Preparation method and application of pyrazole dicarboxylate copper-based coordination polymer suitable for fertilizer
The copper-based coordination polymer of pyrazole dicarboxylate prepared by hydrothermal method is used as an urease inhibitor, which solves the problem of poor inhibition rate of copper-based coordination polymers in the prior art, and achieves efficient urea hydrolysis inhibition and high yield , suitable for fertilizer applications.
Patent Information
- Application Number
- CN202411111680.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-14
AI Technical Summary
In the prior art, the inhibition rate of copper-based coordination polymers as urease inhibitors in fertilizers is poor, and the yield is difficult to meet the requirements of industrial applications.
The hydrothermal method is used to construct a copper-based coordination polymer with 3,5-pyrazole dicarboxylic acid and CuCl2·2H2O. The high-efficiency copper-based coordination polymer of pyrazole dicarboxylic acid is formed as urease inhibition. The agent is used in fertilizers.
It has achieved effective inhibition of urease activity, extended the urea hydrolysis time, reduced the decomposition of nitrogen fertilizer and environmental pollution, and the yield of copper-based coordination polymer is high, which is suitable for a wide range of applications in fertilizers.
Smart Images

Figure CN118638322B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal complex preparation, and specifically relates to a preparation method and application of a pyrazoledicarboxylate copper-based coordination polymer suitable for fertilizers. Background Art
[0002] Coordination polymers are a type of polymer material formed by metal ions or metal clusters connected to organic ligands through coordination bonds. Common metal ions or metal clusters are copper, zinc, cobalt, etc., and organic ligands are usually organic molecules containing multiple coordination atoms. Coordination polymers have a highly ordered pore structure and can be used for gas adsorption, storage and separation. Due to the rich active sites of coordination polymers, they are often used in catalytic reactions such as photocatalysis and water decomposition. Some coordination polymers show unique magnetic or optical properties and can be used in sensors, data storage, drug delivery, biosensors and other fields.
[0003] In the use of fertilizers, urease activity is a key factor affecting urea hydrolysis. Controlling the activity of urease in the first step of urea hydrolysis can slow down the hydrolysis rate of urea and reduce nitrogen loss. At present, a more common practice is to add an appropriate amount of urease inhibitors to urea. Among them, Cu-containing coordination polymers have attracted widespread attention as urease inhibitors. Cu coordination polymers can not only inhibit the activation process of urease apoprotein, but also fill in the active pocket of urease well, establish interactions with the active sites of urease, so that the active center sites of urease are occupied, thereby causing irreversible inhibition of urease activity, and then blocking the path of urea entering the active site, achieving the effect of inhibiting urease activity, effectively reducing ammonia volatilization, and improving urea utilization.
[0004] In the prior art, the solution method is basically adopted to prepare Cu coordination polymer, and by controlling the temperature, pH value and other conditions of the solution, the coordination polymer is self-assembled to form. Although the Cu coordination polymer obtained by this preparation method can play an inhibitory effect on urease, there is a lower crystal quality, and the inhibitory effect on urease is relatively poor. For example, in the patent of CN109456343A in the prior art, the amount of coordination polymer as urease inhibitor additive is relatively large, and the inhibitory effect is relatively poor. Meanwhile, another major factor restricting Cu coordination polymer is exactly productivity, and Cu coordination polymer needs to have higher productivity and urease inhibition rate when forming industrial application, and Cu coordination polymer in the prior art is difficult to meet this requirement, and therefore still has certain difficulties in industrial formation and application. Summary of the invention
[0005] The present application proposes a preparation method and application of a pyrazoledicarboxylic acid copper-based coordination polymer suitable for fertilizers, aiming to develop a copper-based coordination polymer and a preparation method thereof, by adding a smaller amount of the copper-based coordination polymer to the fertilizer to inhibit urease, thereby solving the technical problem of poor inhibition rate of the copper-based coordination polymer in the above-mentioned prior art, while also ensuring that the copper-based coordination polymer has a higher yield.
