A method for preparing nano tungsten powder using waste cemented carbide
Through the steps of oxidation and roasting, stirring and hydrogen reduction, the coordinated reduction of tungsten acid and tungsten oxide mixed powder was used to solve the problems of impurities introduction and low purity in waste cemented carbide recycling, and high-performance nanotungsten powder was prepared to realize tungsten efficient recycling and efficient utilization of resources.
Patent Information
- Application Number
- CN202411114893.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing waste cemented carbide recycling technology has problems such as the introduction of impurities, low purity, cumbersome process, high energy consumption and environmental pollution. The preparation methods of nanotungsten powder have their own limitations, making it difficult to obtain high-performance nanotungsten powder.
The steps of oxidation roasting, crushing, hydrochloric acid stirring and heating, washing and hydrogen reduction are adopted, and the mixed powder of tungsten acid and tungsten oxide are used to prepare nanotungsten powder, control the particle size and morphology, and achieve efficient recycling and resource utilization of tungsten.
The uniformization of nano-tungsten powder is achieved, with an average particle size of ≤55nm and a tungsten recovery rate of up to 93.24%. It has simple equipment, simple operation, and small environmental pollution, which has increased the added value of the product.
Smart Images

Figure CN118621158B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource processing of waste cemented carbide, and specifically relates to a method for preparing nano tungsten powder by utilizing waste cemented carbide. Background Art
[0002] At present, the recycling technologies of waste cemented carbide mainly include zinc melting method, electrolysis method, mechanical crushing method, high temperature treatment method and sodium sulfate smelting method. Although these methods have achieved the recycling of cemented carbide to a certain extent, there are still some problems that need to be solved. For example, the zinc melting method is easy to introduce impurities when recycling high-cobalt cemented carbide and powder materials, resulting in low purity of the recycled powder; although the electrolysis method has high purity, the process is cumbersome, the cost is high and there is a large loss; the mechanical crushing method is difficult to achieve a complete separation of the bonding phase and the hard phase when processing high-cobalt cemented carbide, and it is easy to introduce impurities and oxygen; the high temperature treatment method has huge energy consumption, and the cobalt element is easy to lose during the recycling process, which limits the application scope of the recycled material; the sodium sulfate smelting method has the risk of environmental pollution.
[0003] In addition, with the continuous advancement of nanomaterial technology, the preparation technology of nano tungsten powder has also received widespread attention. Nano tungsten powder has shown great application potential in many fields due to its unique physical and chemical properties. For example, nano tungsten powder can be used to manufacture high-performance electronic devices and catalysts, and can also be used in medical and energy storage fields. At present, the preparation methods of nano tungsten powder mainly include high-energy ball milling, gas evaporation, plasma, self-propagating high-temperature reduction and tungsten oxide powder reduction. These methods have their own advantages and limitations. Choosing a suitable preparation process is crucial to obtaining high-performance nano tungsten powder. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a method for preparing nano tungsten powder by using waste cemented carbide.
[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0006] A method for preparing nano tungsten powder using waste cemented carbide comprises the following steps:
[0007] S1. Oxidative roasting of waste cemented carbide;
[0008] S2, crushing the waste cemented carbide after oxidation roasting into waste cemented carbide powder with a particle size less than 0.25 mm;
[0009] S3, adding hydrochloric acid to the waste cemented carbide powder to obtain a slurry, and adding an organic dispersant and stirring and heating;
[0010] S4, filtering the stirred liquid, first washing it with dilute hydrochloric acid, then washing it with distilled water, and finally washing it with alcohol to obtain a moist yellow solid powder;
[0011] S5. The yellow solid powder is air-dried and then reduced with hydrogen to obtain nano tungsten powder.
[0012] As a preferred embodiment of the method for preparing nano tungsten powder by using waste cemented carbide described in the present invention, wherein: in the step S1, the roasting temperature is 600-900°C, and the roasting time is 3-8h.
[0013] As a preferred embodiment of the method for preparing nano tungsten powder by using waste cemented carbide described in the present invention, wherein: in the step S1, the stains on the surface of the waste cemented carbide are washed away with acetone and then placed in a muffle furnace for oxidation roasting.
