A preparation process for cold-rolled fan-shaped plate and the product obtained therefrom
The reinforcement layer with different hardness is formed through surface laser quenching and ultrasonic impact processes, which solves the problem of poor fatigue resistance of cold-rolled fan plates and improves the service life and production efficiency of fan plates.
Patent Information
- Application Number
- CN202411080325.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The existing cold-rolled fan plates have poor fatigue resistance under bending force and torque conditions, which are prone to microcracks, resulting in low life and high replacement frequency, affecting the production efficiency and operating costs of rolling steel.
The surface laser quenching composite strengthening process is adopted to form a hardened layer through surface laser quenching, and combined with surface strengthening processes such as ultrasonic impact or ultrasonic shot peening, a reinforcement layer with different hardness is formed to improve the fatigue resistance of the fan plate.
It significantly improves the fatigue resistance of cold-rolled fan plates, extends service life, and reduces shear and impact pressure wear during steel plate coiling, improving production efficiency and economic benefits.
Smart Images

Figure CN118621098B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cold-rolled sector plates, and more specifically, relates to a preparation process of cold-rolled sector plates and a product obtained therefrom. Background Art
[0002] The coiling shaft is the core equipment for coiling steel plates in the steel rolling production line. The steel plates move along the steel rolling line. During the coiling process, the surface of the cold-rolled fan-shaped plate is in direct contact with the steel plates. The fan-shaped plate is subjected to tension, bending force and torque. At the same time, the surface is constantly impacted and rubbed by the steel plates, which makes it very easy to produce fatigue cracks on the arc surface of the cold-rolled fan-shaped plate. Under the action of the impact force, the fatigue cracks gradually expand and eventually break the cold-rolled fan-shaped plate. The existing cold-rolled fan-shaped plates have a short lifespan and a high replacement frequency, resulting in low production efficiency of the steel rolling production line and high operating costs of the steel mill.
[0003] After searching, patent CN109694943A discloses a composite surface treatment method for gear surface strengthening, which can be used for surface strengthening of wind power and automobile gears. The invention adopts laser quenching treatment and shot peening composite treatment to avoid the problem of laser quenching and tempering softening, while increasing the residual compressive stress of the tooth root and the hardness value of the gear tooth surface. The comprehensive coordination of the two significantly improves the surface performance of the gear. However, since the tooth surface of the gear is a linear contact fit, compared with the tension, impact force and impact force borne by the surface of the sector plate, the gear requires more wear resistance of the tooth surface sliding against each other during the torque transmission process, so the entire gear surface needs to be quenched.
[0004] Patent CN110802218A discloses a rapid creep aging forming method for large curvature corrugated plates. The invention firstly solid-solution-treats the aluminum alloy plate at 430-540℃ for 1-5h and then quenches it with flowing water; then performs bilateral synchronous laser shot peening strengthening treatment on the selected area of the plate; then the plate is bent in a mold; and finally the plate is creep-aged in an autoclave. The invention forms uniform compressive stress in the bilateral bending area of the plate by performing bilateral synchronous laser shot peening strengthening treatment on the aluminum alloy plate, avoids the generation of microcracks during the bending forming of large curvature corrugated plates, increases the dispersion and precipitation efficiency of the strengthening phase, and enhances the corrosion resistance and fatigue resistance of the corrugated plate. Patent CN110508616A discloses a method for achieving gradient strengthening of metal material surface by corrugation rolling. The method combines corrugation rolling and flat roll rolling. By repeatedly rolling and continuously changing the direction of the rolled sample, each part of the plate surface is locally deformed, and a uniformly distributed surface large strain shallow deformation layer is obtained, thereby forming a gradient strengthening structure with gradually decreasing hardness from the surface to the inside on the entire metal plate. The above patents all process the plate into a large deformation corrugated plate before use, but the large deformation corrugated plate has poor surface fatigue resistance and is still prone to microcracks under bending force and torque conditions. Summary of the invention
[0005] 1. Problem to be solved
[0006] In view of the problem that the existing cold-rolled sector plates have poor surface fatigue resistance and are prone to microcracks under bending force and torque conditions, the present invention provides a preparation process for cold-rolled sector plates, which utilizes a surface laser quenching composite surface strengthening process to strengthen the cold-rolled sector plates, and the prepared cold-rolled sector plates have higher fatigue resistance.
[0007] 2. Technical solution
[0008] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0009] A preparation process for a cold-rolled sector plate, wherein the cold-rolled sector plate substrate is subjected to a surface laser quenching process to obtain a hardened layer, and then subjected to a surface strengthening process to obtain a strengthened layer, wherein the surface strengthening process is selected from one of ultrasonic impact, ultrasonic shot peening and laser shot peening.
[0010] The preparation process of the cold-rolled sector plate comprises the following steps: smelting→blanking→forging heat treatment→rough machining→tempering heat treatment→finishing→surface laser quenching→surface treatment.
[0011] The cold-rolled sector plate substrate is prepared by smelting → blanking → forging heat treatment → rough machining → quenching and tempering heat treatment → finishing, and the specific steps are as follows:
[0012] (1) Smelting: The high-quality alloy is prepared according to the composition ratio and then smelted in an electric furnace, and LF refining and VD vacuum degassing processes are adopted.
[0013] Preferably, the chemical composition of the alloy includes, by mass percentage: C: 0.28%-0.32%, Mn: 0.30%-0.60%, Si: 0.10%-0.30%, P: ≤0.020%, S≤0.015%, Ni: 2.00%-2.20%, Cr: 2.00%-2.20%, and the balance is Fe.
[0014] (2) Billet making: Cut the steel ingot according to the weight of the cold-rolled sector plate blank, heat it at a forging temperature of 1000-1150℃, and then perform upsetting and drawing forging on a 10-ton forging hammer machine, with a forging ratio ≥6.