[0006] The technical scheme adopted by the invention is: a preparation method of a pyrazole dicarboxylic acid copper-based coordination polymer, the preparation method comprising: using 3,5-pyrazole dicarboxylic acid as a ligand and CuCl2·2H2O to construct a copper-based coordination polymer by a hydrothermal method.
[0007] Furthermore, the preparation method comprises the following steps:
[0008] Step 1, weighing CuCl2·2H2O and 3,5-pyrazoledicarboxylic acid and putting them into a tetrafluoroethylene liner;
[0009] Step 2, adding deionized water and sodium hydroxide into the tetrafluoroethylene liner to dissolve CuCl2·2H2O and 3,5-pyrazoledicarboxylic acid;
[0010] Step 3, placing the tetrafluoroethylene liner of step 2 into a hydrothermal reactor, sealing the reactor, and heating it in an oven at a constant temperature of 120-150° C. for 4 to 5 days. After obtaining blue block crystals, the block crystals are washed, filtered and dried to obtain a copper-based coordination polymer of pyrazole dicarboxylate.
[0011] Preferably, the molar ratio of the 3,5-pyrazoledicarboxylic acid to copper chloride is 1-2:2.
[0012] Preferably, the preparation method is:
[0013] Step 1, weighing 0.015g of ligand 3,5-pyrazoledicarboxylic acid and 0.034g of CuCl2·2H2O, and placing them in a tetrafluoroethylene liner; Step 2, adding 7mL of deionized water into the tetrafluoroethylene liner to dissolve CuCl2·2H2O and 3,5-pyrazoledicarboxylic acid, and adding 3mL of NaOH sodium hydroxide with a concentration of 0.1mol / L into the tetrafluoroethylene liner; Step 3, placing the tetrafluoroethylene liner of step 1 and step 2 into a hydrothermal autoclave, sealing the autoclave, and heating it in a drying oven at 120°C for 4 days, and then washing, filtering and drying the block crystals to obtain a pyrazoledicarboxylic acid copper-based coordination polymer.
[0014] A pyrazole dicarboxylic acid copper-based coordination polymer prepared by the preparation method, wherein the copper-based coordination polymer is based on Cu Ⅱ The complex has a monoclinic crystal form and a space group of P21 / m.
[0015] The invention discloses an application of a pyrazole dicarboxylate copper-based coordination polymer as a urease inhibitor.
[0016] The invention discloses an application of a pyrazole dicarboxylate copper-based coordination polymer as a urease inhibitor in a fertilizer containing urea.
[0017] Compared with the prior art, the preparation method of the pyrazole dicarboxylic acid copper-based coordination polymer of the present invention is simple, the structure is simple, the safety is high, and the urease activity is well inhibited. The urease structure can be denatured and inactivated, the conversion of urea nitrogen to ammonium nitrogen can be inhibited, the hydrolysis time of urea can be prolonged, the release period of fertilizer urea can be effectively delayed, the decomposition of nitrogen fertilizer can be delayed, and the loss of fertilizer urea can be reduced. The copper-based coordination polymer has the characteristics of long time effectiveness, and adding a smaller amount can better reduce the environmental pollution problem caused by the fertilizer during the release process, solve the technical problem of poor inhibition rate of the copper-based coordination polymer in the prior art, and also ensure that the copper-based coordination polymer has a higher yield. Therefore, it can be widely used in fertilizer urea. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0019] Figure 1 This is a single crystal data diagram of copper-based coordination polymer;
[0020] Figure 2 The figure is a comparison between the powder X-ray diffraction pattern of the copper-based coordination polymer and the simulated single crystal data;
[0021] Figure 3 This is the half-inhibitory concentration diagram of copper-based coordination polymers as urease inhibitors. DETAILED DESCRIPTION
[0022] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0023] The present invention provides a method for preparing a pyrazole dicarboxylic acid copper-based coordination polymer suitable for fertilizers. The present invention mainly uses 3,5-pyrazole dicarboxylic acid as a ligand and CuCl2·2H2O to construct a copper-based coordination polymer by a hydrothermal method, and specifically comprises the following steps:
[0024] Step 1, weighing CuCl2·2H2O and 3,5-pyrazoledicarboxylic acid and putting them into a tetrafluoroethylene liner;
[0025] Step 2, adding deionized water and sodium hydroxide into the tetrafluoroethylene liner to dissolve CuCl2·2H2O and 3,5-pyrazoledicarboxylic acid;
[0026] Step 3, placing the tetrafluoroethylene liner of step 2 into a hydrothermal reactor, sealing the reactor, and heating it in an oven at a constant temperature of 120-150° C. for 4 to 5 days. After obtaining blue block crystals, the block crystals are washed, filtered and dried to obtain a copper-based coordination polymer.
