Preparation method of porous carbon material and preparation method of durable membrane electrode

By using the B and N doped porous carbon material NBSPC synthesized by sodium alginate and ammonium borate in fuel cells as the buffer zone between the diffusion layer and the catalytic layer, the problems of carbon support corrosion and Pt agglomeration are solved, and the life of the membrane electrode is improved and performance.

CN118637599BActive Publication Date: 2024-11-08JIANGSU YUANHYDROGEN NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095469.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-08
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Under the start-stop idle operation conditions of fuel cells, the carbon carrier corrosion severely leads to Pt agglomeration, affecting the life of the membrane electrode. The preparation of porous carbon materials is limited by the complex template removal process and the high cost of soft templates.

Method used

Sodium alginate is used as the carbon precursor, ammonium borate introduces B atoms and nitrogen as N atoms, and the porous carbon material NBSPC that is doped with B and N doped is synthesized by hydrothermal and high-temperature calcination, which serves as a buffer zone for the diffusion layer and the catalytic layer to reduce Carbon support corrosion and Pt aggregation.

Benefits of technology

It effectively improves the life of the membrane electrode, improves the conductivity and wettability, avoids the collapse of the carbon layer and Pt agglomeration, reduces the corrosion of the carbon carrier, and extends the service life of the membrane electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118637599B_ABST
    Figure CN118637599B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a porous carbon material and a method for preparing a durable membrane electrode, wherein a mixed solution prepared by dissolving sodium alginate SA and ammonium borate in water is hydrothermally and freeze-dried to obtain a SA precursor, the SA precursor is calcined and pyrolyzed at high temperature, and then reacted in an N2 atmosphere, and then washed with hydrochloric acid and deionized water, and ground into NBSPC after drying; NBSPC is dissolved in an organic solvent, and a slurry is obtained after ultrasonic dispersion, and the slurry is sprayed on a cathode diffusion layer and an anode diffusion layer, and a catalyst slurry is sprayed on the cathode diffusion layer and the anode diffusion layer to form a catalytic layer, and the cathode diffusion layer, a proton exchange membrane, and an anode diffusion layer are hot-pressed to obtain a membrane electrode. The present invention uses sodium alginate as a carbon precursor, uses ammonium borate to introduce B atoms, and nitrogen is introduced as a N atom to synthesize NBSPC as a buffer zone between a diffusion layer and a catalytic layer, effectively reducing the corrosion of a carbon carrier, avoiding Pt agglomeration, and effectively improving the life of a membrane electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fuel cells, and in particular to a method for preparing a porous carbon material and a method for preparing a durable membrane electrode. Background Art

[0002] The development of fuel cells is an important way to pursue carbon neutrality. It has the characteristics of high energy conversion, low pollution, fast startup speed and low temperature. It is widely favored by the industry. Due to the influence of start-stop idling conditions, the corrosion of the carbon carrier of the fuel cell is particularly serious, which in turn causes the agglomeration of Pt and affects the life of the membrane electrode.

[0003] In order to reduce the occurrence of this phenomenon, porous carbon materials are added to the diffusion layer. Porous carbon materials have the characteristics of strong structural design, low cost and environmental protection. However, the complex hard template removal process and the high price of soft templates limit the large-scale preparation of porous carbon. Therefore, it is necessary to explore a method to synthesize porous carbon materials without adding templates. Summary of the invention

[0004] The main technical problem solved by the present invention is to provide a method for preparing a porous carbon material and a method for preparing a durable membrane electrode. Sodium alginate is used as a carbon precursor, ammonium borate is used to introduce B atoms, nitrogen is introduced as N atoms, NBSPC is synthesized and used as a buffer zone between a diffusion layer and a catalytic layer, which effectively reduces the corrosion of the carbon carrier, avoids the agglomeration of Pt, and effectively improves the life of the membrane electrode.