[0015] (3) Forging heat treatment: The forged billet is reheated at a temperature of 1000-1150°C and then
[0016] Forging is carried out with an arc anvil to ensure that the final forging temperature is around 900-950℃; the basic size of the forging blank meets the requirements of the blank drawing, and after forging, it is slowly cooled to 300-350℃ and kept warm for 6h, and then normalized at 900-920℃, and quickly cooled to 620-650℃ for tempering and kept warm for 6h, so that the banded structure is ≤level 1 and the grain size is ≥level 7; the arc surface of the cold-rolled sector plate forged with an arc anvil has less material removed in rough machining, uniform structure, and refined grains, which improves the overall performance of the entire workpiece.
[0017] (4) Rough machining: Rough machining the forging blank according to the drawing.
[0018] (5) Quenching and tempering heat treatment: The rough-processed cold-rolled sector plate is kept at 850±10℃ for 180min to austenitize, then oil-cooled to about 150℃, and the maximum cooling rate of the quenching oil is maintained at 120℃ / s for quenching and cooling, and then tempered at 580±10℃ for 6 hours. After tempering, it is taken out of the furnace and air-cooled. The matrix structure after quenching and tempering includes: more than 90% troostite, the rest is bainite with a content of ≤10% and a very small amount of ferrite. The surface hardness of the matrix meets HB280-320 (HV284-328; HRC29.5-34.7), and the matrix performance index reaches: 900MPa≤σ b ≤1000MPa, 800MPa≤σ s ≤900MPa, 15%≤δ≤20%, 60%≤Ψ≤70%, AK(u)≥100J.
[0019] (6) Finishing: The cold-rolled sector plate after quenching and tempering shall be finished according to the drawing to meet the shape and position tolerance and roughness requirements of the drawing.
[0020] The cold-rolled sector plate substrate obtained above is subjected to a composite strengthening process, wherein the composite strengthening process includes surface laser quenching and at least one of ultrasonic impact, ultrasonic shot peening and laser shot peening.
[0021] In the surface laser quenching process, a rectangular spot is used to perform surface laser quenching along the width direction of the cold-rolled sector plate. The laser power determines the hardness and depth of the surface after laser quenching. The heat flux density is high, and the surface is easily burned and defects are generated. After testing, the depth L of the hardened layer produced by surface laser quenching on the curved surface of the cold-rolled sector plate satisfies:
[0022]
[0023] In the formula, λ is the correction coefficient, and its value range is 0.20-0.30; P is the laser heat source power, unit is W; a is the spot width, unit is mm, which is basically the same as the quenching layer width; b is the spot length, unit is mm; v is the laser scanning speed, unit is mm / s.
[0024] The laser power is 2000-2400W, the spot width is 10-12mm, the spot length is 6-8mm, the scanning speed is 6-8mm / s, the hardened layer L thickness is 1mm≤L≤1.2mm, and the hardened layer structure is: content ≥90% martensite, the rest is austenite, content ≤10%, the surface hardness reaches HRC45-50 (HV441-512), and the quenching bandwidth of the arc surface of the cold-rolled fan plate is 10-12mm wide. After the laser quenching of the arc surface of the cold-rolled fan plate, a surface with alternating soft and hard bands is formed. The tensile stress on the surface will cause the cold-rolled fan plate to be gradually released during the later use, causing the cold-rolled fan plate to be distorted and deformed, and even micro cracks to appear on the surface. Therefore, it is necessary to further strengthen the surface of the fan plate after quenching.
[0025] The surface strengthening process of the material obtained by surface laser quenching is as follows: the arc area of the cold-rolled fan plate is treated by a surface strengthening process, preferably ultrasonic impact, and its process parameters are: current 1.2±0.1A, resonant voltage 15±1V, vibration frequency 40±2KHz. After ultrasonic impact, the difference in thickness and roughness of the strengthening layer formed under the same impact process causes a 0.05-0.2mm size thickness difference on the surface of the fan plate, and micro-ripples appear in the quenched area and the non-quenched area. During the use of the steel rolling production line, the arc surface of the cold-rolled fan plate is constantly subjected to the friction and impact force of the steel plate. Due to the hardness difference between the quenched area and the non-quenched area ≥HRC10, the wear amount of the non-quenched area is greater than that of the quenched area, and the depth of the arc surface ripples gradually increases, which is conducive to buffering the shear and impact pressure brought by the steel plate to the arc surface of the fan plate.
[0026] The cold-rolled sector plate obtained by the above method comprises: a quenching area and a non-quenching area:
[0027] The surface hardness difference between the quenched area and the non-quenched area is ≥HRC10, wherein the quenched area includes the substrate, the hardened layer generated on the substrate surface after surface laser quenching, and the strengthening layer generated on the hardened layer surface after surface strengthening, and the non-quenched area includes the substrate and the strengthening layer generated on the substrate surface after surface strengthening. The quenched area and the non-quenched area are sequentially spaced along the surface laser quenching direction, the interval between the quenched area and the non-quenched area is 10-12mm, and the thickness difference between the hardened layer and the strengthening layer in the quenched area and the strengthening layer in the non-quenched area is 0.05-0.2mm.
[0028] Among them, the thickness of the hardened layer in the quenching area is: 1mm≤L≤1.2mm, the metallographic structure is martensite ≥90%, and the rest is austenite with a content of ≤10%, and the surface hardness is HRC45-50 (HV441-512).
[0029] After surface strengthening, the hardness of the quenching area is HRC50-55 (HV512-596), the metallographic structure is martensite content ≥90%, the thickness of the strengthening layer is 0.05mm-0.15mm, and the surface deformation is ≤0.05mm;
[0030] The hardness of the non-quenched area is HB330-360 (HV338-371; HRC35.7-39), the metallographic structure is sorbite ≥90%, the rest is bainite and ferrite, the thickness of the strengthening layer is 0.2mm-0.25mm, and the surface deformation is 0.15-0.20mm.
[0031] The matrix includes more than 90% of troostite, the rest of which is bainite and a very small amount of ferrite, and the surface hardness of the matrix meets HB280-320.