[0027] 1. The following is an example of a specific preparation of a copper-based coordination polymer: Embodiment 1
[0028] 0.015 g (0.1 mmol) of the ligand 3,5-pyrazoledicarboxylic acid and 0.034 g (0.2 mmol) of CuCl2·2H2O were weighed and placed in a tetrafluoroethylene liner. 7 mL of deionized water and 3 mL of 0.1 mol / L NaOH solution were added. The reactor was sealed and heated in a drying oven at 120 °C for 4 days. The block crystals were then washed, filtered and dried to obtain a blue block copper-based coordination polymer with a yield of about 51%. Embodiment 2
[0029] 0.031 g (0.2 mmol) of the ligand 3,5-pyrazoledicarboxylic acid and 0.034 g (0.2 mmol) of CuCl2·2H2O were weighed and placed in a tetrafluoroethylene liner. 7 mL of deionized water and 3 mL of 0.1 mol / L NaOH solution were added. The reactor was sealed and heated in a drying oven at 120 °C for 4 days. The block crystals were then washed, filtered and dried to obtain a blue block copper-based coordination polymer with a yield of about 40%. Embodiment 3
[0030] 0.023 g (0.1 mmol) of the ligand 3,5-pyrazoledicarboxylic acid and 0.034 g (0.2 mmol) of CuCl2·2H2O were weighed and placed in a tetrafluoroethylene liner. 6 mL of deionized water and 2 mL of 0.1 mol / L NaOH solution were added. The reactor was sealed and calcined in a drying oven at 120°C for 4 days. The block crystals were then washed, filtered and dried to obtain a blue block copper-based coordination polymer with a yield of about 46%. Embodiment 4
[0031] 0.015 g (0.1 mmol) of the ligand 3,5-pyrazoledicarboxylic acid and 0.034 g (0.2 mmol) of CuCl2·2H2O were weighed and placed in a tetrafluoroethylene liner. 7 mL of deionized water and 3 mL of 0.1 mol / L NaOH solution were added. The reactor was sealed and heated in a drying oven at 130 °C for 4 days. The block crystals were then washed, filtered and dried to obtain a blue block copper-based coordination polymer with a yield of about 49%. Embodiment 5
[0032] 0.015 g (0.1 mmol) of the ligand 3,5-pyrazoledicarboxylic acid and 0.034 g (0.2 mmol) of CuCl2·2H2O were weighed and placed in a tetrafluoroethylene liner. 7 mL of deionized water and 3 mL of 0.1 mol / L NaOH solution were added. The reactor was sealed and heated in a drying oven at 140 °C for 4 days. The block crystals were then washed, filtered and dried to obtain a blue block copper-based coordination polymer with a yield of about 46%. Embodiment 6
[0033] 0.015 g (0.1 mmol) of the ligand 3,5-pyrazoledicarboxylic acid and 0.034 g (0.2 mmol) of CuCl2·2H2O were weighed and placed in a tetrafluoroethylene liner. 7 mL of deionized water and 3 mL of 0.1 mol / L NaOH solution were added. The reactor was sealed and heated in a drying oven at 150 °C for 4 days. The block crystals were then washed, filtered and dried to obtain a blue block copper-based coordination polymer with a yield of about 50%. Embodiment 7
[0034] 0.015 g (0.1 mmol) of the ligand 3,5-pyrazoledicarboxylic acid and 0.034 g (0.2 mmol) of CuCl2·2H2O were weighed and placed in a tetrafluoroethylene liner. 7 mL of deionized water and 3 mL of 0.1 mol / L NaOH solution were added. The reactor was sealed and heated in a drying oven at 150 °C for 5 days. The block crystals were then washed, filtered and dried to obtain a blue block copper-based coordination polymer with a yield of about 50%.
