An iron oxide desulfurizer capable of effectively avoiding sulfur plugging and a preparation method thereof
By loading iron oxide on composite zeolite and activated carbon with surface-grafted hydrophobic chains, using its microporous and porous structure, combined with the adsorption capacity of phosphate ester groups and amine groups, the sulfur problem of iron oxide desulfurizers when adsorbing sulfides is solved. Blockage problem is solved, desulfurization efficiency and stability are improved, and efficient hydrogen sulfide removal is achieved.
Patent Information
- Application Number
- CN202411095451.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-12
AI Technical Summary
Iron oxide desulfurizers are prone to sulfur blockage during the adsorption of sulfides, resulting in reduced desulfurization efficiency and reduced stability. It is difficult to effectively solve this problem with existing technology.
By loading iron oxide on composite zeolite and activated carbon with hydrophobic chains grafted on the surface, the microporous structure of the zeolite and the porous structure of the activated carbon are combined with the adsorption capacity of the phosphate group and the amine group to improve the anti-sulfur blocking performance of the desulfurizer.
It effectively avoids sulfur blockage, improves the sulfur capacity and desulfurization efficiency of the desulfurizer, enhances the ability and stability to resist sulfur blockage, and is suitable for the removal of hydrogen sulfide in waste gas.
Smart Images

Figure CN118634785B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of desulfurization, and in particular relates to an iron oxide desulfurizer capable of effectively avoiding sulfur plugging and a preparation method thereof. Background Art
[0002] Iron oxide desulfurizer uses iron oxide as the main active component. It is very popular among users because of its low price and the ability to be regenerated by air at room temperature.
[0003] However, iron oxide will generate iron sulfide when adsorbing sulfide. As the reaction proceeds, iron sulfide gradually accumulates on the surface of the desulfurizer, hindering the diffusion of gas, thereby causing a decrease in desulfurization efficiency. The iron oxide desulfurizer has a small specific surface area and limited active sites, and is easily covered by iron sulfide and inactivated. Water vapor will be generated during the reaction, and the water vapor condenses in the pores of the desulfurizer, further aggravating the problem of sulfur plugging. Therefore, it is of great significance to improve the anti-sulfur plugging performance of the iron oxide desulfurizer, thereby improving the desulfurization efficiency and stability of the desulfurizer. Summary of the invention
[0004] In order to solve the above problems, the purpose of the present invention is to provide an iron oxide desulfurizer which can effectively avoid sulfur plugging and a preparation method thereof.
[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0006] An iron oxide desulfurizer capable of effectively avoiding sulfur plugging is obtained by loading iron oxide on the surface of a composite zeolite and activated carbon with a hydrophobic chain grafted on the surface;
[0007] The composite zeolite and activated carbon with surface grafted hydrophobic chains are prepared by hydroxylating the surfaces of zeolite and activated carbon and then grafting phosphate groups.
[0008] The composite zeolite and activated carbon with surface grafted hydrophobic chains are prepared according to the following method:
[0009] 1) The washed and dried zeolite and activated carbon are immersed in a mixed solution of hydrogen peroxide and concentrated sulfuric acid, heated to 50-80°C for reaction for 24-48 hours, and filtered after the reaction. The filter cake is washed with water and ethanol for 2-3 times, respectively, and dried under nitrogen protection to obtain a surface hydroxylated composite zeolite and activated carbon;
[0010] 2) adding the surface hydroxylated composite zeolite and activated carbon obtained in step 1) into toluene, then adding 3-chloropropyltriethoxysilane, heating to 40-50° C., stirring for reaction for 12-24 hours, and filtering after the reaction is completed. The obtained filter cake is washed 2-3 times with anhydrous ethanol, and dried to obtain chlorine-terminated composite zeolite and activated carbon;
[0011] 3) Add diphenylphosphoramidate to an organic solvent, stir to dissolve, then add a base and the chlorine-terminated composite zeolite and activated carbon obtained in step 2), heat to 50-70° C., react for 8-12 hours, filter after the reaction is completed, wash the filter cake with water for 3-5 times, and obtain a composite zeolite and activated carbon with surface grafted hydrophobic chains.
