A starch-based degradable lunch box material and preparation method thereof

By adding esterified starch and EBP oxidation-biodegradation additives to polylactic acid materials, the degradation is accelerated by microbial and environmental factors, the problem of slow degradation of degradable plastic materials in the prior art is solved, and the degradation rate in different environments is achieved. Combination of efficient degradation and mechanical properties.

CN118620362BActive Publication Date: 2024-11-15SHANGHAI ZHENFENG APARTMENT MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410736978.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-11-15
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

Existing degradable plastic materials are slow to degrade in natural environments, especially in soil environments with lack of light and high temperature conditions, which are difficult to degrade effectively. The dependence of the prior art on photosensitizers leads to a decrease in the degradation rate, which cannot meet the high mechanics. Performance and controllable degradability requirements.

Method used

Using the combination of polylactic acid, esterified starch, EBP oxidation-biodegradation additive, TMC nucleation agent, coupling agent, anti-hydrolytic agent and light stabilizer, the acidic substances are generated under the action of microorganisms by esterified starch, and the hydrolysis of polylactic acid is promoted. , and use EBP to accelerate degradation under the action of light, heat, water and oxygen to form a porous structure to improve degradation efficiency.

Benefits of technology

The starch-based degradable lunch box material with good mechanical strength and controllable biodegradability in various environments can be achieved, which can degrade evenly in the soil and outdoor environment, significantly alleviating environmental pollution problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004882083000000081
    Figure BDA0004882083000000081
Patent Text Reader

Abstract

The invention provides a starch-based degradable lunch box material and a preparation method thereof, comprising the following components: polylactic acid, esterified starch, a compatibilizer, an EBP oxidation-biological dual degradation additive, a TMC nucleating agent, a coupling agent, an anti-hydrolysis agent, and a light stabilizer. The invention solves the problem of poor dispersibility of polylactic acid and EBP by adding a compatibilizer and esterified starch, thereby ensuring that the starch-based degradable lunch box material has good mechanical strength. In addition, by exerting different degradation mechanisms of esterified starch and EBP, it is ensured that the material of the invention has good degradability whether it is buried in soil or directly placed in an outdoor environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the field of degradable plastics, and more specifically to a starch-based degradable lunch box material and a preparation method thereof. Background technology:

[0002] Plastic is one of the greatest inventions of mankind in the history of materials. However, as the plastic industry in countries around the world has experienced explosive growth, non-degradable plastics will cause unprecedented damage to the natural environment, and the control of "white pollution" has become urgent.

[0003] In 2008, my country issued regulations to restrict the production and sale of plastic bags. The introduction of the plastic restriction order can reduce "white pollution" to a certain extent, but it cannot eliminate it from the root. Although people's environmental awareness is gradually increasing, various types of plastic waste can often be seen in the wild and scenic spots. After the plastic waste is collected, it is generally buried in the soil. Only by developing and researching biodegradable plastics to replace non-degradable plastics can the white pollution crisis be resolved into an invisible one. However, there is no substitute that can completely match the non-degradable plastic in the biodegradable material market. Its performance and high cost cannot meet the needs of people's daily life. Therefore, the development of new biodegradable plastic materials with excellent performance and low cost is still a hot topic of current research.

[0004] The degradable high molecular weight polyester exhibits excellent mechanical properties, and also has thermal processing properties, as well as excellent biodegradability and biocompatibility. The most commonly used method is to use degradable polyester as the base material and then add a certain amount of starch as a filler to obtain a starch / polyester composite material, which can inherit the degradation ability of starch and meet the requirements of mechanical properties through complementarity. However, although high molecular weight polyesters such as polylactic acid are degradable materials, their degradation is generally divided into two processes: hydrolysis and depolymerization and microbial degradation. The hydrolysis and depolymerization of polyester still requires high temperature, light or strong acid and alkali conditions, so its overall biodegradation rate is slow and the degradation cycle is difficult to control.

[0005] The existing technology generally promotes the polyester material to accelerate the hydrolysis and depolymerization into low molecular weight oligomers by adding photosensitizers. The disadvantage of adding photosensitizers is that when the discarded polyester material is buried in the soil or shaded by plants, the photosensitizer's excessive dependence on light will seriously reduce its degradation rate. Therefore, it is very necessary to develop a starch-based degradable lunch box material with high mechanical strength and controllable degradability in various environments. Summary of the invention:

[0006] The present invention intends to provide a starch-based degradable lunch box material and a preparation method thereof, wherein the material has excellent mechanical properties and controllable biodegradability.