[0014] As a preferred embodiment of the method for preparing nano-tungsten powder by using waste cemented carbide described in the present invention, in step S2, a jaw crusher is used for crushing.
[0015] As a preferred embodiment of the method for preparing nano tungsten powder using waste cemented carbide described in the present invention, wherein: in the step S3, the concentration of hydrochloric acid is 25-36wt%, and the liquid-to-solid ratio of hydrochloric acid to waste cemented carbide powder is (3-7)mL:1g.
[0016] As a preferred embodiment of the method for preparing nano tungsten powder by using waste cemented carbide described in the present invention, wherein: in the step S3, the volume ratio of the organic dispersant to the slurry is (1-3):5.
[0017] As a preferred embodiment of the method for preparing nano tungsten powder using waste cemented carbide described in the present invention, wherein: in the step S3, stirring and heating are carried out in a heat-collecting constant temperature magnetic stirrer, the temperature is controlled to be 80-100°C, the magnetic stirring speed is 400-600r / min, and the stirring time is 2-6h.
[0018] As a preferred embodiment of the method for preparing nano-tungsten powder by using waste cemented carbide described in the present invention, wherein: in the step S4, suction filtration is performed in a Buchner funnel.
[0019] As a preferred embodiment of the method for preparing nano tungsten powder using waste cemented carbide described in the present invention, wherein: in the step S5, hydrogen reduction is carried out in a tubular furnace, the hydrogen flow rate is 3-5 L / min, and the heating rate is 10°C / min.
[0020] As a preferred embodiment of the method for preparing nano tungsten powder by using waste cemented carbide according to the present invention, in step S5, a staged reduction process is adopted:
[0021] The first stage reduction temperature is 300~350℃, and the reduction time is 0.5~1h;
[0022] The second stage reduction temperature is 500~550℃, and the reduction time is 1~3h;
[0023] The third stage reduction temperature is 650~700℃, and the reduction time is 1~3h.
[0024] The beneficial effects of the present invention are as follows:
[0025] The present invention proposes a method for preparing nano tungsten powder using waste cemented carbide, wherein waste cemented carbide is used to prepare nano tungsten powder, and tungstic acid and tungsten oxide mixed powder are innovatively used to synergistically reduce and inhibit the volatilization, deposition and growth of tungsten to prepare nano tungsten powder, which can effectively control the particle size and morphology of nano tungsten powder, so that the prepared nano tungsten powder is uniform, and the average particle size of the prepared nano tungsten powder is ≤55nm. The present invention does not require the addition of additional substances and has less environmental pollution; the equipment is simple and easy to operate, saving manpower and equipment costs; it can not only realize the recovery of tungsten resources, with a tungsten recovery rate of 93.24%, but also increase the added value of products and realize efficient utilization of resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0027] Figure 1 This is the XRD diagram of the waste cemented carbide after sintering in Example 1 of the present invention.
[0028] Figure 2 This is the XRD pattern of the wet yellow solid powder in Example 1 of the present invention.
[0029] Figure 3 This is the XRD pattern of the nano tungsten powder prepared in Example 1 of the present invention.
[0030] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0031] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] According to one aspect of the present invention, the present invention provides the following technical solution:
[0033] A method for preparing nano tungsten powder using waste cemented carbide comprises the following steps:
[0034] S1. Oxidative roasting of waste cemented carbide;
[0035] S2, crushing the waste cemented carbide after oxidation roasting into waste cemented carbide powder with a particle size less than 0.25 mm;
[0036] S3, adding hydrochloric acid to the waste cemented carbide powder to obtain a slurry, and adding an organic dispersant and stirring and heating;
[0037] S4, filtering the stirred liquid, first washing it with dilute hydrochloric acid, then washing it with distilled water, and finally washing it with alcohol to obtain a moist yellow solid powder;
[0038] S5. The yellow solid powder is air-dried and then reduced with hydrogen to obtain nano tungsten powder.