[0032] 3. Beneficial effects
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The present invention adopts a surface laser quenching composite strengthening process, first performs surface laser quenching treatment on the cold-rolled sector plate, and then performs surface strengthening, so that the hardness difference between the quenching area and the non-quenching area is ≥HRC10, and under the same impact force, the surface hardness of the quenching area is high, and the plastic deformation generated on the surface is small, the hardness of the non-quenching area is low, and the plastic deformation is large. The difference in deformation between the quenching area and the non-quenching area is 0.05-0.2mm, so that micro-ripples appear on the surface of the cold-rolled sector plate, which is beneficial to buffering the shear and impact pressure of the steel plate on the arc surface of the sector plate during the steel plate coiling process, improving the fatigue resistance of the cold-rolled sector plate, and improving the service life of the cold-rolled sector plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but it should be understood that these drawings are designed only for explanation purposes and are not intended to limit the scope of the present invention. In addition, unless otherwise specified, these drawings are intended only to conceptually illustrate the structural configurations described herein and are not necessarily drawn to scale.
[0036] Figure 1 It is a schematic diagram of the stress condition of the cold-rolled sector plate of the present invention;
[0037] Figure 2 It is a schematic diagram of forging of the cold-rolled sector plate of the present invention;
[0038] Figure 3 and Figure 4 This is a schematic diagram of the surface laser quenching direction of the present invention;
[0039] Figure 5 This is the stress distribution trend before strengthening in the quenching area of Example 1;
[0040] Figure 6 This is the stress distribution trend after strengthening in the quenching area of Example 1;
[0041] Figure 7 The stress distribution trend of the non-quenching area before strengthening in Example 1;
[0042] Figure 8 The stress distribution trend of the non-quenched area after strengthening in Example 1, where Figure 5-Figure 8 In the figure, the stress curve is the main stress distribution trend detected by the fully automatic gradient stress detection and analysis system within 1mm from the surface, and is the stress distribution trend at different depths at the same position;
[0043] Fig. 9 This is the metallographic structure diagram of the non-quenched area after strengthening in Example 1;
[0044] Fig.10 This is the metallographic structure diagram of Example 1 after quenching area strengthening. DETAILED DESCRIPTION
[0045] The following detailed description of exemplary embodiments of the present invention refers to the accompanying drawings, which form a part of the description, and in which exemplary embodiments of the present invention that can be implemented are shown as examples. Although these exemplary embodiments are described in sufficient detail to enable those skilled in the art to implement the present invention, it should be understood that other embodiments can be implemented and various changes can be made to the present invention without departing from the spirit and scope of the present invention. The following more detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but is only for the purpose of illustrating and not limiting the description of the characteristics and features of the present invention, so as to propose the best mode for performing the present invention and to enable those skilled in the art to implement the present invention. Therefore, the scope of the present invention is limited only by the appended claims.
[0046] It should be understood that the following text is only used to describe one or several specific embodiments of the present invention, and does not strictly limit the scope of protection of the specific claims of the present invention. As used herein, the terms "parallel" and "perpendicular" are not limited to their strict geometric definitions, but include tolerances for reasonable and inconsistent machining or human errors.
[0047] The coiling shaft is the core equipment for coiling steel plates in the steel rolling production line. The steel plates travel along the steel rolling line at a speed of 30 meters / min. During the coiling process, the surface of the cold-rolled sector plate is in direct contact with the steel plate and is subjected to a large tension. Taking the steel plate with a thickness of 1.8-3mm and a strength of ≥800MPa as an example, the cold-rolled sector plate is subjected to 45N / mm during the coiling process. 2 Tension, steel plate width 1100mm~1120mm, such as Figure 1At the same time, the steel plate produces a certain impact and friction on the surface of the cold-rolled fan-shaped plate, causing the cold-rolled fan-shaped plate to bear bending force and torque. Under the continuous impact and friction, microcracks or even fractures are prone to occur on the surface of the cold-rolled fan-shaped plate, causing failure.
[0048] Therefore, the present application aims at the arc surface position of the cold-rolled sector plate, controls the quenching and tempering and surface treatment processes, and improves the uniformity of the structure and the surface fatigue resistance of the alloy workpiece. Furthermore, by optimizing the forging process, using an arc anvil, and forging the arc surface, the grain size and structure of the forging are uniform.
[0049] The cold-rolled sector plate substrate is subjected to surface laser quenching and strengthening impact to form a cold-rolled sector plate product.
[0050] This application adopts the workpiece forged by medium carbon alloy steel, the grain size after forging is ≥6, and the internal metallographic structure and surface hardness of the matrix are controlled after rough machining. According to the stress and production line safety factor requirements of the cold-rolled sector plate, the mechanical performance index of the cold-rolled sector plate matrix meets the following requirements: 900MPa≤σ b ≤1000MPa, 800MPa≤σ s ≤900MPa, 15%≤δ≤20%, 60%≤Ψ≤70%, AK(u)≥100J. The surface laser quenching and surface strengthening process are used to carry out composite strengthening treatment on the arc surface of the cold-rolled sector plate to enhance its wear resistance and impact resistance, so as to improve the service life of the product.
[0051] The cold-rolled sector plate raw material of the present application is prepared by smelting → blanking → forging heat treatment → rough processing, and is subjected to quenching and tempering treatment to obtain a composite strengthened matrix material, which satisfies: the metallographic structure includes more than 90% troostite, the rest is bainite and a very small amount of ferrite, and the matrix performance index reaches: 900MPa≤σ b ≤1000MPa, 800MPa≤σ s ≤900MPa, 15%≤δ≤20%, 60%≤Ψ≤70%, AK(u)≥100J, the surface hardness of the substrate meets HB280-320 (HV284-328; HRC29.5-34.7).