[0005] In order to solve the above technical problems, a technical solution adopted by the present invention is: to provide a method for preparing a porous carbon material, comprising the following steps: S1. dissolving sodium alginate SA and ammonium borate in water, and stirring evenly to prepare a mixed solution; S2. subjecting the mixed solution prepared in S1 to hydrothermal and freeze-drying to obtain an SA precursor, which is a sodium alginate-derived precursor; S3. The SA precursor is subjected to high-temperature calcination and pyrolysis, and then reacted in a N2 atmosphere, and then washed with hydrochloric acid and deionized water, and then ground into NBSPC after drying, which is a porous carbon derived from SA doped with B and N.

[0006] In a preferred embodiment of the present invention, the mass ratio of sodium alginate SA to ammonium borate in step S1 is 1:5-5:2.

[0007] In a preferred embodiment of the present invention, in step S1, sodium alginate SA and ammonium borate are dissolved in water and stirred by a stirrer at a speed of 200-500 rpm for 24-36 hours at a stirring temperature of 25°C.

[0008] In a preferred embodiment of the present invention, the mixed solution in step S2 is placed in a high temperature reactor under reaction conditions of 160-180°C, and after sufficient hydrothermal treatment for 12-16 hours, the reactor is placed in a freezing environment of -30--50°C and freeze-dried for 48 hours.

[0009] In a preferred embodiment of the present invention, in step S3, the SA precursor is pyrolyzed in a tube furnace at a calcination temperature of 600-800°C and a heating rate of 5°C / min, and then reacted for 2 hours in a N2 atmosphere. After cooling to room temperature, it is washed with 1 mol / L hydrochloric acid and deionized water, dried at 80°C for 6-8 hours, and ground to obtain NBSPC.

[0010] In order to solve the above technical problems, another technical solution adopted by the present invention is: to provide a method for preparing a durable membrane electrode, comprising the following steps: S4. Take the above-mentioned NBSPC, dissolve it in an organic solvent, and obtain a slurry after ultrasonic dispersion, and spray the slurry on the cathode diffusion layer and the anode diffusion layer, and the NBSPC loading of the anode diffusion layer is greater than the NBSPC loading of the cathode diffusion layer; S5. Take the catalyst slurry and spray it on the cathode diffusion layer and the anode diffusion layer obtained in step S4 to form a catalytic layer, and NBSPC forms a porous buffer zone between the diffusion layer and the catalytic layer; S6. The cathode diffusion layer, the proton exchange membrane, and the anode diffusion layer are hot pressed to obtain the final membrane electrode.

[0011] In a preferred embodiment of the present invention, the NBSPC loading of the cathode diffusion layer in step S4 is 0.2 mg / cm 2 The NBSPC loading of the anode diffusion layer is 0.05 mg / cm 2 .

[0012] In a preferred embodiment of the present invention, the catalyst loading of the cathode diffusion layer in step S5 is 0.3 mg / cm 2 The catalyst loading of the anode diffusion layer is 0.1 mg / cm 2 .

[0013] In a preferred embodiment of the present invention, the hot pressing temperature in step S6 is 120-150° C., the hot pressing time is 3-5 min, and the hot pressing pressure is 120-150 kPa.

[0014] The beneficial effects of the present invention are as follows: the preparation method of the porous carbon material and the preparation method of the durable membrane electrode of the present invention, sodium alginate has a high specific surface area and an extremely high average molecular weight (AR 12000-14000), and is suitable for use as a carbon carrier. Sodium alginate and ammonium borate are co-decomposed to produce a large number of porous structures. At the same time, ammonium borate will decompose at high temperatures, so that B atoms can adhere to the surface of sodium alginate, and N atoms are introduced at the same time. The synergistic effect of B atoms and N atoms is used to prepare new NBSPC. This B and N co-doped element improves the conductivity and wettability of the membrane electrode, avoids the collapse of the carbon layer during the aging process, causes Pt agglomeration, and then causes the membrane electrode to deactivate. Synthesized NBSPC is used as a buffer zone between the diffusion layer and the catalytic layer, effectively reduces the corrosion of the carbon carrier, avoids the agglomeration of Pt, and effectively improves the life of the membrane electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:

[0016] Figure 1 is a SEM image of the durable membrane electrode of Example 1 of the present invention;

[0017] Figure 2 is the particle size statistics of Pt nanoparticles;

[0018] Figure 3 Polarization performance comparison table. DETAILED DESCRIPTION

[0019] The technical scheme in the embodiment of the present invention will be described clearly and completely below. The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification, so that people familiar with this technology can understand and read them, and are not used to limit the limiting conditions that the present invention can implement, so they have no substantial technical significance. Any modification of the structure, change of the proportional relationship, or adjustment of the size should still fall within the scope that the technical content disclosed by the present invention can cover without affecting the effects that the present invention can produce and the purposes that can be achieved. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and so on quoted in this specification are only for the convenience of narration, and are not used to limit the scope that can be implemented. The change or adjustment of the relative relationship should also be regarded as the scope that the present invention can implement without substantially changing the technical content.

[0020] Example 1: Weigh 2g sodium alginate and 5g ammonium borate, add them to 200ml water, stir at 200rpm, 25℃, and stir for 24h. Transfer the mixed solution to a high temperature reactor, fully hydrothermally heat at 160℃ for 12h, and after the reaction is complete, place in a -30℃ freezing environment and freeze-dry for 48h to obtain a SA precursor.

[0021] The obtained SA precursor was placed in a tube furnace and calcined at 800°C from room temperature to 800°C at a heating rate of 5°C / min. After heating to 800°C, it was reacted for 2 hours in a N2 atmosphere. After cooling to room temperature, the reactant was taken out and rinsed repeatedly with 1 mol / L hydrochloric acid and deionized water for 3-5 times to remove impurities. It was dried at 80°C for 6 hours. After sufficient grinding, the final NBSPC mass was weighed to be 1.2 g.

[0022] Weigh 0.5g NBSPC and 20ml isopropanol, disperse them by ultrasonic dispersion for 20min, put the dispersed slurry in a sprayer, cut two 5*5 sheets of Toray diffusion layer Toray-055, spray them on one side of the anode and cathode diffusion layer, so that the NBSPC loading of the cathode diffusion layer is 0.2mg / cm 2 The NBSPC loading of the anode diffusion layer is 0.05 mg / cm 2 .

[0023] Weigh 0.15 g of 50% Pt / C catalyst, 10 ml of deionized water, 10 ml of isopropanol, and 0.2 ml of Nafion 520 dispersion, disperse by ultrasonic dispersion for 20 min, and spray the dispersed catalyst slurry on the cathode diffusion layer and anode diffusion layer prepared above until the cathode catalyst loading is 0.3 mg / cm 2 , the anode catalyst loading is 0.1 mg / cm 2 .

[0024] The cathode diffusion layer, gore 12um proton exchange membrane and anode diffusion layer were hot-pressed at 120°C and 120kPa for 5 minutes to obtain the final membrane electrode, and the single cell was assembled for durability testing.

[0025] Durability test: Scan from open circuit potential to 0.55V, run for 3min at each current, anode stoichiometry 1.2, cathode stoichiometry 2.5. Anode humidity 40% RH, cathode humidity 40% RH, hydrogen back pressure 200 kPa, air back pressure 200 kPa, anode 75℃, cathode 75℃, single cell temperature 75℃.

[0026] After nitrogen was cycled for 0, 2000, and 5000 times at a potential of 1-1.5 V, polarization testing was performed to obtain the final data.

[0027] SEM test: The initial membrane electrode was cross-sectioned for SEM test, and the membrane electrode after 5000 cycles was cross-sectioned for test, and the particle size obtained by SEM was analyzed.

[0028] Example 2: Weigh 5g sodium alginate and 8g ammonium borate, add them to 200ml water, stir at 400rpm, 20°C for 24h. Transfer the mixture to a high temperature reactor, fully hydrothermally heat at 180°C for 12h, and after the reaction is complete, place in a -50°C freezing environment and freeze-dry for 48h to obtain a SA precursor.

