powder, and improves the mechanical properties of the overlay material. In addition, the modified basalt fibers and modified asphalt work together to prevent the further development of microcracks, so that the overlay material has excellent crack resistance and durability. Detailed Implementation

[0040] The present invention will be further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.

[0041] It should be noted that, unless otherwise specified, all chemical reagents involved in this invention were purchased through commercial channels.

[0042] The aggregate used in this invention is river pebbles, composed of a first aggregate with a continuous gradation of 3-5 mm and a second aggregate with a continuous gradation of 0-3 mm, wherein the mass ratio of the first aggregate to the second aggregate is 6:4; the base asphalt is 70# base asphalt; the CAS number of molybdenum disulfide is 1317-33-5, and the mesh size is 100 mesh; the relative molecular mass of polyethyleneimine is 3000; the epoxy resin is bisphenol A type epoxy resin E51; the mineral powder is limestone powder with a particle size of 2-10 μm; the basalt fiber is purchased from Jiangxi Shuobang New Material Technology Co., Ltd.; and the CAS number of octadeceneamine is 112-90-3.

[0043] Example 1

[0044] A method for preparing a high- and low-temperature resistant, high-elasticity, ultrathin cover material includes the following steps:

[0045] After mixing 90 parts of aggregate and 3 parts of mineral powder evenly, heat to 180℃, then add 3 parts of modified basalt fiber and stir for 45 seconds. Then add 10 parts of modified asphalt and stir at 180℃ for 4 minutes. The specimen is then formed at this temperature to obtain a high-temperature and low-temperature resistant, high-elasticity, ultra-thin cover material.

[0046] The preparation method of modified asphalt is as follows:

[0047] S1. Disperse 8g of molybdenum disulfide ultrasonically in 100mL of 80wt% ethanol aqueous solution, then add 1g of silane coupling agent KH550, stir at room temperature for 2h, and then filter, wash and dry to obtain pretreated molybdenum disulfide.

[0048] S2. Disperse 5g of pretreated molybdenum disulfide in 100mL of deionized water using ultrasound, adjust the pH of the solution to 10, then add 4g of polyethyleneimine and 6g of glutaraldehyde, heat and stir at 65℃ for 5h, and after the reaction is complete, filter, wash and dry to obtain modified molybdenum disulfide.

[0049] S3. Heat 80g of base asphalt to melt at a melting temperature of 180℃, then add 4g of modified molybdenum disulfide and 10g of epoxy resin. Shear and disperse evenly in a dispersing emulsifier at a speed of 4000r / min for 2h to obtain modified asphalt.

[0050] The preparation method of modified basalt fiber is as follows:

[0051] (1) 5g of basalt fiber was ultrasonically dispersed in 100mL of 80wt% ethanol aqueous solution, and then 1g of vinyltrimethoxysilane was added to it. The mixture was stirred at room temperature for 2h, and then filtered, washed and dried to obtain pretreated basalt fiber.

[0052] (2) Disperse 8g of pretreated basalt fiber in 100mL of toluene solvent, then add 4g of octadeceneamine, 0.8g of N,N'-methylenebisacrylamide and 0.2g of benzoyl peroxide to it, stir and react at 60℃ for 4h, and after the reaction is completed, filter, wash and dry to obtain modified basalt fiber.

[0053] Example 2

[0054] A method for preparing a high- and low-temperature resistant, high-elasticity, ultrathin cover material includes the following steps:

[0055] After mixing 92 parts of aggregate and 5 parts of mineral powder evenly, heat to 175℃, then add 2 parts of modified basalt fiber and stir for 60s. Then add 14 parts of modified asphalt and stir at 175℃ for 5min. The specimen is then formed at this temperature to obtain a high-temperature and low-temperature resistant, high-elasticity, ultra-thin cover material.

[0056] The preparation method of modified asphalt is as follows:

[0057] S1. 12g of molybdenum disulfide was ultrasonically dispersed in 100mL of 80wt% ethanol aqueous solution, and then 3g of silane coupling agent KH550 was added. The mixture was stirred at room temperature for 2h, and then filtered, washed and dried to obtain pretreated molybdenum disulfide.

[0058] S2. Disperse 5g of pretreated molybdenum disulfide in 100mL of deionized water using ultrasound, adjust the pH of the solution to 10, then add 6g of polyethyleneimine and 6g of glutaraldehyde, heat and stir at 80℃ for 3h, and after the reaction is complete, filter, wash and dry to obtain modified molybdenum disulfide.