[0039] Preferably, in step S1, the waste cemented carbide is placed in a muffle furnace for roasting after stains on the surface of the waste cemented carbide are washed away with acetone; the roasting temperature is 600-900° C. and the roasting time is 3-8 hours; the waste cemented carbide with a dense structure is roasted into an expanded and loose structure under oxygen conditions.
[0040] Preferably, in step S2, a jaw crusher is used for crushing.
[0041] Preferably, in step S3, the concentration of hydrochloric acid is 25-36wt%, and the liquid-solid ratio of hydrochloric acid to waste cemented carbide powder is (3-7)mL:1g; the volume ratio of organic dispersant to slurry is (1-3):5; stirring and heating in a heat-collecting constant temperature magnetic stirrer, the temperature is controlled to be 80-100°C, the magnetic stirring speed is 400-600r / min, and the stirring time is 2-6h. The organic dispersant can be, for example, alcohol. This step can remove impurities such as iron, cobalt, nickel, and chromium. At the same time, concentrated hydrochloric acid can accelerate and promote the conversion of cobalt tungstate into powdered yellow tungstic acid to a certain extent because of its high concentration, so there is no need to add an oxidant. At this time, the water-insoluble solid is a mixed powder of tungsten trioxide and tungstic acid, and the solution is impurities and CoCl2. Organic dispersant alcohol can disperse tungstic acid and tungsten oxide particles through a variety of mechanisms: solvent effect, forming hydrogen bonds with polar compounds such as tungstic acid and tungsten oxide, thereby helping them to disperse; reducing surface tension and preventing agglomeration, alcohol adsorbs on the surface of tungstic acid and tungsten oxide to form a protective film, reducing direct contact between particles, thereby preventing them from agglomerating. The purpose of stirring is to completely transform cobalt tungstate into tungstic acid, while making tungstic acid and tungsten oxide evenly distributed; at the same time, it can also completely convert solid impurities into ions. If not stirred sufficiently, the tungsten recovery rate will be low, the impurities will be high, and the distribution of tungstic acid and tungsten oxide will be uneven, resulting in poor uniformity of the particle size distribution of the obtained tungsten powder. Similarly, heating is also to make the cobalt tungstate transform more thoroughly and quickly.
[0042] Preferably, in step S4, suction filtration is performed in a Buchner funnel. The purpose of washing is to further remove impurities and purify, and finally washing with alcohol can achieve the above-mentioned effects and improve air-drying efficiency.
[0043] Preferably, in step S5, hydrogen reduction is carried out in a tubular furnace, the hydrogen flow rate is 3-5 L / min, and the heating rate is 10° C. / min; a staged reduction process is adopted:
[0044] The first stage reduction temperature is 300~350℃, and the reduction time is 0.5~1h;
[0045] The second stage reduction temperature is 500~550℃, and the reduction time is 1~3h;
[0046] The third stage reduction temperature is 650~700℃, and the reduction time is 1~3h.
[0047] By setting multiple temperatures, the particle size of tungsten can be refined to avoid the rapid growth of tungsten powder due to excessive reaction. The mixed powder has a more irregular shape than the single tungsten acid or tungsten oxide powder, which can promote the formation of tungsten. At the same time, the synergistic reduction of tungsten acid and tungsten oxide mixed powder can inhibit the volatilization, deposition and growth of tungsten. The principle is: tungsten acid is adsorbed on the surface of tungsten oxide in solution and crystallized. Then in the tube furnace, the first temperature is the thermal decomposition of tungsten acid to form tungsten oxide and water vapor. The newly formed tungsten oxide is also formed on the original tungsten oxide, and the water vapor enters the tail pipe with hydrogen; the second and third temperatures are used to control the reduction path of tungsten oxide to achieve the purpose of refining tungsten powder. At the same time, during the reduction process, the water vapor decomposed from the original and newly generated tungsten oxide can be adsorbed by the newly generated tungsten oxide and then reduced, thereby inhibiting the volatilization, deposition and growth.