[0052] Yield strength index σ s It is the minimum strength of the cold-rolled sector plate when the moment generated by the steel plate and the elastic-plastic bending moment are balanced under the coiling tension borne by the cold-rolled sector plate during the coiling process; the tensile strength σ b Determined according to the yield strength ratio coefficient of 0.9±0.2; the metal material reaches the tensile strength σ bUnder the premise of, the plasticity index δ and Ψ values are indicators to measure the degree of deformation of the cold-rolled fan-shaped plate when it is subjected to stress. δ is the elongation deformation rate of the test block in the length direction during the tensile test, and Ψ is the shrinkage deformation rate of the test block in the diameter direction during the tensile test; the toughness index AK (u) is the ability of the cold-rolled fan-shaped plate to resist deformation and fracture, which is not less than 100J. The higher the value, the better the plasticity of the cold-rolled fan-shaped plate, which helps to improve the fatigue performance.
[0053] Surface laser hardening:
[0054] The arc surface of the cold-rolled fan-shaped plate substrate is subjected to surface laser quenching treatment along the width direction, such as Figure 3-4 As shown, the spot width of the surface laser quenching is controlled to form an alternating soft and hard structure on the surface of the fan-shaped plate. The alternating width is controlled by the spot width. The spot width of the laser head is 10-12mm, forming a hardened layer. The surface hardness of the hardened layer reaches HRC45-50 (HV441-512), the depth of the hardened layer is 1-2mm, and the structure of the hardened layer includes martensite with a content of ≥90%, and the rest is austenite.
[0055] Surface strengthening:
[0056] The arc surface of the fan-shaped plate is laser quenched. The quenched area has a hardened layer with high hardness, and the non-quenched area maintains the original quenched and tempered structure and hardness of the matrix. When using surface strengthening, the main process parameters are related to the chemical composition of the material itself and the original grain structure.
[0057] Specifically, for ultrasonic impact, the magnitude of current and voltage determines the impact force on the workpiece surface, and is related to the chemical composition of the material itself and the original grain structure. The parameters of ultrasonic impact need to consider the performance of the hardened layer after surface laser quenching. For the quenching area, compressive stress is generated in the surface area through ultrasonic impact, and the organization is refined. If the ultrasonic impact energy in this area is too large, micro defects will be generated, and if the energy is too small, the required compressive stress will not be achieved; for the non-quenching area, the tensile stress generated by surface machining is eliminated by ultrasonic impact, and compressive stress is generated at the same time. If the ultrasonic impact energy in this area is too large, the thickening of the surface strengthening layer is not conducive to absorbing the impact work in the process of coiling the steel plate. If the energy is too small, the preset compressive stress is too small and the strengthening effect cannot be achieved.
[0058] Furthermore, the hardness ratio between the quenching area and the non-quenching area is controlled to be between 1.3-1.5, and the hardness difference is ≥HRC 10, so as to ensure that no micro defects will be generated at the transition between the quenching area and the non-quenching area. This effect is controlled by controlling the parameters of ultrasonic impact and surface laser quenching. The parameters of ultrasonic impact and surface laser quenching are different, and the energy applied to the material surface is different. Therefore, the present application controls the parameters of ultrasonic impact and surface laser quenching. The process parameters of ultrasonic impact are such as current <1.1A, voltage <14V, the thickness of the strengthening layer generated on the surface after impact is less than 100um, and the compressive stress in the non-quenching area is less than 150Mpa; if the current is >1.2A and the voltage is >16V, when the surface with hardness >HRC45 (HV441) is impacted, the hardened layer in the quenching area is a martensite structure with high strength, and the non-quenching area is a troostite structure with good toughness, and micro defects are easily generated at the intersection of the two. Therefore, the present invention has determined the ultrasonic impact process parameters through repeated experiments, which are suitable for both the quenching area and the non-quenching area and will not produce micro defects.
[0059] After ultrasonic impact, a thickness difference of ≥0.05mm appears between the hardened layer and the strengthening layer in the quenching area and the strengthening layer in the non-quenching area, and the thickness difference is controlled to be ≤0.2mm, preferably 0.01-0.2mm, so that the quenching area and the non-quenching area show micro-ripples. During the use of the steel rolling production line, the hardness difference of ≥HRC10 between the quenching area and the non-quenching area is used to make the wear amount of the non-quenching area greater than that of the quenching area. In the process of continuous friction and impact of the steel plate on the arc surface of the cold-rolled fan-shaped plate, the depth of the corrugation of the arc surface of the fan-shaped plate gradually increases, which is conducive to buffering the shear and impact pressure brought by the steel plate on the arc surface. The service life of the obtained cold-rolled fan-shaped plate reaches more than 12 months, which has significant economic benefits.
[0060] Compressive stress and tensile stress: After mechanical processing, the surface of the cold-rolled fan-shaped plate generates tensile stress. After surface laser quenching of the fan-shaped plate, the quenching area produces a structural transformation, and there is structural stress. In the later use process, the stress is gradually released, causing the cold-rolled fan-shaped plate to twist and deform, and even produce micro cracks on the surface. Therefore, it is necessary to further strengthen the surface of the fan-shaped plate after quenching. The tensile stress in the quenching area and the non-quenching area, after surface strengthening, under high-frequency and high-energy impact, first changes the stress field distribution on the surface of the cold-rolled fan-shaped plate, eliminates the tensile stress, and at the same time, the surface structure of the fan-shaped plate produces plastic deformation, and the strengthening layer produces a certain value of compressive stress, which buffers the shear and impact pressure of the steel plate on the curved surface of the fan-shaped plate during the coiling process.
[0061] Surface ripples:
[0062] The hardness difference between the quenching area and the non-quenching area of the fan-shaped plate is ≥HRC10. When the same impact process parameters are used to impact the surface of the cold-rolled fan-shaped plate, the surface hardness of the quenching area is high, the plastic deformation of the surface is small, and the surface deformation after impact is ≤0.05mm; while the hardness of the non-quenching area is low, the plastic deformation is large, and the deformation is 0.15-0.20mm. The difference in deformation between the quenching area and the non-quenching area is 0.05-0.2mm, which causes micro-ripples to appear in the quenching area and the non-quenching area of the cold-rolled fan-shaped plate surface.