[0035] Examples 1 to 7 obtain the same type of copper-based coordination polymers of pyrazole dicarboxylate, among which the solution of Example 1 has the best yield, and its preparation method is simpler and uses less raw materials.
[0036] 2. Determination of the Structure of Copper-Based Coordination Polymers of Pyrazole Dicarboxylate
[0037] The single crystal diffraction intensity data were collected on a Bruker D8-ray diffractometer using graphite monochromatized Mo Kα (λ = 0.71073 Å) radiation as the diffraction light source. The crystallographic data table is shown in Table 1. The pyrazole dicarboxylate copper-based coordination polymer (SC-XRD data obtained from the blue block crystals prepared in Example 1, and the structure diagram obtained is shown in FIG. Figure 1 shown), Figure 1 The metal Cu is shown II The coordination environment of the ion is monoclinic, the space group is P21 / m, Cu II The ion adopts a penta-coordinated coordination mode, coordinated with one chlorine atom, two nitrogen atoms on the pyridine ring from the N,N′-bis(3-pyridinecarboxamide)-1,2-ethane ligand, and two oxygen atoms from the benzoate anion (Cu–N = 2.024(3)–2.054(3) Å, Cu–O =1.964(2)–1.983(2) Å, Cu–Cl= 2.5457(9) Å), showing a distorted tetrahedral geometry.
[0038] Table 1. Crystallographic data of copper-based coordination polymers
[0039] The powder diffraction experiments on the crystals were carried out using a Bruker D8 Advance X-ray powder diffractometer: graphite monochromatized CuKα radiation, wavelength λ = 1.54056 Å, solid detector, step size 0.01°, step time 0.3 sec, scanning range 5°≤2θ≤45°. Figure 2 , the powder X-ray diffraction pattern obtained in Example 1 matches the single crystal data simulation pattern.
[0040] Application verification of copper-based coordination polymers based on pyrazole dicarboxylate
[0041] The method is as follows: the pyrazole dicarboxylic acid copper-based coordination polymer prepared in Example 1 is used for the experiment, and 4 mL of copper-based coordination polymer with concentrations of 0.3 μM, 0.6 μM, 1.2 μM, 2.4 μM, 4.8 μM, 9.6 μM, 19.2 μM and 38.4 μM are taken respectively (the sample is dissolved in DMSO, DMSO: H2O = 1:1), and placed in 3 centrifuge tubes respectively, and then 4 mL of 10 KU / L urease is added to each centrifuge tube, and phenol red indicator is added after culturing at 25°C in a constant temperature shaking incubator for 1 hour to obtain a test solution. Immediately thereafter, a UV-visible spectrophotometer is used to measure the absorbance of the test solution at a wavelength of 570 nm, and the measurement is performed every 1 hour to obtain a graph showing the changes in urease inhibition rate of different amounts of copper-based coordination polymers at different times. By Figure 3It can be seen that different added amounts of copper-based coordination polymers have an inhibitory effect on urease, and the higher the concentration, the better the inhibitory effect.