[0048] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0049] Example 1
[0050] A method for preparing nano tungsten powder using waste cemented carbide comprises the following steps:
[0051] S1. Use acetone to wash away the stains on the surface of the waste cemented carbide and then put it into a muffle furnace for oxidation roasting. The roasting temperature is 850℃ and the roasting time is 5h. The XRD pattern of the waste cemented carbide after roasting is as follows: Figure 1 As shown;
[0052] S2. The waste cemented carbide after oxidation roasting is crushed into waste cemented carbide powder with a particle size less than 0.25 mm by a jaw crusher;
[0053] S3, adding hydrochloric acid to the waste cemented carbide powder to obtain a slurry, and adding alcohol to stir and heat; the concentration of hydrochloric acid is 36wt%, the liquid-solid ratio of hydrochloric acid to the waste cemented carbide powder is 3mL:1g; the volume ratio of alcohol to the slurry is 2:5; stirring and heating in a heat-collecting constant temperature magnetic stirrer, the temperature is controlled at 100°C, the magnetic stirring speed is 500r / min, and the stirring time is 4h;
[0054] S4. The stirred liquid is filtered in a Buchner funnel, first washed with dilute hydrochloric acid, then washed with distilled water, and finally washed with alcohol to obtain a wet yellow solid powder; the XRD pattern of the wet yellow solid powder is as follows: Figure 2 As shown;
[0055] S5. After the yellow solid powder is air-dried, it is reduced by hydrogen in a tubular furnace with a hydrogen flow rate of 5 L / min and a heating rate of 10°C / min. A staged reduction process is adopted: the first stage reduction temperature is 350°C and the reduction time is 1h; the second stage reduction temperature is 550°C and the reduction time is 2h; the third stage reduction temperature is 700°C and the reduction time is 2h; and nano tungsten powder is obtained.
[0056] The XRD pattern of the nano tungsten powder prepared in this example is as follows: Figure 3 As shown, the average particle size is 48 nm, and the recovery rate of tungsten is 95.38% (the recovery rate of tungsten in each embodiment and comparative example = the mass of nano tungsten powder / the mass of tungsten in waste cemented carbide).
[0057] Example 2
[0058] A method for preparing nano tungsten powder using waste cemented carbide comprises the following steps:
[0059] S1. Wash the stains on the surface of the waste cemented carbide with acetone and then put it into a muffle furnace for oxidation roasting. The roasting temperature is 700°C and the roasting time is 8h;
[0060] S2. The waste cemented carbide after oxidation roasting is crushed into waste cemented carbide powder with a particle size less than 0.25 mm by a jaw crusher;
[0061] S3, adding hydrochloric acid to the waste cemented carbide powder to obtain a slurry, and adding alcohol to stir and heat; the concentration of hydrochloric acid is 32wt%, the liquid-solid ratio of hydrochloric acid to the waste cemented carbide powder is 7mL:1g; the volume ratio of alcohol to the slurry is 3:5; stirring and heating in a heat-collecting constant temperature magnetic stirrer, the temperature is controlled at 90°C, the magnetic stirring speed is 600r / min, and the stirring time is 6h;
[0062] S4, filtering the stirred liquid in a Buchner funnel, washing it with dilute hydrochloric acid, then washing it with distilled water, and finally washing it with alcohol to obtain a moist yellow solid powder;
[0063] S5. After the yellow solid powder is air-dried, it is reduced by hydrogen in a tubular furnace with a hydrogen flow rate of 3 L / min and a heating rate of 10°C / min. A staged reduction process is adopted: the first stage reduction temperature is 300°C and the reduction time is 0.5h; the second stage reduction temperature is 500°C and the reduction time is 1h; the third stage reduction temperature is 650°C and the reduction time is 1h. Nano tungsten powder is obtained. The average particle size of the nano tungsten powder prepared in this embodiment is 45nm, and the tungsten recovery rate is 93.87%.