[0029] The obtained SA precursor was placed in a tube furnace and calcined at 600°C from room temperature to 600°C at a heating rate of 5°C / min. After heating to 600°C, it was reacted for 2 hours in a N2 atmosphere. After cooling to room temperature, the reactant was taken out and rinsed repeatedly with 1 mol / L hydrochloric acid and deionized water for 3-5 times to remove impurities. It was dried at 80°C for 8 hours. After sufficient grinding, the final NBSPC mass was weighed to be 3.6 g.

[0030] Weigh 0.5g NBSPC and 20ml n-butanol, disperse them by ultrasonic dispersion for 20min, put the dispersed slurry in a sprayer, cut two 5*5 sheets of SGL 22BB diffusion layer, spray them on one side of the anode and cathode diffusion layer, so that the NBSPC loading of the cathode diffusion layer is 0.2mg / cm 2 The NBSPC loading of the anode diffusion layer is 0.05 mg / cm 2 .

[0031] Weigh 0.15 g of 50% Pt / C catalyst, 10 ml of deionized water, 10 ml of isopropanol, and 0.5 ml of Nafion 520 dispersion, disperse by ultrasonic dispersion for 20 min, and spray the dispersed catalyst slurry on the prepared cathode diffusion layer and anode diffusion layer until the cathode catalyst loading is 0.3 mg / cm 2 , the anode catalyst loading is 0.1 mg / cm 2 .

[0032] The cathode catalyst layer, gore 8um proton exchange membrane and anode catalyst layer were hot-pressed at 120°C and 120kPa for 5 minutes to obtain the final membrane electrode, which was then assembled into a single cell for durability testing.

[0033] Durability test: Scan from open circuit potential to 0.55V, run for 3min at each current, anode stoichiometry 1.2, cathode stoichiometry 2.5. Anode humidity 40% RH, cathode humidity 40% RH, hydrogen back pressure 200 kPa, air back pressure 200 kPa, anode 75℃, cathode 75℃, single cell temperature 75℃.

[0034] After nitrogen was cycled for 0, 2000, and 5000 times at a potential of 1-1.5 V, polarization testing was performed to obtain the final data.

[0035] SEM test: The initial membrane electrode was cross-sectioned for SEM test, and the membrane electrode after 5000 cycles was cross-sectioned for test, and the particle size obtained by SEM was analyzed.

[0036] Example 3: Weigh 3g sodium alginate and 2g ammonium borate, add them to 200ml water, stir at 500rpm, 25℃, and stir for 24h. Transfer the mixed solution to a high temperature reactor, fully hydrothermally heat at 170℃ for 12h, and after the reaction is complete, place in a -40℃ freezing environment and freeze-dry for 48h to obtain SA precursor.

[0037] The obtained SA precursor was placed in a tube furnace and calcined at 700°C from room temperature to 700°C at a heating rate of 5°C / min. After heating to 800°C, it was reacted for 2 hours in a N2 atmosphere. After cooling to room temperature, the reactant was taken out and rinsed repeatedly with 1 mol / L hydrochloric acid and deionized water for 3-5 times to remove impurities. It was dried at 80°C for 7 hours. After sufficient grinding, the final NBSPC mass was weighed to be 1.2 g.

[0038] Weigh 0.5g NBSPC and 20ml isopropanol, disperse them by ultrasonic dispersion for 20min, put the dispersed slurry in a sprayer, cut two 5*5 sheets of Toray diffusion layer Toray-055, spray them on one side of the anode and cathode diffusion layer, so that the NBSPC loading of the cathode diffusion layer is 0.2mg / cm 2 The NBSPC loading of the anode diffusion layer is 0.05 mg / cm 2 .

[0039] Weigh 0.15 g of 50% Pt / C catalyst, 10 ml of deionized water, 10 ml of isopropanol, and 1 ml of Nafion 520 dispersion, disperse by ultrasonic dispersion for 20 min, and spray the dispersed catalyst slurry on the cathode diffusion layer and anode diffusion layer prepared above until the cathode catalyst loading is 0.3 mg / cm 2 , the anode catalyst loading is 0.1 mg / cm 2 .