[0063] Example 1
[0064] A preparation process for a cold-rolled sector plate comprises the following steps:
[0065] The chemical composition of the cold-rolled sector plate material is C: 0.30%, Mn: 0.50%, Si: 0.20%, P: 0.015%, S: 0.010%, Ni: 2.03%, Cr: 2.05%, and the balance is Fe.
[0066] The preparation process of the coiling shaft cold-rolled fan-shaped plate comprises the following steps:
[0067] Smelting → billet making → forging heat treatment → rough machining → quenching and tempering heat treatment → finishing → surface laser quenching → surface treatment, including:
[0068] (1) Smelting: The high-quality alloy is prepared according to the composition ratio and then smelted in an electric furnace, and LF refining and VD vacuum degassing processes are adopted.
[0069] (2) Billet making: Cut the steel ingot according to the weight required for the cold-rolled sector plate blank, heat it at a forging temperature of 1120°C, and then perform upsetting and drawing forging on a 10-ton forging hammer machine, with a forging ratio of 7±0.5;
[0070] (3) Forging heat treatment: reheat the forged billet to 1120±10℃, and then use a curved anvil for forging to ensure that the final forging temperature is around 920±10℃; ensure that the basic size of the forging billet meets the requirements of the billet drawing, slowly cool to 320±10℃ and keep warm for 6h after forging, then normalize at 920±10℃, quickly cool to 630±10℃ and temper for 6h, so that the banded structure reaches level 1 and the grain size reaches level 7; Figure 2 As shown in the figure, the arc surface of the cold-rolled sector plate formed by arc anvil forging has less material removal during rough machining, uniform structure, and refined grains, which improves the overall performance of the entire workpiece.
[0071] (4) Rough machining: Rough machining of the forging blank according to the drawing;
[0072] (5) Quenching and tempering heat treatment: The rough-processed cold-rolled sector plate is kept at 850±10℃ for 180min to austenitize, then oil-cooled to 150℃, and the maximum cooling rate of the quenching oil is maintained at 120℃ / s for quenching cooling, and then tempered at 580±10℃ for 6 hours. After tempering, it is taken out of the furnace and air-cooled. The matrix of the obtained cold-rolled sector plate includes: 95% troostite, the rest is bainite and ferrite, the content is 5%, the hardness is HB310 (HV317; HRC33.5), σ b :980MPa,σ s :870MPa, δ: 16%, Ψ: 62%, AK(u): 108J;
[0073] (6) Finishing: The cold-rolled sector plate after quenching and tempering shall be finished according to the drawing to meet the shape and position tolerance and roughness requirements of the drawing.
[0074] (7) Surface laser quenching treatment:
[0075] According to the arc-shaped part of the cold-rolled fan-shaped plate, a rectangular spot is used to perform surface laser quenching along the width direction of the cold-rolled fan-shaped plate. The surface laser quenching direction is as follows: Figure 3-4 As shown in the figure, the laser power determines the hardness and depth of the surface after laser quenching. The heat flux is high and the surface is easily burned and defects are generated. After testing, the depth L of the hardened layer after surface laser quenching on the curved surface of the cold-rolled fan-shaped plate meets the following requirements:
[0076]
[0077] In the formula, λ is the correction coefficient, and its value range is 0.20-0.30; P is the laser heat source power, unit is W; a is the spot width, unit is mm, which is basically the same as the quenching layer width; b is the spot length, unit is mm; v is the laser scanning speed, unit is mm / s.
[0078] In this embodiment, the parameters of the steel plate coiled by the cold-rolled fan-shaped plate are: thickness 2.8mm, width 1100mm; the laser power used is 2350W, the spot width is 11mm, the spot length is 7mm, the scanning speed is 7mm / s, the hardened layer L thickness is 1.18mm, the correction coefficient λ is 0.271, the hardened layer structure is: 95% martensite + 5% austenite structure, the surface hardness reaches HRC48-50 (HV482-512), the surface average hardness is HRC49 (HV497), and the cold-rolled fan-shaped plate arc surface quenching band width interval is 11mm. After the cold-rolled fan-shaped plate arc surface is laser quenched, a soft and hard band is formed. The non-quenched area retains the original tempered structure from the surface to the core of the quenched area. The structure of the quenched area gradually transitions from complete martensite to a mixed structure of troostite and ferrite in the matrix. The minimum tensile stress in the area 0.05mm from the surface is 110Mpa. From 0.05mm to 1mm from the surface, the stress value gradually transitions from tensile stress to compressive stress, and the compressive stress value is 80Mpa. In the non-quenched area between the quenched areas, the tensile stress value in the area 0.05mm from the surface is as low as 10Mpa. The existence of surface tensile stress will cause the stress to be gradually released during the later use of the cold-rolled sector plate, causing the cold-rolled sector plate to distort and deform, and even produce micro cracks on the surface.