[0059] S3. Heat 90g of base asphalt to melt at a melting temperature of 180℃, then add 8g of modified molybdenum disulfide and 15g of epoxy resin. Shear and disperse evenly in a dispersing emulsifier at a speed of 4500r / min for 2h to obtain modified asphalt.

[0060] The preparation method of modified basalt fiber is as follows:

[0061] (1) 10g of basalt fiber was ultrasonically dispersed in 100mL of 80wt% ethanol aqueous solution, and then 3g of vinyltrimethoxysilane was added to it. The mixture was stirred at room temperature for 2h, and then filtered, washed and dried to obtain pretreated basalt fiber.

[0062] (2) Disperse 10g of pretreated basalt fiber in 100mL of toluene solvent, then add 6g of octadeceneamine, 1g of N,N'-methylenebisacrylamide and 0.5g of benzoyl peroxide to it, stir and react at 80℃ for 2h, and after the reaction is completed, filter, wash and dry to obtain modified basalt fiber.

[0063] Example 3

[0064] A method for preparing a high- and low-temperature resistant, high-elasticity, ultrathin cover material includes the following steps:

[0065] After mixing 95 parts of aggregate and 4 parts of mineral powder evenly, heat to 180℃, then add 2.5 parts of modified basalt fiber and stir for 60s. Then add 12 parts of modified asphalt and stir at 180℃ for 5min. The specimen is then formed at this temperature to obtain a high-temperature and low-temperature resistant, high-elasticity, ultra-thin cover material.

[0066] The preparation method of modified asphalt is as follows:

[0067] S1. 10g of molybdenum disulfide was ultrasonically dispersed in 100mL of 80wt% ethanol aqueous solution, and then 2g of silane coupling agent KH550 was added. The mixture was stirred at room temperature for 2h, and then filtered, washed and dried to obtain pretreated molybdenum disulfide.

[0068] S2. Disperse 10g of pretreated molybdenum disulfide in 100mL of deionized water using ultrasound, adjust the pH of the solution to 10, then add 6g of polyethyleneimine and 8g of glutaraldehyde, heat and stir at 70℃ for 4h, and after the reaction is complete, filter, wash and dry to obtain modified molybdenum disulfide.

[0069] S3. Heat 85g of base asphalt to melt at a melting temperature of 180℃, then add 6g of modified molybdenum disulfide and 12g of epoxy resin. Shear and disperse evenly in a dispersing emulsifier at a speed of 4500r / min for 2h to obtain modified asphalt.

[0070] The preparation method of modified basalt fiber is as follows:

[0071] (1) 8g of basalt fiber was ultrasonically dispersed in 100mL of 80wt% ethanol aqueous solution, and then 2g of vinyltrimethoxysilane was added to it. The mixture was stirred at room temperature for 2h, and then filtered, washed and dried to obtain pretreated basalt fiber.

[0072] (2) Disperse 10g of pretreated basalt fiber in 100mL of toluene solvent, then add 5g of octadeceneamine, 0.8g of N,N'-methylenebisacrylamide and 0.4g of benzoyl peroxide to it, stir and react at 70℃ for 3h, and after the reaction is completed, filter, wash and dry to obtain modified basalt fiber.

[0073] Example 4

[0074] A method for preparing a high- and low-temperature resistant, high-elasticity, ultrathin cover material includes the following steps:

[0075] After mixing 93 parts of aggregate and 5 parts of mineral powder evenly, heat to 175℃, then add 2.8 parts of modified basalt fiber and stir for 60s. Then add 10 parts of modified asphalt and stir at 175℃ for 5min. The specimen is then formed at this temperature to obtain a high-temperature and low-temperature resistant, high-elasticity, ultra-thin cover material.

[0076] The preparation method of modified asphalt is as follows:

[0077] S1. 10g of molybdenum disulfide was ultrasonically dispersed in 100mL of 80wt% ethanol aqueous solution, and then 3g of silane coupling agent KH550 was added. The mixture was stirred at room temperature for 2h, and then filtered, washed and dried to obtain pretreated molybdenum disulfide.

[0078] S2. 10g of pretreated molybdenum disulfide was ultrasonically dispersed in 100mL of deionized water, the pH of the solution was adjusted to 10, and then 8g of polyethyleneimine and 8g of glutaraldehyde were added. The mixture was heated and stirred at 80℃ for 4h. After the reaction was completed, the modified molybdenum disulfide was obtained by filtration, washing and drying.