[0040] The cathode diffusion layer, gore 12um proton exchange membrane and anode diffusion layer were hot-pressed at 120°C and 120kPa for 5 minutes to obtain the final membrane electrode, and the single cell was assembled for durability testing.

[0041] Durability test: Scan from open circuit potential to 0.55V, run for 3min at each current, anode stoichiometry 1.2, cathode stoichiometry 2.5. Anode humidity 40% RH, cathode humidity 40% RH, hydrogen back pressure 200 kPa, air back pressure 200 kPa, anode 75℃, cathode 75℃, single cell temperature 75℃.

[0042] After nitrogen was cycled for 0, 2000, and 5000 times at a potential of 1-1.5 V, polarization testing was performed to obtain the final data.

[0043] SEM test: The initial membrane electrode was cross-sectioned for SEM test, and the membrane electrode after 5000 cycles was cross-sectioned for test, and the particle size obtained by SEM was analyzed.

[0044] In the above three embodiments, the organic solvent may also be one or a mixture of n-propanol, isopropanol, ethylene glycol, and n-butanol. The proton exchange membrane may be other proton exchange membranes available in the art, and the same is true for carbon paper.

[0045] Comparative example: weigh 0.15g of 50% Pt / C catalyst, 10ml of deionized water, 10ml of isopropanol, and 0.2ml of Nafion520 dispersion, disperse them by ultrasonic dispersion for 20min, and spray the dispersed cathode and cathode catalyst slurry on two 5*5 cathode and cathode diffusion layers of Toray-055 until the cathode catalyst loading is 0.3mg / cm 2 , the anode catalyst loading is 0.1 mg / cm 2 .

[0046] The cathode catalyst layer, gore 12um proton exchange membrane and anode catalyst layer were hot-pressed at 120°C and 120kpa for 5 minutes to obtain the final membrane electrode, and the single cell was assembled for durability testing.

[0047] Using sodium alginate (SA) as a carbon precursor, ammonium borate to introduce B atoms, nitrogen (N2) as N atoms, and sodium alginate (SA) and ammonium borate co-decompose to produce a large number of porous structures, synthesizing NBSPC as a buffer between the diffusion layer and the catalytic layer. This B and N co-doped element improves the conductivity and wettability of the membrane electrode, avoids the collapse of the carbon layer due to aging, causes Pt agglomeration, and then causes the membrane electrode to deactivate, effectively improving the life of the membrane electrode. The use of SA and ammonium borate mixed method avoids the problem of difficult hard template removal.

[0048] Sodium alginate has a high specific surface area and an extremely high average molecular weight (AR 12000-14000), which makes it suitable as a carbon carrier. At the same time, ammonium borate will decompose at high temperatures, allowing B atoms to adhere to the surface of sodium alginate and introducing N atoms. The synergistic effect of B atoms and N atoms can play a wetting role. The newly prepared NBSPC is used as a buffer zone between the catalytic layer and the diffusion layer, which can effectively reduce carbon corrosion in the diffusion layer, reduce Pt agglomeration, and increase the life of the membrane electrode.

[0049] from Figure 1 It can be clearly seen that the upper layer is the catalytic layer, and the linear in and out in the middle is the buffer layer of NBSPC, proving that there is indeed a buffer layer between the diffusion layer and the catalytic layer. Figure 2 The particle size analysis of the existing Pt shows that the particle size growth range is not large, which proves that the synergistic effect of BN effectively slows down the corrosion of the carbon carrier and avoids the agglomeration of Pt. The particle size of the comparative example increases to 7.2nm. Figure 3 It is a statement of performance. Under the potential of 1-1.5V carbon carrier aging, 0.65V is used as the reference potential. The current density attenuation ratios of Examples 1-3 after 5000 cycles are 25%-33% respectively, and the current density attenuation ratio of the comparative example is 71.19%. It is also proved from the performance aspect that the buffer layer of NBSPC in the examples plays a role, reduces the corrosion of the carbon carrier, and avoids the agglomeration of Pt.