[0012] The mass ratio of the zeolite, activated carbon and the mixed solution of hydrogen peroxide-concentrated sulfuric acid in step 1) is 1:1~3:15~30.
[0013] In step 1), the volume ratio of hydrogen peroxide to concentrated sulfuric acid in the mixed solution of hydrogen peroxide and concentrated sulfuric acid is 1:3-5.
[0014] The mass ratio of the surface hydroxylated composite zeolite to the activated carbon, toluene and 3-chloropropyltriethoxysilane in step 2) is 1:10-15:5-8.
[0015] The water content of toluene in step 2) is less than 50 ppm.
[0016] The organic solvent in step 3) is acetonitrile, chloroform or tetrahydrofuran.
[0017] The base in step 3) is sodium carbonate, sodium bicarbonate, potassium carbonate or potassium bicarbonate.
[0018] In step 3), the mass ratio of the diphenylphosphoramidate, the organic solvent, the base, the chlorine-terminated composite zeolite and the activated carbon is 5-9:25-50:3-5:1.
[0019] The method for preparing the iron oxide desulfurizer capable of effectively avoiding sulfur plugging comprises the following steps:
[0020] The composite zeolite with hydrophobic chains grafted on the surface and activated carbon are added to an aqueous solution of iron salt with a concentration of 0.1-0.5 mol / L, stirred and soaked at 40-60°C for 2-4 hours, and then filtered. The filter cake is washed with water, dried at 100°C for 3-7 hours, and then calcined at 300-400°C for 2-4 hours under nitrogen protection to obtain an iron oxide desulfurizer that can effectively avoid sulfur blockage.
[0021] The iron salt is iron nitrate, iron chloride or iron sulfate; the mass volume ratio of the composite zeolite with hydrophobic chains grafted on the surface and the activated carbon to the iron salt aqueous solution is 1g:2-5ml.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] The iron oxide desulfurizer capable of effectively avoiding sulfur plugging of the present invention is characterized in that iron oxide is loaded on modified composite zeolite and activated carbon. The zeolite has a microporous structure, and the micropores can increase the specific surface area and adsorption capacity of the desulfurizer, thereby increasing the sulfur capacity of the desulfurizer. The activated carbon is a porous carbon material with abundant micropores, mesopores and macropores. The mesoporous structure is conducive to the rapid diffusion of hydrogen sulfide and improves the desulfurization efficiency. The macropores are conducive to the discharge of sulfides, thereby avoiding sulfur plugging. The adsorption performance and anti-sulfur plugging ability of the desulfurizer are improved through the reasonable ratio of the pore structure.
[0024] The iron oxide desulfurizer capable of effectively avoiding sulfur plugging of the present invention has hydrophobic chains grafted on the surface of the desulfurizer. On the one hand, the hydrophobic chains can reduce the condensation of water vapor in the pores of the desulfurizer, reduce the deposition and accumulation of sulfides on the surface, and avoid sulfur plugging; on the other hand, the hydrophobic chains contain phosphate groups and amine groups, which can adsorb and capture hydrogen sulfide and increase the active sites of the desulfurizer; the phosphate groups are relatively stable in acidic and alkaline environments, thereby improving the stability of the desulfurizer and facilitating the long-term use of the desulfurizer.
[0025] The desulfurizer prepared by the invention has high sulfur capacity and desulfurization efficiency, fast desulfurization speed, and certain anti-sulfur plugging ability, and can be used for removing hydrogen sulfide in waste gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a scanning electron microscope image of the iron oxide desulfurizer prepared in Example 3 of the present invention that can effectively avoid sulfur plugging. DETAILED DESCRIPTION
[0027] In order to better understand the technical solution of the present invention, the above content of the present invention is further described in detail below through specific implementation methods in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above content of the present invention belong to the scope of the present invention.