[0007] To achieve the technical purpose of the present invention, the present invention provides a starch-based degradable lunch box material, which is made of the following raw materials in parts by weight: 50-60 parts of polylactic acid, 15-20 parts of esterified starch, 1-2 parts of a compatibilizer, 1-2 parts of an EBP oxidation-biodegradable dual-degradation additive, 0.5-2 parts of a TMC nucleating agent, 1-2 parts of a coupling agent, 0.5-1 parts of an anti-hydrolysis agent, and 0.5-1 parts of a light stabilizer.

[0008] Furthermore, the polylactic acid model is selected as PLA3052 or PLA3251D.

[0009] Furthermore, the esterified starch is octyl succinate esterified starch or acetate esterified starch.

[0010] Furthermore, the compatibilizer is maleic anhydride grafted polyolefin elastomer (POE-g-MAH).

[0011] Furthermore, the TMC nucleating agent is one or more of TMC-200, TMC-300, and TMC-306.

[0012] Furthermore, the anti-hydrolysis agent is a carbodiimide anti-hydrolysis agent.

[0013] Furthermore, the coupling agent is an aluminum-titanium composite coupling agent.

[0014] Furthermore, the light stabilizer is a hindered amine light stabilizer (HALS).

[0015] The method for preparing the starch-based degradable lunch box material comprises the following steps:

[0016] (1) Add esterified starch, compatibilizer, and EBP oxidation-biological dual degradation additive into a mixer and stir for 10-20 minutes;

[0017] (2) Continue to add polylactic acid, TMC nucleating agent, coupling agent, anti-hydrolysis agent, and light stabilizer into the mixer and stir and mix for 30-40 minutes to obtain a mixed material;

[0018] (3) The mixed materials are put into a twin-screw extruder for extrusion, and then cooled and pelletized to obtain the product.

[0019] Furthermore, in step (1), the temperature of the mixer is 70-80° C. and the rotation speed is 800-1200 r / min.

[0020] Furthermore, the temperature of the mixer in step (2) is 90-110° C., and the rotation speed is 800-1200 r / min.

[0021] Furthermore, the setting conditions of the extruder in step (3) are as follows: the temperature of each section of the extruder is 130-150°C, 140-160°C, 160-170°C, 170-180°C, 160-170°C, 150-160°C; the feeding speed is 20-30r / min, and the main engine speed is 80-100r / min.

[0022] The oxidative-biodegradable additive EBP is a degradable masterbatch produced by Shandong Tianzhuang Environmental Protection Technology Co., Ltd. by adding an additive that can accelerate the oxidative-biodegradation process to a polyolefin resin. This masterbatch is suitable for polyolefin systems such as polyethylene. When it is applied to the polylactic acid system, there will be problems such as poor dispersion effect and inability to effectively promote the hydrolysis and degradation of polylactic acid; the present invention effectively solves the problem of poor dispersion effect of polylactic acid and EBP by adding a compatibilizer and esterified starch to EBP; at the same time, compared with polylactic acid, esterified starch can be degraded first under the action of microorganisms to form acidic substances and generate porous structures at the same time, further effectively exerting the degradation function of EBP.

[0023] When the starch-based degradable lunch box material of the present invention is buried in the soil, the material as a whole is in anaerobic conditions, and the esterified starch will be eroded by microorganisms in the soil, causing CC and CO bonds to gradually break, producing acidic substances, thereby promoting the hydrolysis of the polylactic acid material; at the same time, the degradation of the esterified starch will cause the material to form a porous structure, so that the active components in EBP have more opportunities to contact with oxygen and moisture in the soil, so that the degradation effect of EBP can be exerted, prompting polylactic acid and esterified starch to further form low-molecular-weight fragments.

[0024] When the starch-based degradable lunch box material of the present invention is directly placed in an outdoor environment, the active components in EBP will form low molecular weight fragments of polylactic acid and esterified starch under the combined effects of light, heat, water and oxygen, and eventually degrade. Even if the lunch box material is blocked by vegetation, the active components of EBP will play a certain role only under the action of water and oxygen, thereby alleviating the excessive dependence of polylactic acid on light during degradation to a certain extent. The starch-based degradable lunch box material prepared by the present invention should be stored in a light-proof, low-temperature and dry environment.

[0025] The present invention ensures that the starch-based degradable lunch box material has good mechanical strength by compounding esterified starch, EBP and a compatibilizer, and has good degradability whether buried in the soil or directly placed in an outdoor environment.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The present invention adds EBP to the starch-based degradable lunch box material, ensuring that it can be effectively degraded in various environments; that is, the material can be gradually degraded whether it is randomly discarded outdoors or buried in the soil, which can greatly alleviate the problem of environmental pollution.