[0079] (8) Surface strengthening treatment: The arc area of the cold-rolled fan-shaped plate is treated with ultrasonic impact strengthening process. The process parameters are: current 1.3A, resonance voltage 16V, vibration frequency 41KHz. After ultrasonic impact, a strengthening layer is formed. Its metallographic structure is as follows Figure 9-10 As shown, in the strengthening layer of the quenching area:
[0080] The tensile stress at 0.1mm away from the laser quenching surface is eliminated, the preset compressive stress is 230Mpa, the thickness of the strengthening layer formed on the surface is 0.12mm, the surface deformation is 0.03mm, the martensite content is 95%, and the surface structure grain refinement is level 7, such as Fig.10 As shown, the surface hardness reaches HRC53-55 (HV561-596), the average surface hardness is HRC54 (HV578), and the roughness is increased from the original 1.68um to 0.66um;
[0081] After surface strengthening, in the non-quenched area:
[0082] The thickness of the strengthening layer is 0.23mm, the surface deformation is 0.16mm, it contains 95% troostite, and the rest is bainite + ferrite, with a content of 5%. Fig. 9As shown in the figure, the compressive stress within 0.1mm from the surface reaches 368Mpa, the hardness is increased to HRC37-39 (HV350-371; HB341-360), and the average surface hardness is HRC38 (HV360). The roughness is increased from 1.48um of the substrate to 0.26um. The surface roughness leads to a decrease in the stress concentration factor in the valley, and the possibility of fatigue crack initiation is reduced. The difference in thickness and roughness of the strengthening layer formed under the same impact process causes a 0.15mm size thickness difference on the surface, such as Figure 3 As shown, the quenched area and the non-quenched area show micro-ripples. During the use of the steel rolling production line, the steel plate continuously rubs and impacts the arc surface of the cold-rolled fan-shaped plate. Since the average hardness difference between the quenched area and the non-quenched area is HRC16, the wear amount of the non-quenched area is greater than that of the quenched area. During the coiling process of the steel plate, the depth of the arc surface ripples gradually increases, which is conducive to buffering the shear and impact pressure of the steel plate on the arc surface of the fan-shaped plate.
[0083] like Figure 5-8 The stress and metallographic examination of the quenched and non-quenched areas show that before strengthening, the tensile stress in the quenched area at 0.1 mm from the surface is 110 MPa. Figure 5 As shown, the compressive stress in the non-quenched area is 5Mpa. Figure 7 As shown; after strengthening, the compressive stress in the quenched area at 0.1mm from the surface is 230MPa, as shown Figure 6 As shown in Figure 2, the compressive stress in the non-quenched area at 0.1 mm from the surface is 368 MPa. Figure 8 As shown, the compressive stress in both the quenched and non-quenched areas increases significantly. The compressive stress and hardness are positively correlated with fatigue properties and negatively correlated with tensile stress. The increase in compressive stress is beneficial to the improvement of product fatigue properties.
[0084] Example 2
[0085] The material of the cold-rolled sector plate in Example 2 is the same as that in Example 1. The cold-rolled sector plate manufactured in Example 2 is mainly used for coiling 2 mm thick steel plates.
[0086] The base material of the cold-rolled sector plate is 92% troostite, the rest is bainite and a very small amount of ferrite, the hardness is HB295 (HV301; HRC31.6), σ b :950MPa,σ s :840MPa, δ: 18%, Ψ: 65%, AK(u): 115J.
[0087] Since the thickness of the coiled steel plate is thinner than that of Example 1, when the weight of the steel coil is constant, the thickness of the steel plate decreases, the number of steel coil layers increases, and the impact force on the surface of the cold-rolled fan-shaped plate during the coiling process decreases. Therefore, the surface laser quenching process parameters are controlled as follows: laser power: 2300 W, spot width 10.5 mm, spot length 6 mm, scanning speed 7.5 mm / s, correction coefficient λ 0.226, depth of hardened layer obtained by quenching: 1.1 mm, hardened layer structure of 92% martensite and 8% austenite, surface hardness of HRC47-49 (HV468-497), surface average hardness of HRC48 (HV482), and quenching bandwidth interval of 11 mm.
[0088] After surface laser quenching, the tensile stress in the area 0.05mm from the surface is 26.5Mpa; in the area 0.1mm, the compressive stress value is 29Mpa; and the tensile stress value in the non-quenched area 0.01mm reaches 118Mpa.
[0089] Ultrasonic impact process parameters: working current 1.2A, resonance voltage 15V, vibration frequency 40kHz. After impact strengthening, a strengthening layer is formed, in which the quenching area:
[0090] The tensile stress at 0.1mm from the laser quenching surface is eliminated, the preset compressive stress is 272Mpa, the thickness of the strengthening layer formed on the surface is 0.10mm, the surface deformation is 0.03mm, the martensite content is ≥92%, the surface structure grain refinement is 8 levels, the surface hardness reaches HRC52-54 (HV544-578), the surface average hardness is HRC53 (HV561), and the roughness is increased from the original 1.54um to 0.62um;
[0091] In the non-quenching area:
[0092] The thickness of the strengthening layer is 0.25mm, the surface deformation is 0.18mm, it contains 93% troostite, the rest is bainite and ferrite, the content is 7%, the compressive stress within 0.1mm from the surface reaches 168Mpa, the hardness is increased to HRC36-38 (HV340-360), the average surface hardness is HRC37 (HV350), and the roughness is increased from the original 1.42um to 0.23um. Under the same impact process, there is a 0.15mm size thickness difference between the quenched area and the non-quenched area, which makes the quenched area and the non-quenched area show micro-ripples, and the hardness difference is HRC16.
[0093] Example 3
[0094] The material of the cold-rolled sector plate in Example 3 is the same as that in Example 1. The cold-rolled sector plate manufactured in Example 3 is mainly used for coiling a 2.3 mm thick steel plate. The base material of the cold-rolled sector plate is 90% troostite, the rest is bainite and a very small amount of ferrite, the hardness is HB285 (HV290; HRC30.3), σ b :920MPa,σ s :830MPa, δ: 19%, Ψ: 67%, AK(u): 122J.
[0095] The control surface laser quenching process parameters are: laser power: 2240W, spot width 11.5mm, spot length 6mm, scanning speed 6.5mm / s, correction coefficient λ 0.216, quenching hardened layer depth: 1.08mm, hardened layer structure is 91% martensite and 9% austenite, surface hardness is HRC45-48 (HV441-482), surface average hardness is HRC46.5 (HV461), quenching bandwidth interval is 10mm;
[0096] After surface laser quenching, the tensile stress in the area 0.05mm from the surface is 24Mpa; the compressive stress in the area 0.1mm is 26Mpa; the tensile stress in the non-quenched area reaches 112Mpa.