[0028] Example 1 Preparation of composite zeolite and activated carbon with hydrophobic chains grafted on the surface:
[0029] 0.1 kg of zeolite and 0.1 kg of activated carbon that had been washed and dried were immersed in a mixed solution of 1.5 kg of hydrogen peroxide and concentrated sulfuric acid, wherein the volume ratio of hydrogen peroxide to concentrated sulfuric acid was 1:3, and heated to 50°C for 24 hours. After the reaction was completed, the filter cake was filtered and washed twice with water and ethanol, respectively, and dried under nitrogen protection to obtain a surface hydroxylated composite zeolite and activated carbon.
[0030] 0.1 kg of surface hydroxylated composite zeolite and activated carbon were added to 1 kg of toluene, and then 0.5 kg of 3-chloropropyltriethoxysilane was added, and the mixture was heated to 40°C and stirred for reaction for 12 hours. After the reaction was completed, the filter cake was filtered and washed twice with anhydrous ethanol and dried to obtain chlorine-terminated composite zeolite and activated carbon.
[0031] Add 0.5 kg of diphenylphosphoramidate to 2.5 kg of chloroform, stir to dissolve, then add 0.3 kg of sodium carbonate and 0.1 kg of chlorine-terminated composite zeolite and activated carbon, heat to 50°C, react for 8 hours, filter after the reaction is completed, wash the filter cake with water 3 times, and obtain composite zeolite and activated carbon with surface grafted hydrophobic chains.
[0032] Preparation of iron oxide desulfurizer that can effectively avoid sulfur plugging:
[0033] 0.1 kg of composite zeolite with surface grafted hydrophobic chains and activated carbon were added to 500 mL of 0.1 mol / L ferric nitrate aqueous solution, stirred and soaked at 40°C for 4 hours and then filtered. The filter cake was washed with water, dried at 100°C for 3 hours, and then calcined at 300°C for 2 hours under nitrogen protection to obtain an iron oxide desulfurizer that can effectively avoid sulfur blockage.
[0034] Example 2 Preparation of composite zeolite and activated carbon with surface grafted hydrophobic chains:
[0035] 0.1 kg of zeolite and 0.15 kg of activated carbon that had been washed and dried were immersed in a mixed solution of 1.8 kg of hydrogen peroxide and concentrated sulfuric acid, wherein the volume ratio of hydrogen peroxide to concentrated sulfuric acid was 1:4, and heated to 55°C for 45 hours. After the reaction was completed, the filter cake was filtered and washed with water and ethanol for 3 times, respectively, and dried under nitrogen protection to obtain a surface hydroxylated composite zeolite and activated carbon.
[0036] 0.1 kg of surface hydroxylated composite zeolite and activated carbon were added to 1.1 kg of toluene, and then 0.6 kg of 3-chloropropyltriethoxysilane was added, and the mixture was heated to 42°C and stirred for reaction for 20 hours. After the reaction was completed, the filter cake was filtered and washed with anhydrous ethanol for 3 times, and dried to obtain chlorine-terminated composite zeolite and activated carbon.
[0037] Add 0.6 kg of diphenylphosphoramidate to 3 kg of tetrahydrofuran, stir to dissolve, then add 0.35 kg of sodium bicarbonate and 0.1 kg of chlorine-terminated composite zeolite and activated carbon, heat to 55°C, react for 9 hours, filter after the reaction is completed, wash the filter cake with water 4 times, and obtain composite zeolite and activated carbon with surface grafted hydrophobic chains.
[0038] Preparation of iron oxide desulfurizer that can effectively avoid sulfur plugging:
[0039] 0.1 kg of composite zeolite with surface grafted hydrophobic chains and activated carbon were added to 400 mL of 0.2 mol / L ferric chloride aqueous solution, stirred and soaked at 45°C for 3.5 hours and then filtered. The filter cake was washed with water, dried at 100°C for 6 hours, and then calcined at 340°C for 2.5 hours under nitrogen protection to obtain an iron oxide desulfurizer that can effectively avoid sulfur blockage.