[0079] S3. Heat 88g of base asphalt to melt at a melting temperature of 180℃, then add 6g of modified molybdenum disulfide and 14g of epoxy resin. Shear and disperse evenly in a dispersing emulsifier at a speed of 4500r / min for 2h to obtain modified asphalt.

[0080] The preparation method of modified basalt fiber is as follows:

[0081] (1) 6g of basalt fiber was ultrasonically dispersed in 100mL of 80wt% ethanol aqueous solution, and then 2g of vinyltrimethoxysilane was added to it. The mixture was stirred at room temperature for 2h, and then filtered, washed and dried to obtain pretreated basalt fiber.

[0082] (2) Disperse 9g of pretreated basalt fiber in 100mL of toluene solvent, then add 6g of octadeceneamine, 0.8g of N,N'-methylenebisacrylamide and 0.5g of benzoyl peroxide to it, stir and react at 70℃ for 4h, and after the reaction is completed, filter, wash and dry to obtain modified basalt fiber.

[0083] Comparative Example 1

[0084] A method for preparing a high- and low-temperature resistant, high-elasticity, ultrathin cover material includes the following steps:

[0085] After mixing 90 parts of aggregate and 3 parts of mineral powder evenly, heat to 180℃, then add 3 parts of modified basalt fiber and stir for 45 seconds. Then add 10 parts of modified asphalt and stir at 180℃ for 4 minutes. The specimen is then formed at this temperature to obtain a high-temperature and low-temperature resistant, high-elasticity, ultra-thin cover material.

[0086] The preparation method of modified asphalt is as follows:

[0087] S1. Disperse 8g of molybdenum disulfide ultrasonically in 100mL of 80wt% ethanol aqueous solution, then add 1g of silane coupling agent KH550, stir at room temperature for 2h, and then filter, wash and dry to obtain pretreated molybdenum disulfide.

[0088] S2. Heat 80g of base asphalt to melt at a melting temperature of 180℃, then add 4g of pretreated molybdenum disulfide and 10g of epoxy resin. Shear and disperse evenly in a dispersing emulsifier at a speed of 4000r / min for 2h to obtain modified asphalt.

[0089] The preparation method of modified basalt fiber is as follows:

[0090] (1) 5g of basalt fiber was ultrasonically dispersed in 100mL of 80wt% ethanol aqueous solution, and then 1g of vinyltrimethoxysilane was added to it. The mixture was stirred at room temperature for 2h, and then filtered, washed and dried to obtain pretreated basalt fiber.

[0091] (2) Disperse 8g of pretreated basalt fiber in 100mL of toluene solvent, then add 4g of octadeceneamine, 0.8g of N,N'-methylenebisacrylamide and 0.2g of benzoyl peroxide to it, stir and react at 60℃ for 4h, and after the reaction is completed, filter, wash and dry to obtain modified basalt fiber.

[0092] Compared with Example 1, Comparative Example 1 did not utilize polyethyleneimine to modify the pretreated molybdenum disulfide.

[0093] Comparative Example 2

[0094] A method for preparing a high- and low-temperature resistant, high-elasticity, ultrathin cover material includes the following steps:

[0095] After mixing 90 parts of aggregate and 3 parts of mineral powder evenly, heat to 180℃, then add 3 parts of basalt fiber and stir for 45 seconds. Then add 10 parts of modified asphalt and stir at 180℃ for 4 minutes. The specimen is then formed at this temperature to obtain a high-temperature and low-temperature resistant, high-elasticity, ultra-thin cover material.

[0096] The preparation method of modified asphalt is as follows:

[0097] S1. Disperse 8g of molybdenum disulfide ultrasonically in 100mL of 80wt% ethanol aqueous solution, then add 1g of silane coupling agent KH550, stir at room temperature for 2h, and then filter, wash and dry to obtain pretreated molybdenum disulfide.

[0098] S2. Disperse 5g of pretreated molybdenum disulfide in 100mL of deionized water using ultrasound, adjust the pH of the solution to 10, then add 4g of polyethyleneimine and 6g of glutaraldehyde, heat and stir at 65℃ for 5h, and after the reaction is complete, filter, wash and dry to obtain modified molybdenum disulfide.

[0099] S3. Heat 80g of base asphalt to melt at a melting temperature of 180℃. Then add 4g of modified molybdenum disulfide and 10g of epoxy resin. Shear and disperse evenly in a dispersing emulsifier at a speed of 4000r / min for 2h to obtain modified asphalt.

[0100] Compared with Example 1, Comparative Example 2 did not involve any modification treatment of the basalt fibers.