[0097] Ultrasonic impact process parameters: working current 1.2A, resonance voltage 15V, vibration frequency 40kHz. After impact strengthening, a strengthening layer is formed, in which the quenching area:
[0098] The tensile stress at 0.1mm from the laser quenching surface is eliminated, the preset compressive stress is 264Mpa, the thickness of the strengthening layer formed on the surface is 0.14mm, the surface deformation is 0.04mm, the martensite content is ≥90%, the surface structure grain refinement is 8 levels, the surface hardness reaches HRC50-53 (HV512-561), the surface average hardness is HRC51.5 (HV535), and the roughness is increased from the original 1.60um to 0.68um;
[0099] In the non-quenching area:
[0100] The thickness of the strengthening layer is 0.22mm, the surface deformation is 0.15mm, it contains 92% troostite, the rest is bainite and ferrite, the content is 8%, the compressive stress within 0.1mm from the surface reaches 160Mpa, the hardness is increased to HRC36-38 (HV340-360; HB332-350), the average surface hardness is HRC37 (HV350), and the roughness is increased from the original 1.38um to 0.18um. The difference in thickness and roughness of the strengthening layer formed under the same impact process causes a 0.11mm size thickness difference on the surface, causing the quenched area and the non-quenched area to show micro-ripples, and the hardness difference is ≥HRC10.
[0101] Example 4
[0102] Example 4: The cold-rolled sector plate is strengthened by surface laser quenching and ultrasonic shot peening in sequence. The process parameters of surface laser quenching are the same as those of Example 1. The process parameters of ultrasonic shot peening are shot peening time of 60 min, ultrasonic amplitude of 40 um, shot diameter of 5 mm, and shot peening distance of 20 mm. The parameters of the obtained product are as follows: the compressive stress of the original quenching area at 0.08 mm from the surface is 150 MPa, the thickness of the strengthening layer formed on the surface after ultrasonic shot peening is 0.08 mm, the surface structure grain refinement is level 7, the surface hardness reaches HRC51-53 (HV527-561), and the surface average hardness is 1.374 W / cm2. The surface hardness is HRC52 (HV544), and the roughness is reduced from the original 1.68um to 1.82um; after ultrasonic shot peening in the non-quenched area, the thickness of the strengthening layer is 0.15mm, so that the compressive stress within 0.1mm from the surface reaches 180Mpa, the hardness is increased to HRC35-38 (HV331-360), the average surface hardness is HRC36.5 (HV347), the roughness is reduced from the original 1.48um to 1.66um, and a 0.05mm size thickness difference appears on the surface. The surface laser quenching area and the non-quenching area show micro-ripples, and the hardness difference is ≥HRC10.
[0103] Example 5
[0104] Example 5: The cold rolled sector plate is strengthened by surface laser quenching and laser shot peening in sequence. The process parameters of surface laser quenching are the same as those of Example 1, and the process parameters of laser shot peening are: pulse energy 6J, pulse power density 5GW / cm 2, pulse width 30ns, the parameters of the obtained product are: the compressive stress of the original quenching area at 0.08mm away from the surface is 180Mpa, the thickness of the strengthening layer formed on the surface is 0.65mm, the surface grain refinement is level 7, the surface hardness reaches HRC53-55 (HV561-596), the surface average hardness is HRC54 (HV578), and the roughness is reduced from the original 1.68um to 2.62um; after ultrasonic shot peening in the non-quenching area, the compressive stress within 0.1mm from the surface reaches 230Mpa, the thickness of the strengthening layer formed on the surface is 0.83mm, the hardness is increased to HRC37-39 (HV350-371), the surface average hardness is HRC38 (HV360), the roughness is reduced from the original 1.48um to 2.76um, and a size thickness difference of 0.07mm appears on the surface. The surface laser quenching area and the non-quenching area show micro-ripples, and the hardness difference is ≥HRC10.
[0105] Comparative Example 1
[0106] In Comparative Example 1, the arc surface of the cold-rolled sector plate is only subjected to surface laser quenching without ultrasonic strengthening treatment.
[0107] The material of the cold-rolled sector plate in Comparative Example 1 is the same as that in Example 1. The base material of the cold-rolled sector plate comprises 96% troostite, the remaining 4% bainite and a very small amount of ferrite, the base hardness is HB290 (HV295; HRC30.8), and the base satisfies: σ b :940MPa,σ s :850MPa, δ: 18%, Ψ: 69%, AK(u): 126J.
[0108] The control surface laser quenching process parameters are: laser power: 2380W, spot width 11mm, spot length 7mm, scanning speed 7mm / s, correction coefficient λ 0.260, quenching hardened layer depth: 1.15mm, microstructure is 94% martensite and 6% austenite, surface hardness is HRC47-49 (HV468-497), surface average hardness is HRC48 (HV482), quenching bandwidth interval is 11mm;
[0109] After surface laser quenching, the tensile stress in the area 0.05mm from the surface is 27Mpa; the compressive stress at 0.1mm is 24Mpa; the stress value in the non-quenched area reaches 116Mpa.
[0110] It can be seen that there is tensile stress on the surface of the workpiece. In the process of coiling the steel plate, the arc surface is easily deformed and microcracks are easily generated under the action of surface tensile stress, causing the workpiece to break. The fan-shaped plate product was used for 8 months before strengthening, and there were wear and microcracks on the surface; after strengthening, there were no microcracks on the surface after 1 year of use.
[0111] The performance parameters of the products obtained in Examples 1-5 and Comparative Example 1 are shown in Table 1, wherein the fatigue performance of the products is close to the prediction law of gear fatigue performance. According to the literature such as "Science China. Technological Sciences: Research on Basic Technology of High-Performance Gears" and "Experimental Investigation of the Relation between the Surface Integrity and Bending Fatigue Strength of Carburized Gears", the prediction calculation formula related to fatigue performance, surface hardness and stress is:
[0112]
[0113] Wherein, σ is fatigue performance, SR is residual stress (MPa), SH is surface hardness (HV), and the fatigue performance calculation results are shown in Tables 1 and 2. In the table, tensile stress is a positive value and compressive stress is a negative value. The conversion of hardness units is based on GB / T 1172-1999 "Conversion Values of Hardness and Strength of Ferrous Metals".