[0064] Example 3
[0065] A method for preparing nano tungsten powder using waste cemented carbide comprises the following steps:
[0066] S1. Wash the stains on the surface of the waste cemented carbide with acetone and then put it into a muffle furnace for oxidation roasting. The roasting temperature is 900°C and the roasting time is 7h;
[0067] S2. The waste cemented carbide after oxidation roasting is crushed into waste cemented carbide powder with a particle size less than 0.25 mm by a jaw crusher;
[0068] S3, adding hydrochloric acid to the waste cemented carbide powder to obtain a slurry, and adding alcohol to stir and heat; the concentration of hydrochloric acid is 28wt%, the liquid-solid ratio of hydrochloric acid to the waste cemented carbide powder is 5mL:1g; the volume ratio of alcohol to the slurry is 2:5; stirring and heating in a heat-collecting constant temperature magnetic stirrer, the temperature is controlled to 80°C, the magnetic stirring speed is 600r / min, and the stirring time is 4h;
[0069] S4, filtering the stirred liquid in a Buchner funnel, washing it with dilute hydrochloric acid, then washing it with distilled water, and finally washing it with alcohol to obtain a moist yellow solid powder;
[0070] S5. After air-drying the yellow solid powder, the powder was reduced by hydrogen in a tubular furnace with a hydrogen flow rate of 4 L / min and a heating rate of 10°C / min. A staged reduction process was adopted: the first stage reduction temperature was 350°C and the reduction time was 1 h; the second stage reduction temperature was 550°C and the reduction time was 1 h; the third stage reduction temperature was 700°C and the reduction time was 2 h. Nano tungsten powder was obtained. The average particle size of the nano tungsten powder prepared in this embodiment was 52 nm, and the tungsten recovery rate was 95.86%.
[0071] Example 4
[0072] A method for preparing nano tungsten powder using waste cemented carbide comprises the following steps:
[0073] S1. Wash the stains on the surface of the waste cemented carbide with acetone and then put it into a muffle furnace for oxidation roasting. The roasting temperature is 600°C and the roasting time is 8h;
[0074] S2. The waste cemented carbide after oxidation roasting is crushed into waste cemented carbide powder with a particle size less than 0.25 mm by a jaw crusher;
[0075] S3, adding hydrochloric acid to the waste cemented carbide powder to obtain a slurry, and adding alcohol to stir and heat; the concentration of hydrochloric acid is 30wt%, the liquid-solid ratio of hydrochloric acid to the waste cemented carbide powder is 4mL:1g; the volume ratio of alcohol to the slurry is 1:5; stirring and heating in a heat-collecting constant temperature magnetic stirrer, the temperature is controlled at 90°C, the magnetic stirring speed is 600r / min, and the stirring time is 3h;
[0076] S4, filtering the stirred liquid in a Buchner funnel, washing it with dilute hydrochloric acid, then washing it with distilled water, and finally washing it with alcohol to obtain a moist yellow solid powder;
[0077] S5. After the yellow solid powder is air-dried, it is reduced by hydrogen in a tubular furnace with a hydrogen flow rate of 5 L / min and a heating rate of 10°C / min. A staged reduction process is adopted: the first stage reduction temperature is 300°C and the reduction time is 1 h; the second stage reduction temperature is 500°C and the reduction time is 2 h; the third stage reduction temperature is 700°C and the reduction time is 2 h. Nano tungsten powder is obtained. The average particle size of the nano tungsten powder prepared in this embodiment is 55 nm, and the tungsten recovery rate is 93.24%.
[0078] Comparative Example 1
[0079] The difference from Example 1 is that the calcination temperature in step S1 is 500° C. and the calcination time is 8 hours.
[0080] The scrap hard alloy in this comparative example slightly expanded and deformed, was difficult to crush, and ultimately failed to be recycled.
[0081] Comparative Example 2
[0082] The difference from Example 1 is that the calcination time in step S1 is 1 hour.
[0083] The scrap hard alloy in this comparative example slightly expanded and deformed, was difficult to crush, and ultimately failed to be recycled.
[0084] Comparative Example 3
[0085] The difference from Example 1 is that the concentration of hydrochloric acid in step S3 is 20 wt %.
[0086] In this comparative example, a moist green solid powder was obtained after alcohol washing; analysis showed that the green solid powder was a mixture of cobalt tungstate and tungsten trioxide, and recovery failed.
[0087] Comparative Example 4
[0088] The difference from Example 1 is that no alcohol is added in step S3.
[0089] In this comparative example, a moist green solid powder was obtained after alcohol washing; analysis showed that the green solid powder was a mixture of cobalt tungstate and tungsten trioxide, and recovery failed.