[0040] Example 3 Preparation of composite zeolite and activated carbon with hydrophobic chains grafted on the surface:
[0041] 0.1 kg of zeolite and 0.2 kg of activated carbon that had been washed and dried were immersed in a mixed solution of 2 kg of hydrogen peroxide and concentrated sulfuric acid, wherein the volume ratio of hydrogen peroxide to concentrated sulfuric acid was 1:4, and heated to 60°C for 40 hours. After the reaction was completed, the filter cake was filtered and washed with water and ethanol for 3 times, respectively, and dried under nitrogen protection to obtain a composite zeolite and activated carbon with surface hydroxylation.
[0042] 0.1 kg of surface hydroxylated composite zeolite and activated carbon were added to 1.2 kg of toluene, and then 0.65 kg of 3-chloropropyltriethoxysilane was added, and the mixture was heated to 45°C and stirred for reaction for 18 hours. After the reaction was completed, the filter cake was filtered and washed with anhydrous ethanol for 3 times, and dried to obtain chlorine-terminated composite zeolite and activated carbon;
[0043] Add 0.7 kg of diphenylphosphoramidate to 3.5 kg of acetonitrile, stir to dissolve, then add 0.4 kg of potassium bicarbonate and 0.1 kg of chlorine-terminated composite zeolite and activated carbon, heat to 60°C, react for 10 hours, filter after the reaction is completed, wash the filter cake with water 5 times, and obtain composite zeolite and activated carbon with surface grafted hydrophobic chains.
[0044] Preparation of iron oxide desulfurizer that can effectively avoid sulfur plugging:
[0045] 0.1kg of composite zeolite with hydrophobic chains grafted on the surface and activated carbon were added to 350mL of 0.3mol / L ferric chloride aqueous solution, stirred and soaked at 50℃ for 3h, and then filtered. The filter cake was washed with water, dried at 100℃ for 5h, and then calcined at 360℃ for 3h under nitrogen protection to obtain an iron oxide desulfurizer that can effectively avoid sulfur blockage. The scanning electron microscope image is as follows: Figure 1 shown.
[0046] Example 4 Preparation of composite zeolite and activated carbon with hydrophobic chains grafted on the surface:
[0047] 0.1 kg of zeolite and 0.25 kg of activated carbon that had been washed and dried were immersed in a mixed solution of 2.5 kg of hydrogen peroxide-concentrated sulfuric acid, wherein the volume ratio of hydrogen peroxide to concentrated sulfuric acid was 1:4.5, and heated to 70°C for 30 hours. After the reaction was completed, the filter cake was filtered and washed with water and ethanol for 3 times, respectively, and dried under nitrogen protection to obtain a surface hydroxylated composite zeolite and activated carbon.
[0048] 0.1 kg of surface hydroxylated composite zeolite and activated carbon were added to 1.4 kg of toluene, and then 0.75 kg of 3-chloropropyltriethoxysilane was added, and the mixture was heated to 48°C and stirred for 15 hours. After the reaction was completed, the filter cake was filtered and washed with anhydrous ethanol for 3 times, and dried to obtain chlorine-terminated composite zeolite and activated carbon.
[0049] Add 0.8 kg of diphenylphosphoramidate to 4.5 kg of acetonitrile, stir to dissolve, then add 0.45 kg of potassium carbonate and 0.1 kg of chlorine-terminated composite zeolite and activated carbon, heat to 65 ° C, react for 11 hours, filter after the reaction is completed, wash the filter cake with water 5 times, and obtain composite zeolite and activated carbon with surface grafted hydrophobic chains.
[0050] Preparation of iron oxide desulfurizer that can effectively avoid sulfur plugging:
[0051] 0.1 kg of composite zeolite with surface grafted hydrophobic chains and activated carbon were added to 250 mL of 0.4 mol / L ferric sulfate aqueous solution, stirred and soaked at 55°C for 3.5 hours, and then filtered. The filter cake was washed with water, dried at 100°C for 6 hours, and then calcined at 380°C for 3.5 hours under nitrogen protection to obtain an iron oxide desulfurizer that can effectively avoid sulfur blockage.