[0050] Different from the prior art, the preparation method of the porous carbon material and the preparation method of the durable membrane electrode of the present invention use sodium alginate as a carbon precursor, use ammonium borate to introduce B atoms, and introduce nitrogen as N atoms to synthesize NBSPC and use it as a buffer zone between the diffusion layer and the catalytic layer, which effectively reduces the corrosion of the carbon carrier, avoids the agglomeration of Pt, and effectively improves the life of the membrane electrode.

[0051] The present invention and its embodiments are described schematically above, and the description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and designs a structural method and an embodiment similar to the technical solution without creativity without departing from the purpose of the invention, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a durable membrane electrode, It is characterized in that The following steps are involved: S1. Dissolve sodium alginate SA and ammonium borate in water and stir to prepare a mixed solution; S2. The mixed solution obtained in S1 is subjected to hydrothermal treatment and freeze drying to obtain a SA precursor, wherein the SA precursor is a sodium alginate-derived precursor; S3. Take the SA precursor, calcine it at high temperature, and then pyrolyze it in N 2 The reaction was carried out under an atmosphere, and then washed with hydrochloric acid and deionized water, dried and ground into NBSPC, which is a porous carbon derived from SA doped with B and N; S4. Take the NBSPC obtained in S3, dissolve it in an organic solvent, and prepare a slurry after ultrasonic dispersion. The slurry is sprayed on the cathode diffusion layer and the anode diffusion layer. The NBSPC loading of the anode diffusion layer is greater than the NBSPC loading of the cathode diffusion layer. S5. Spray the catalyst slurry onto the cathode diffusion layer and the anode diffusion layer obtained in step S4 to form a catalytic layer, and NBSPC forms a porous buffer zone between the diffusion layer and the catalytic layer; S6. Hot-pressing the cathode diffusion layer, the proton exchange membrane, and the anode diffusion layer to obtain the final membrane electrode.

2. The method for preparing a durable membrane electrode according to claim 1, It is characterized in that The NBSPC loading of the cathode diffusion layer in step S4 is 0.2 mg / cm 2 The NBSPC loading of the anode diffusion layer is 0.05 mg / cm 2 .

3. The method for preparing a durable membrane electrode according to claim 2, It is characterized in that The catalyst loading of the cathode diffusion layer in step S5 is 0.3 mg / cm 2 The catalyst loading of the anode diffusion layer is 0.1 mg / cm 2 .

4. The method for preparing a durable membrane electrode according to claim 3, It is characterized in that The hot pressing temperature in step S6 is 120-150° C., the hot pressing time is 3-5 min, and the hot pressing pressure is 120-150 kPa.

5. The method for preparing a durable membrane electrode according to claim 1, It is characterized in that In step S1, the mass ratio of sodium alginate SA to ammonium borate is 1:5-5:

2.

6. The method for preparing a durable membrane electrode according to claim 5, It is characterized in that In step S1, sodium alginate SA and ammonium borate are dissolved in water and stirred for more than 24 hours by a stirrer at a speed of 200-500 rpm and a stirring temperature of 25°C.

7. The method for preparing a durable membrane electrode according to claim 1, It is characterized in that In step S2, the mixed solution is placed in a high-temperature reactor under a reaction condition of 160-180° C., and after being fully hydrothermal for more than 12 hours, the reactor is placed in a freezing environment of -50 to -30° C. and freeze-dried for 48 hours.

8. The method for preparing a durable membrane electrode according to claim 1, It is characterized in that In step S3, the SA precursor is pyrolyzed in a tube furnace at a calcination temperature of 600-800°C and a heating rate of 5°C / min, and then heated at N 2 The mixture was reacted for 2 h under atmosphere, cooled to room temperature, washed with 1 mol / L hydrochloric acid and deionized water, dried at 80°C for 6-8 h, and ground to obtain NBSPC.