[0114] From the calculation of fatigue performance prediction data, it can be seen that compressive stress and hardness are positively correlated with fatigue performance, and negatively correlated with tensile stress. After strengthening treatment, the hardness value, compressive stress and distribution depth of compressive stress of the product are significantly improved, which effectively improves fatigue performance. When the steel plate is subjected to bending, shearing, impact and other loads during coiling, the wear resistance, bending and fatigue resistance are improved. Finally, the product has been verified through use and its service life is at least 4 months longer than that of products manufactured by the original process.
[0115] Table 1 Performance parameters of the quenching area of the products in Examples 1-5 and Comparative Example 1 before and after surface strengthening treatment
[0116]
[0117] Table 2 Performance parameters of the non-quenching area of the products in Examples 1-5 and Comparative Example 1 before and after surface strengthening treatment
[0118]
[0119] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope involved in the present application is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept, such as a technical solution formed by replacing the above-mentioned features with (but not limited to) technical features with similar functions disclosed in this application.
[0120] Except for the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described here in detail.
Claims
1. A process for preparing a cold-rolled sector plate, characterized in that: The substrate of the cold-rolled sector plate is subjected to a surface laser quenching process to obtain a hardened layer with intervals, and then subjected to a surface strengthening process to obtain a strengthening layer, so that a quenched area and a non-quenched area are formed on the surface of the cold-rolled sector plate, the quenched area includes the substrate, the hardened layer generated on the substrate surface and the strengthening layer generated on the hardened layer surface, the non-quenched area includes the substrate and the strengthening layer generated on the substrate surface, and the quenched area and the non-quenched area are sequentially spaced along the surface laser quenching direction; The surface hardness difference between the quenching area and the non-quenching area is ≥HRC10; The thickness difference between the hardened layer and the strengthening layer in the quenching area and the strengthening layer in the non-quenching area is 0.05-0.2 mm; The surface laser quenching process adopts a rectangular spot to perform surface laser quenching along the width direction of the cold-rolled sector plate. The depth L of the hardened layer formed on the surface of the cold-rolled sector plate after the surface laser quenching satisfies: Where, λ is the correction coefficient; P is the laser heat source power, unit W; a is the spot width, unit mm; b is the spot length, unit mm; v is the laser scanning speed, unit mm / s; The surface strengthening process is selected from one of ultrasonic impact, ultrasonic shot peening and laser shot peening.
2. The preparation process according to claim 1, characterized in that: The correction coefficient λ is 0.20-0.30, the laser power P is 2000-2400W, the spot width a is 10-12mm, the spot length b is 6-8mm, the scanning speed v is 6-8mm / s, and the thickness of the hardened layer L is 1mm≤L≤1.2mm.
3. The preparation process according to claim 2, characterized in that: The surface strengthening process is ultrasonic impact, and the process parameters of ultrasonic impact are: current is 1.2±0.1A, resonance voltage is 15±1V, and vibration frequency is 40±2KHz.
4. The preparation process according to claim 3, characterized in that: The matrix satisfies: 900MPa≤σb≤1000MPa, 800MPa≤σs≤900MPa, 15%≤δ≤20%, 60%≤Ψ≤70%, AKu≥100J, and the surface hardness of the matrix satisfies HRC29.5-34.7 or HB280-320.
5. The preparation process according to claim 4, characterized in that: In the matrix, the content of troostite is ≥90%, and the rest is bainite and ferrite.
6. The preparation process according to claim 5, characterized in that: The preparation process of the cold-rolled sector plate comprises the following steps: smelting→blank making→forging heat treatment→rough machining→quenching and tempering heat treatment→finishing→surface laser quenching→surface strengthening treatment.
7. A cold-rolled sector plate produced by the preparation process according to any one of claims 1 to 6, characterized in that: It includes a quenching area and a non-quenching area, the quenching area includes a substrate, a hardened layer generated on the surface of the substrate and a strengthening layer generated on the surface of the hardened layer, the non-quenching area includes a substrate and a strengthening layer generated on the surface of the substrate, the quenching area and the non-quenching area are distributed in sequence along the surface laser quenching direction, the thickness difference between the hardened layer and the strengthening layer in the quenching area and the strengthening layer in the non-quenching area is 0.05-0.2mm; the surface hardness difference between the quenching area and the non-quenching area is ≥HRC10.
8. The cold-rolled sector plate according to claim 7, characterized in that: The hardness ratio between the quenched area and the non-quenched area is 1.3-1.
5.
9. The cold-rolled sector plate according to claim 7, characterized in that: The interval between the quenching area and the non-quenching area is 10-12 mm.
10. The cold-rolled sector plate according to claim 7, characterized in that: The thickness of the hardened layer in the quenching area is: 1mm≤δ≤1.2mm, the metallographic structure includes martensite with a content of ≥90%, and the rest is austenite, and the surface hardness of the hardened layer is HRC45-50.
11. The cold-rolled sector plate according to claim 7, characterized in that: After surface strengthening treatment, the hardness of the quenching area is HRC50-55, the metallographic structure includes martensite with a content of ≥90%, and the thickness of the strengthening layer is 0.05mm-0.15mm.
12. The cold-rolled sector plate according to claim 7, characterized in that: The hardness of the non-quenched area is HRC35.8-39, the metallographic structure includes troostite with a content of ≥90%, and the rest is bainite and ferrite, and the thickness of the strengthening layer is 0.2mm-0.25mm.
13. The cold-rolled sector plate according to claim 7, characterized in that: The matrix includes troostite with a content of ≥90%, and the rest is bainite and ferrite, and the matrix hardness meets HRC29.5-34.7.