[0052] Example 5 Preparation of composite zeolite and activated carbon with surface grafted hydrophobic chains:
[0053] 0.1 kg of zeolite and 0.3 kg of activated carbon that had been washed and dried were immersed in a mixed solution of 3 kg of hydrogen peroxide and concentrated sulfuric acid, wherein the volume ratio of hydrogen peroxide to concentrated sulfuric acid was 1:5, and heated to 80°C for 24 hours. After the reaction was completed, the filter cake was filtered and washed twice with water and ethanol, respectively, and dried under nitrogen protection to obtain a surface hydroxylated composite zeolite and activated carbon.
[0054] 0.1 kg of surface hydroxylated composite zeolite and activated carbon were added to 1.5 kg of toluene, and then 0.8 kg of 3-chloropropyltriethoxysilane was added, and the mixture was heated to 50°C and stirred for reaction for 12 hours. After the reaction was completed, the filter cake was filtered and washed with anhydrous ethanol for 3 times, and dried to obtain chlorine-terminated composite zeolite and activated carbon.
[0055] Add 0.9 kg of diphenylphosphoramidate to 5 kg of acetonitrile, stir to dissolve, then add 0.5 kg of potassium bicarbonate and 0.1 kg of chlorine-terminated composite zeolite and activated carbon, heat to 70°C, react for 12 hours, filter after the reaction is completed, wash the filter cake with water 4 times, and obtain composite zeolite and activated carbon with hydrophobic chains grafted on the surface.
[0056] Preparation of iron oxide desulfurizer that can effectively avoid sulfur plugging:
[0057] 0.1 kg of composite zeolite with surface grafted hydrophobic chains and activated carbon were added to 200 mL of 0.5 mol / L aqueous ferric sulfate solution, stirred and soaked at 60°C for 4 hours and then filtered. The filter cake was washed with water, dried at 100°C for 7 hours, and then calcined at 400°C for 4 hours under nitrogen protection to obtain an iron oxide desulfurizer that can effectively avoid sulfur blockage.
[0058] Example 6 Preparation of composite zeolite and activated carbon with surface grafted hydrophobic chains:
[0059] 0.1 kg of zeolite and 0.2 kg of activated carbon that had been washed and dried were immersed in a mixed solution of 1.5 kg of hydrogen peroxide and concentrated sulfuric acid, wherein the volume ratio of hydrogen peroxide to concentrated sulfuric acid was 1:4, and heated to 80°C for 48 hours. After the reaction was completed, the filter cake was filtered and washed with water and ethanol for 3 times, respectively, and dried under nitrogen protection to obtain a surface hydroxylated composite zeolite and activated carbon.
[0060] 0.1 kg of surface hydroxylated composite zeolite and activated carbon were added to 1.5 kg of toluene, and then 0.5 kg of 3-chloropropyltriethoxysilane was added, and the mixture was heated to 40°C and stirred for reaction for 12 hours. After the reaction was completed, the filter cake was filtered and washed with anhydrous ethanol for 3 times, and dried to obtain chlorine-terminated composite zeolite and activated carbon;
[0061] Add 0.9 kg of diphenylphosphoramidate to 2.5 kg of tetrahydrofuran, stir to dissolve, then add 0.5 kg of sodium carbonate and 0.1 kg of chlorine-terminated composite zeolite and activated carbon, heat to 60°C, react for 10 hours, filter after the reaction is completed, wash the filter cake with water 3 times, and obtain composite zeolite and activated carbon with surface grafted hydrophobic chains.
[0062] Preparation of iron oxide desulfurizer that can effectively avoid sulfur plugging:
[0063] 0.1 kg of composite zeolite with surface grafted hydrophobic chains and activated carbon were added to 200 mL of 0.1 mol / L ferric chloride aqueous solution, stirred and soaked at 60°C for 2 hours and then filtered. The filter cake was washed with water, dried at 100°C for 5 hours, and then calcined at 400°C for 2 hours under nitrogen protection to obtain an iron oxide desulfurizer that can effectively avoid sulfur blockage.
[0064] Comparative Example: 0.1 kg of zeolite and 0.2 kg of activated carbon were added to 250 mL of 0.2 mol / L ferric chloride aqueous solution, stirred and soaked at 50°C for 3 h, and then filtered. The filter cake was washed with water, dried at 100°C for 5 h, and then calcined at 350°C for 2 h under nitrogen protection to obtain an iron oxide desulfurizer.