[0028] (2) The present invention makes full use of the dual hydrophilic and lipophilic properties of esterified starch and compatibilizer to well connect polylactic acid and EBP, thereby ensuring the degradability and mechanical strength of the final product. Specific implementation method:

[0029] In order to make the purpose, technical scheme and advantages of the present invention more clear, the technical scheme of the present invention is further described below through specific implementation methods. Those skilled in the art should know that the embodiments are only to help understand the technical content and technical effects of the present invention and should not be regarded as limiting the present invention.

[0030] In the embodiments and comparative examples of the present invention, the polylactic acid is selected from NatureWorks' PLA3052 or PLA3251D; the anti-hydrolysis agent is selected from Bio-SW100 or Bio-SW500; the aluminum-titanium composite coupling agent is selected from OL-AT1618; the EBP is selected from EBP-pp-1502 or EBP-pp-1501 produced by Shandong Tianzhuang Environmental Protection Co., Ltd.; the compatibilizer POE-g-MAH is selected from DuPont's Fusabond N495; the light stabilizer is selected from Hefei Tianjian Chemical Co., Ltd.'s hindered amine light stabilizer UV-3853 or UV944.

[0031] The esterified starch in the examples and comparative examples was purchased from Suzhou Minghua Sugar Alcohol Co., Ltd., and the ordinary cassava starch was purchased from Shandong Gushuo Biotechnology Co., Ltd.; TMC nucleating agent, aluminum-titanium composite coupling agent, anti-hydrolysis agent, and chain extender were all purchased from Shanxi Chemical Research Institute (Co., Ltd.).

[0032] The present invention includes 4 embodiments and 4 comparative examples.

[0033] Embodiment 1:

[0034] (1) Add 15 parts of octyl succinate starch, 1.5 parts of EBP-pp-1501, and 1 part of compatibilizer Fusabond N495 into a mixer, and stir and mix at 80°C and 1000 r / min for 15 minutes;

[0035] (2) Continue to add 50 parts of polylactic acid PLA3052, 1 part of nucleating agent TMC-200, 1 part of coupling agent OL-AT1618, 0.5 parts of anti-hydrolysis agent Bio-SW500, and 0.5 parts of light stabilizer UV-3853 into the mixer, and stir and mix at 100° C. and 1200 r / min for 30 minutes to obtain a mixed material;

[0036] (3) feeding the mixed materials into a twin-screw extruder for extrusion granulation, and obtaining the starch-based biodegradable lunch box material of the present invention after cooling and pelletizing; the setting conditions of the extruder are as follows: the temperatures of each section of the extruder are 145° C., 155° C., 165° C., 170° C., 165° C., 155° C., the feeding speed is 30 r / min, and the main engine speed is 100 r / min.

[0037] Embodiment 2:

[0038] (1) Add 20 parts of octyl succinate starch, 2 parts of EBP-pp-1501, and 2 parts of compatibilizer Fusabond N495 into a mixer, and stir and mix at 70°C and 1200 r / min for 10 min;

[0039] (2) Continue to add 50 parts of polylactic acid PLA3052, 1 part of nucleating agent TMC-300, 1 part of coupling agent OL-AT1618, 0.5 parts of anti-hydrolysis agent Bio-SW100, and 1 part of light stabilizer UV-3853 into the mixer, and stir and mix at 100° C. and 1200 r / min for 30 minutes to obtain a mixed material;

[0040] (3) feeding the mixed materials into a twin-screw extruder for extrusion granulation, and obtaining the starch-based biodegradable lunch box material of the present invention after cooling and pelletizing; the setting conditions of the extruder are as follows: the temperatures of each section of the extruder are 145° C., 155° C., 165° C., 170° C., 165° C., 155° C., the feeding speed is 30 r / min, and the main engine speed is 100 r / min.

[0041] Embodiment 3:

[0042] (1) Add 15 parts of acetic acid starch, 1.5 parts of EBP-pp-1502, and 1 part of compatibilizer Fusabond N495 into a mixer, and stir and mix at 80°C and 1000 r / min for 15 minutes;

[0043] (2) Continue to add 60 parts of polylactic acid PLA3251D, 1 part of nucleating agent TMC-300, 1 part of coupling agent OL-AT1618, 0.5 parts of anti-hydrolysis agent Bio-SW500, and 0.5 parts of UV-944 into the mixer, and stir and mix at 100° C. and 1200 r / min for 30 minutes to obtain a mixed material;

[0044] (3) feeding the mixed materials into a twin-screw extruder for extrusion granulation, and obtaining the starch-based biodegradable lunch box material of the present invention after cooling and pelletizing; the setting conditions of the extruder are as follows: the temperatures of each section of the extruder are 145° C., 155° C., 165° C., 170° C., 165° C., 155° C., the feed speed is 20 r / min, and the main engine speed is 80 r / min.