[0042] Urease was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.
[0043] Calculate the half inhibitory concentration IC of urease 50 Value (μM):
[0044] IC was performed using the modified Koch method 50 Calculation of: 1gIC 50 =Xm-I(P-(3-Pm-Pn) / 4), where Xm: 1g maximum dose, I: 1g (maximum dose / adjacent dose), P: sum of positive reaction rates, Pm: maximum positive reaction rate, Pn: minimum positive reaction rate. IC 50 =0.98±0.05μM, while the IC 50 At 0.62 μM <IC 50 <42.74 μM. Therefore, it can be concluded that the copper-based coordination polymer of pyrazole dicarboxylate of the present invention can be used as a urease inhibitor in urea fertilizer, and the copper-based coordination polymer of pyrazole dicarboxylate as a urease inhibitor has a low half inhibition concentration. Compared with the prior art, the copper-based coordination polymer proposed in the present invention has an IC 50 The value is smaller, which can illustrate the application of the copper-based coordination polymer prepared in the present invention as a urease inhibitor, and the amount of the additive is small, the inhibitory effect on urease is stronger, and the yield can be maintained above 40, with a higher yield.
[0045] At the same time, the copper-based coordination polymer of pyrazole dicarboxylate in the present invention can be added to the fertilizer urea as a urease inhibitor, which can inhibit the urease activity to prolong the decomposition time of urea, reduce the nitrogen loss in the fertilizer, and improve the fertilizer utilization rate.
[0046] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a copper-based coordination polymer of pyrazole dicarboxylate suitable for fertilizer, characterized in that: The preparation method is to use 3,5-pyrazoledicarboxylic acid as a ligand and CuCl2·2H2O to construct a copper-based coordination polymer by a hydrothermal method, which specifically includes the following steps: Step 1, weighing CuCl2·2H2O and 3,5-pyrazoledicarboxylic acid and putting them into a tetrafluoroethylene liner, wherein the molar ratio of 3,5-pyrazoledicarboxylic acid to CuCl2·2H2O is 1-2:2; Step 2, adding deionized water and sodium hydroxide into the tetrafluoroethylene liner to dissolve CuCl2·2H2O and 3,5-pyrazoledicarboxylic acid; Step 3, placing the tetrafluoroethylene liner of step 2 into a hydrothermal reactor, sealing the reactor, and heating it in an oven at a constant temperature of 120-150° C. for 4 to 5 days. After obtaining blue block crystals, the block crystals are washed, filtered and dried to obtain a copper-based coordination polymer of pyrazole dicarboxylate.
2. The preparation method according to claim 1, characterized in that: The preparation method is: Step 1, weigh 0.015 g of ligand 3,5-pyrazoledicarboxylic acid and 0.034 g of CuCl2·2H2O, and place them in a tetrafluoroethylene liner; Step 2, add 7 mL of deionized water into a tetrafluoroethylene liner to dissolve CuCl2·2H2O and 3,5-pyrazoledicarboxylic acid, and add 3 mL of NaOH with a concentration of 0.1 mol / L into the tetrafluoroethylene liner; Step 3, placing the tetrafluoroethylene liner of step 2 into a hydrothermal reactor, sealing the reactor, heating it in a drying oven at 120° C. for 4 days, and then washing, filtering and drying the block crystals to obtain a copper-based coordination polymer of pyrazole dicarboxylate.
3. A pyrazole dicarboxylate copper-based coordination polymer prepared by the preparation method according to claim 1 or 2, characterized in that: The copper-based coordination polymer is based on Cu Ⅱ The complex has a monoclinic crystal form and a space group of P21 / m.
4. Use of the copper-based coordination polymer of pyrazoledicarboxylate as claimed in claim 3 as a urease inhibitor.
5. Use of the copper-based coordination polymer of pyrazoledicarboxylate as claimed in claim 3 as a urease inhibitor in fertilizers containing urea.