[0065] The specific surface area and pore volume of the iron oxide desulfurizers prepared in Examples 1 to 6 of the present invention and the iron oxide desulfurizer prepared in the comparative example were analyzed using an automatic adsorption instrument. The test results are shown in Table 1.
[0066] Table 1 Performance parameters of the iron oxide desulfurizers prepared in Examples 1 to 6 and Comparative Examples
[0067]
[0068] It can be seen from the results in Table 1 that the iron oxide desulfurizer prepared by the present invention which can effectively avoid sulfur plugging has hydrophobic chains grafted on the surfaces of the composite activated carbon and zeolite, resulting in a decrease in specific surface area and pore volume compared with the comparative example.
[0069] The iron oxide desulfurizers prepared in Examples 1 to 6 of the present invention and capable of effectively avoiding sulfur plugging and the iron oxide desulfurizers prepared in the comparative example were subjected to sulfur capacity determination according to the method provided in HG / T 5759-2020. The test results are shown in Table 2.
[0070] Table 2 Sulfur capacity of the iron oxide desulfurizer prepared in Examples 1 to 6 and Comparative Examples
[0071]
[0072] It can be seen from the results in Table 2 that the iron oxide desulfurizer prepared by the present invention that can effectively avoid sulfur blockage has a greater sulfur capacity than the comparative example because the hydrophobic chains grafted on the surface contain phosphate groups and amine groups, which increase the adsorption and capture of hydrogen sulfide.
[0073] The iron oxide desulfurizer prepared in Examples 1 to 6 and the iron oxide desulfurizer prepared in the comparative example, which can effectively avoid sulfur plugging, was loaded in a fixed bed microreactor for desulfurization performance test. The size of the reactor was Φ10mm*12mm*300mm, the loading amount of the desulfurizer was 0.5g, and the upper and lower ends of the fixed bed microreactor were respectively filled with quartz sand. A hydrogen sulfide and nitrogen mixer was used as a simulated raw gas, wherein the content of hydrogen sulfide was 20mg / L, and the hydrogen sulfide that was not removed was absorbed by the tail gas absorption liquid, and the hydrogen sulfide in the absorption liquid was detected every 5 minutes by the iodine method. When the gas concentration after purification was 10% of the hydrogen sulfide concentration in the simulated raw gas, it was considered that the desulfurizer was completely penetrated, the experiment was stopped, and its penetration time was recorded. The desulfurization rate was calculated based on the sulfur content in the absorption liquid after the adsorption was completed, and the calculation formula was:
[0074]
[0075] Where, η is the desulfurization rate of the desulfurizer (%), V is the total gas volume (L), W H2S is the hydrogen sulfide content in the raw gas (mg / L), C1 is the concentration of the I2 standard solution (mol / L), V1 is the volume of the added I2 standard solution (mL), C2 is the concentration of the Na2S2O3 standard solution (mol / L), V2 is the volume of the Na2S2O3 standard solution consumed during titration (mL), and 34 is the molar mass of hydrogen sulfide (g / mol). The desulfurization rate and breakthrough time test results are shown in Table 3.
[0076] Table 3 Desulfurization efficiency of iron oxide desulfurizers prepared in Examples 1 to 6 and Comparative Examples
[0077]
[0078] It can be seen from the results in Table 3 that the iron oxide desulfurizer prepared by the present invention, which can effectively avoid sulfur plugging, reduces the deposition and accumulation of sulfides on the surface due to the hydrophobic chains grafted on the surface, avoids sulfur plugging, and improves the desulfurization efficiency. At the same time, due to the reasonable ratio of the activated carbon and the zeolite pore structure, the adsorption performance and anti-sulfur plugging ability of the desulfurizer are improved, and the desulfurization efficiency of the desulfurizer is further increased.
[0079] Although the above describes the specific implementation methods of the present invention, it does not limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.