[0045] Embodiment 4:

[0046] (1) Add 20 parts of acetic acid starch, 1.5 parts of EBP-pp-1502, and 1.5 parts of compatibilizer Fusabond N495 into a mixer, and stir and mix at 80°C and 1000 r / min for 15 minutes;

[0047] (2) Continue to add 60 parts of polylactic acid PLA3251D, 1 part of nucleating agent TMC-306, 1 part of coupling agent OL-AT1618, 0.5 parts of anti-hydrolysis agent Bio-SW100, and 1 part of UV-944 into the mixer, and stir and mix at 100° C. and 1200 r / min for 30 minutes to obtain a mixed material;

[0048] (3) feeding the mixed materials into a twin-screw extruder for extrusion granulation, and obtaining the starch-based biodegradable lunch box material of the present invention after cooling and pelletizing; the setting conditions of the extruder are as follows: the temperatures of each section of the extruder are 145° C., 155° C., 165° C., 170° C., 165° C., 155° C., the feed speed is 20 r / min, and the main engine speed is 80 r / min.

[0049] Comparative Example 1:

[0050] The difference from Example 1 is that unmodified cassava starch is used to replace the octyl succinate starch.

[0051] Comparative Example 2:

[0052] The difference from Example 1 is that the compatibilizer Fusabond N495 is not added.

[0053] Comparative Example 3:

[0054] The difference from Example 1 is that no EBP was added.

[0055] Comparative Example 4:

[0056] The difference from the example is that the amount of EBP added is changed from 1.5 parts to 4 parts.

[0057] The pellet products prepared in Examples 1-4 and Comparative Examples 1-4 were injected into standard specimens with a size of 100 mm×10 mm×1.0 mm.

[0058] The above standard specimens are tested for various properties using the following standard methods:

[0059] (1) Tensile strength performance test: The specimens were stretched at a speed of 25 mm / min at room temperature, and the mechanical properties of the samples were tested on an electronic tensile testing machine.

[0060] (2) Weight loss rate after 60 days of burial in soil (%): Weigh and record the weight of each standard sample; then wrap the standard sample in gauze and bury it in the soil 20 cm above the ground surface; after 60 days, take out, wash, dry, weigh and record the weight.

[0061] The weight loss rate of the standard sample was calculated by the following method: weight loss rate (%) = (weight before test - weight after 60 days) / weight before test × 100%.

[0062] (3) Weight loss rate (%) after 60 days of exposure to natural environment (with shelter): weigh and record the weight of each standard sample; then wrap the standard sample in gauze and place it in the weeds, and fix the standard sample with a metal grid. After 60 days, wash and dry it, weigh and record the weight.

[0063] The weight loss rate of the standard sample was calculated by the following method: weight loss rate (%) = (weight before test - weight after 60 days) / weight before test × 100%.

[0064] (4) Weight loss rate (%) after 60 days of exposure to natural environment (unshielded): weigh and record the weight of each standard specimen; then wrap the standard specimens in gauze, place them directly on the soil, and fix them with metal grids. After 60 days, wash and dry them, weigh and record the weight.

[0065] The weight loss rate of the standard sample was calculated by the following method: weight loss rate (%) = (weight before test - weight after 60 days) / weight before test × 100%.

[0066] In order to better verify the effect of the present invention, the above tests all use 5 groups of samples, and the final results are averaged, as shown in Table 1.

[0067]

[0068] From the results of Examples 1-4 and Comparative Examples 1-4, it can be seen that the starch-based degradable lunch box material has good mechanical strength through the compounding of esterified starch, EBP, and compatibilizer, and at the same time, whether it is buried in the soil or directly placed in an outdoor environment (with or without shelter), it can have better degradability. When the material is buried in the soil, the esterified starch will produce acidic substances under the erosion of microorganisms in the soil, and at the same time, a porous structure will be formed in the material, so that the active components in EBP have more opportunities to contact with oxygen and moisture in the soil, which promotes polylactic acid and esterified starch to further form low molecular weight fragments, and finally be degraded.