[0101] The performance of the cover materials prepared in Examples 1-4 and Comparative Examples 1-2 was tested, as follows:

[0102] Freeze-thaw splitting strength test: The test was conducted in accordance with the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" JTG E20-2011;

[0103] Water immersion Marshall residual stability test: The test was conducted according to the method in the "Technical Specification for Construction of Asphalt Pavement of Highway" (JTG F40-2004);

[0104] High-temperature durability: The dynamic stability of the asphalt mixture was tested according to the method of JTG E20-2011.

[0105] Crack resistance: The crack resistance was determined by uniaxial compression test according to the method of JTG E20-2011;

[0106] The experimental results are shown in the table below:

[0107]

[0108] Finally, it should be noted that the above embodiments do not limit the present invention in any way. Those skilled in the art can make modifications and improvements based on the present invention. Therefore, any modifications or improvements made without departing from the spirit of the present invention are within the scope of protection claimed by the present invention.

Claims

1. A high-temperature and high-elastic ultra-thin covering material, It is characterized in that The raw materials include the following components in parts by weight: 90-95 parts of aggregate, 10-14 parts of modified asphalt, 3-5 parts of mineral powder, and 2-3 parts of modified basalt fiber; Wherein, the preparation method of the modified asphalt is as follows: S1, ultrasonically dispersing molybdenum disulfide in an ethanol aqueous solution, then adding an aminosilane coupling agent thereto, stirring for reaction, and then filtering, washing, and drying to obtain pretreated molybdenum disulfide; S2, ultrasonically dispersing the pretreated molybdenum disulfide in deionized water, adjusting the pH of the solution to 10-12, then adding polyethyleneimine and glutaraldehyde thereto, heating and stirring to react, after the reaction is completed, filtering, washing, and drying to obtain modified molybdenum disulfide; S3, heating the base asphalt until it is melted, then adding modified molybdenum disulfide and epoxy resin thereto, and shearing and dispersing them evenly in a dispersing and emulsifying machine to obtain modified asphalt; The preparation method of the modified basalt fiber is as follows: (1) ultrasonically dispersing basalt fibers in an ethanol aqueous solution, then adding a vinyl silane coupling agent thereto, stirring for 1-3 hours, and then filtering, washing, and drying to obtain pretreated basalt fibers; (2) The pretreated basalt fiber is dispersed in a toluene solvent, and then octadeceneamine, N,N'-methylenebisacrylamide and benzoyl peroxide are added thereto, and the mixture is stirred and reacted at 60-80°C for 2-4 hours. After the reaction is completed, the modified basalt fiber is obtained by filtering, washing and drying.

2. The high-low temperature resistant and highly elastic ultra-thin covering material according to claim 1, It is characterized in that In step S1, the mass ratio of molybdenum disulfide to aminosilane coupling agent is 8-12:1-3.

3. The high-low temperature resistant and highly elastic ultra-thin covering material according to claim 1, It is characterized in that In step S2, the mass ratio of pretreated molybdenum disulfide, polyethyleneimine and glutaraldehyde is 5-10:4-8:6-8.

4. The high-low temperature resistant and highly elastic ultra-thin covering material according to claim 1, It is characterized in that In step S2, the temperature of the heating and stirring reaction is 65-80° C., and the time of the heating and stirring reaction is 3-5 h.

5. The high-low temperature resistant and highly elastic ultra-thin covering material according to claim 1, It is characterized in that In step S3, the mass ratio of base asphalt, modified molybdenum disulfide and epoxy resin is 80-90:4-8:10-15.

6. The high-low temperature resistant and highly elastic ultra-thin covering material according to claim 1, It is characterized in that In step (1), the mass ratio of basalt fiber to vinyl silane coupling agent is 5-10:1-3.

7. The high-low temperature resistant and highly elastic ultra-thin covering material according to claim 1, It is characterized in that In step (2), the mass ratio of the pretreated basalt fiber, octadeceneamine, N,N'-methylenebisacrylamide and benzoyl peroxide is 8-10:4-6:0.8-1:0.2-0.

5.

8. A method for preparing a high-low temperature resistant and highly elastic ultra-thin covering material as claimed in any one of claims 1 to 7, It is characterized in that The method comprises the following steps: weighing each raw material by weight, mixing the aggregate and the mineral powder evenly, heating to 150-180°C, adding the modified basalt fiber, stirring for 30-60s, subsequently adding the modified asphalt, stirring at 150-180°C for 3-5min, and molding the test piece at this temperature to obtain the high and low temperature resistant and highly ductile ultra-thin covering material.