[0090] Comparative Example 5
[0091] The difference from Example 1 is that a staged reduction process is adopted in step S5: the first stage reduction temperature is 300° C., and the reduction time is 0.5 h; the second stage reduction temperature is 700° C., and the reduction time is 4 h; tungsten powder is obtained.
[0092] The average particle size of the tungsten powder prepared in this comparative example is 164 nm, and the recovery rate of tungsten is 94.54%.
[0093] Comparative Example 6
[0094] The difference from Example 1 is that the third stage reduction temperature in step S5 is 900°C.
[0095] This comparative example finally obtained a mixed powder of tungsten powder and tungsten oxide, and the recovery failed.
[0096] It can be seen from the above embodiments and comparative examples that the present invention uses waste cemented carbide to prepare nano tungsten powder, innovatively uses tungstic acid and tungsten oxide mixed powder to synergistically reduce and inhibit the volatilization, deposition and growth of tungsten to prepare nano tungsten powder, can effectively control the particle size and morphology of nano tungsten powder, make the prepared nano tungsten powder uniform, and the average particle size of the prepared nano tungsten powder is ≤55nm. The present invention does not require the addition of additional substances and has less environmental pollution; the equipment is simple and easy to operate, saving manpower and equipment costs; it can not only realize the recovery of tungsten resources, with a tungsten recovery rate of 93.24%, but also increase the added value of the product and achieve efficient utilization of resources.
[0097] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing nano tungsten powder using waste cemented carbide, characterized in that: The steps include: S1. Oxidative roasting of waste cemented carbide; the roasting temperature is 600-900°C, and the roasting time is 3-8h; S2, crushing the waste cemented carbide after oxidation roasting into waste cemented carbide powder with a particle size less than 0.25 mm; S3, adding hydrochloric acid to the waste cemented carbide powder to obtain a slurry, wherein the concentration of the hydrochloric acid is 25-36wt%, and adding an organic dispersant and stirring and heating; S4, filtering the stirred liquid, first washing it with dilute hydrochloric acid, then washing it with distilled water, and finally washing it with alcohol to obtain a moist yellow solid powder; S5, the yellow solid powder is air-dried and then reduced with hydrogen, using a staged reduction process: the first stage reduction temperature is 300-350°C, and the reduction time is 0.5-1h; the second stage reduction temperature is 500-550°C, and the reduction time is 1-3h; the third stage reduction temperature is 650-700°C, and the reduction time is 1-3h; Nano tungsten powder is obtained, and the average particle size of the nano tungsten powder is ≤55nm.
2. The method for preparing nano tungsten powder using waste cemented carbide according to claim 1, characterized in that: In the step S1, the stains on the surface of the waste cemented carbide are washed away with acetone and then placed in a muffle furnace for oxidation roasting.
3. The method for preparing nano tungsten powder using waste cemented carbide according to claim 1, characterized in that: In the step S2, a jaw crusher is used for crushing.
4. The method for preparing nano tungsten powder using waste cemented carbide according to claim 1, characterized in that: In the step S3, the liquid-to-solid ratio of hydrochloric acid to waste cemented carbide powder is (3-7) mL:1 g.
5. The method for preparing nano tungsten powder using waste cemented carbide according to claim 1, characterized in that: In step S3, the volume ratio of the organic dispersant to the slurry is (1-3):
5.
6. The method for preparing nano tungsten powder using waste cemented carbide according to claim 1, characterized in that: In the step S3, stirring and heating are performed in a heat-collecting constant-temperature magnetic stirrer, the temperature is controlled to be 80-100° C., the magnetic stirring speed is 400-600 r / min, and the stirring time is 2-6 h.
7. The method for preparing nano tungsten powder using waste cemented carbide according to claim 1, characterized in that: In the step S4, suction filtration is performed in a Buchner funnel.
8. The method for preparing nano tungsten powder using waste cemented carbide according to claim 1, characterized in that: In the step S5, hydrogen reduction is carried out in a tubular furnace, the hydrogen flow rate is 3-5 L / min, and the heating rate is 10° C. / min.