[0069] When the starch-based degradable lunch box material of the present invention is directly placed in an outdoor environment, the active components in EBP will form low molecular weight fragments of polylactic acid and esterified starch under the combined effects of light, heat, water and oxygen, and eventually be degraded. Even if the lunch box material is blocked by vegetation, EBP can be gradually degraded under the action of water and oxygen, and microorganisms in the weeds will also degrade the esterified starch, so that the overall degradation rate is also maintained in a higher range.

[0070] From the comparison between Example 1 and Comparative Example 1, it can be seen that the starch that has not been esterified cannot be well blended with polylactic acid and EBP, resulting in the final material having reduced mechanical strength and degradability.

[0071] From the comparison between Example 1 and Comparative Example 2, it can be seen that the polyolefin segment in the compatibilizer can wrap EBP well, and at the same time, the maleic anhydride segment of the compatibilizer can be well combined with polylactic acid, which can more fully exert the effect of EBP and improve the overall mechanical strength and degradability of the material.

[0072] From the comparison between Example 1 and Comparative Example 3, it can be seen that without adding EBP, the degradability of the material will be greatly reduced. From the comparison between Example 1 and Comparative Example 4, it can be seen that excessive addition of EBP will lead to poor overall dispersibility of the material, resulting in a decrease in mechanical strength, and will also affect the degradation of esterified starch.

[0073] From the weight loss rate under different conditions, the final results of the present invention by adding EBP and esterified starch show that a good degradation effect can be achieved whether buried in the soil or exposed to the natural environment. When the EBP is not dispersible enough or the dosage is insufficient or too high, it will have an adverse effect on the degradation effect.

[0074] Judging from the test results, the degradation rate of the materials completely exposed to the unshielded outdoor environment is higher than that of the materials directly buried and shielded. This is because the materials completely exposed to the natural environment can enable EBP to fully exert its oxidative degradation effect, and at the same time form porous structures and acidic substances earlier, thereby comprehensively exerting the degradation effect. This characteristic also means that even if the materials of the present invention are discarded at will, they can be fully degraded, thereby minimizing environmental pollution.

[0075] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A starch-based degradable lunch box material, characterized in that: The invention is prepared from the following raw materials in parts by weight: 50-60 parts of polylactic acid, 15-20 parts of esterified starch, 1-2 parts of a compatibilizer, 1-2 parts of an EBP oxidation-biological dual degradation additive, 0.5-2 parts of a TMC nucleating agent, 1-2 parts of a coupling agent, 0.5-1 parts of an anti-hydrolysis agent, and 0.5-1 parts of a light stabilizer; wherein the esterified starch is octyl succinate esterified starch or acetic esterified starch, and the compatibilizer is a maleic anhydride grafted polyolefin elastomer.

2. The starch-based degradable lunch box material according to claim 1, characterized in that: The polylactic acid model is PLA3052 or PLA3251D.

3. The starch-based degradable lunch box material according to claim 1, characterized in that: The TMC nucleating agent is one or more of TMC-200, TMC-300 and TMC-306; the anti-hydrolysis agent is a carbodiimide anti-hydrolysis agent; the coupling agent is an aluminum-titanium composite coupling agent; and the light stabilizer is a hindered amine light stabilizer.

4. A method for preparing the starch-based degradable lunch box material according to claims 1-3, characterized in that: The steps include: (1) Add esterified starch, compatibilizer, and EBP oxidation-biodegradable additive into a mixer and stir for 10-20 minutes; (2) Continue to add polylactic acid, TMC nucleating agent, coupling agent, anti-hydrolysis agent, and light stabilizer into the mixer and stir for 30-40 minutes to obtain a mixed material; (3) The mixed materials are fed into a twin-screw extruder for extrusion, and then cooled and pelletized to obtain the product.

5. The method for preparing the starch-based degradable lunch box material according to claim 4, characterized in that: In step (1), the temperature of the mixer is 70-80°C; the rotation speed is 800-1200 r / min.

6. The method for preparing the starch-based degradable lunch box material according to claim 4, characterized in that: The temperature of the mixer in step (2) is 90-110° C., and the rotation speed is 800-1200 r / min.

7. The method for preparing the starch-based degradable lunch box material according to claim 4, characterized in that: The setting conditions of the extruder in step (3) are as follows: the temperature of each section of the extruder is 130-150°C, 140-160°C, 160-170°C, 170-180°C, 160-170°C, 150-160°C; the feeding speed is 20-30r / min, and the main engine speed is 80-100r / min.