Claims
1. An iron oxide desulfurizer that can effectively avoid sulfur plugging, characterized in that: The method is obtained by loading iron oxide on the surface of composite zeolite and activated carbon with hydrophobic chains grafted on the surface; The composite zeolite and activated carbon with surface grafted hydrophobic chains are prepared according to the following method: 1) The washed and dried zeolite and activated carbon are immersed in a mixed solution of hydrogen peroxide and concentrated sulfuric acid, heated to 50-80°C for reaction for 24-48 hours, and filtered after the reaction. The filter cake is washed with water and ethanol for 2-3 times, respectively, and dried under nitrogen protection to obtain a surface hydroxylated composite zeolite and activated carbon; 2) adding the surface hydroxylated composite zeolite and activated carbon obtained in step 1) into toluene, then adding 3-chloropropyltriethoxysilane, heating to 40-50° C., stirring for reaction for 12-24 hours, and filtering after the reaction is completed. The obtained filter cake is washed 2-3 times with anhydrous ethanol, and dried to obtain chlorine-terminated composite zeolite and activated carbon; 3) Add diphenylphosphoramidate to an organic solvent, stir and dissolve, then add sodium carbonate, sodium bicarbonate, potassium carbonate or potassium bicarbonate and the chlorine-terminated composite zeolite and activated carbon obtained in step 2), heat to 50-70° C., react for 8-12 hours, filter after the reaction is completed, wash the filter cake with water for 3-5 times, and obtain a composite zeolite and activated carbon with surface grafted hydrophobic chains.
2. The iron oxide desulfurizer capable of effectively avoiding sulfur plugging according to claim 1, characterized in that: The mass ratio of the zeolite, activated carbon and the mixed solution of hydrogen peroxide-concentrated sulfuric acid in step 1) is 1:1~3:15~30.
3. The iron oxide desulfurizer capable of effectively avoiding sulfur plugging according to claim 1, characterized in that: In step 1), the volume ratio of hydrogen peroxide to concentrated sulfuric acid in the mixed solution of hydrogen peroxide and concentrated sulfuric acid is 1:3-5.
4. The iron oxide desulfurizer capable of effectively avoiding sulfur plugging according to claim 1, characterized in that: In step 2), the mass ratio of the surface hydroxylated composite zeolite to activated carbon, toluene and 3-chloropropyltriethoxysilane is 1:10-15:5-8; the water content of the toluene is less than 50 ppm.
5. The iron oxide desulfurizer capable of effectively avoiding sulfur plugging according to claim 1, characterized in that: The organic solvent in step 3) is acetonitrile, chloroform or tetrahydrofuran.
6. The iron oxide desulfurizer capable of effectively avoiding sulfur plugging according to claim 1, characterized in that: In step 3), the mass ratio of the diphenylphosphoramidate, the organic solvent, the sodium carbonate, the sodium bicarbonate, the potassium carbonate or the potassium bicarbonate and the chlorine-terminated composite zeolite and the activated carbon is 5-9:25-50:3-5:
1.
7. The method for preparing an iron oxide desulfurizer capable of effectively avoiding sulfur plugging according to claim 1, characterized in that: The following steps are involved: The composite zeolite with hydrophobic chains grafted on the surface and activated carbon are added to an aqueous solution of iron salt with a concentration of 0.1-0.5 mol / L, stirred and soaked at 40-60°C for 2-4 hours, and then filtered. The filter cake is washed with water, dried at 100°C for 3-7 hours, and then calcined at 300-400°C for 2-4 hours under nitrogen protection to obtain an iron oxide desulfurizer that can effectively avoid sulfur blockage.
8. The method for preparing an iron oxide desulfurizer capable of effectively avoiding sulfur plugging according to claim 7, characterized in that: The iron salt is iron sulfate, iron nitrate or iron chloride; the mass volume ratio of the composite zeolite with hydrophobic chains grafted on the surface and the activated carbon to the iron salt aqueous solution is 1g:2-5ml.
Citation Information
Patent Citations
Ferric oxide desulfurizer based on modified activated carbon loading and preparation method of ferric oxide desulfurizer
CN116173908A
Adsorbent for desulfurization of gasoline and method for desulfurization of gasoline
US20160222302A1