A 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod and a manufacturing method thereof

Through the design of C-Si-Mn-V components and tempering tissue regulation, combined with the online salt bath strong tempering and roller slow cooling technology, the high cost and abnormal tissue precipitation problems of cold heading steel strips for fasteners are solved. High strength and plasticity fastener manufacturing is achieved, suitable for the annealing-free needs of 15.9-level fasteners.

CN118639123BActive Publication Date: 2024-11-19JIANGSU YONGGANG GROUP CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411133210.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-19
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

In the high-strength grade manufacturing of existing cold heading steel strips for fasteners, there are problems such as high material cost, high risk of abnormal tissue precipitation, and difficult to meet the demand for annealing, especially the brittleness and cracking risks caused by the increase of carbon content. overcome.

Method used

The high-carbon alum-containing component design of C-Si-Mn-V is designed, and the plasticity of the strip is significantly improved through tempered pearlite and tempered soxunite tissue regulation, combined with online salt bath strong tempering and roller slow cooling technology. and strength, avoid annealing processes and simplify manufacturing processes.

Benefits of technology

Achieve high tensile strength and cross-section shrinkage rate of 15.9-level fasteners, reduce material costs and cracking risks, improve material yield and manufacturing efficiency, significantly improve the plasticity and strength of the strips, and is suitable for small-sized fasteners manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639123B_ABST
    Figure CN118639123B_ABST
Patent Text Reader

Abstract

The present invention relates to a 15.9-grade annealing-free hot-rolled high-carbon vanadium-containing cold heading steel wire rod and a manufacturing method thereof. The wire rod is rolled and spun into a wire rod by adopting a high-carbon vanadium-containing component design of C-Si-Mn-V, and then subjected to online salt bath strong tempering. The wire rod is first subjected to a front-stage molten salt, and the wire rod is cooled to a troostite phase region at a cooling rate of ≥41°C / s, and partially transformed into a troostite structure. The wire rod is then subjected to a rear-stage molten salt and heated to a pearlite phase region for isothermal treatment, so as to promote pearlite structure transformation, tempering softening and containing Vanadium carbides are precipitated and finally slowly cooled on a roller to form cold heading steel wire rods with a microstructure including tempered pearlite, tempered troostite and quasi-spheroidized carbides. This can improve the utilization value of carbon and vanadium, reduce material costs, achieve strength-plasticity matching, achieve a tensile strength of 1320~1370MPa, and a cross-sectional shrinkage of 45%~50%. It can be used to manufacture 15.9 grade fasteners without the annealing process, reduce the risk of cracking, and improve the yield rate and manufacturing efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and specifically relates to a 15.9-grade annealing-free hot-rolled high-carbon vanadium-containing cold-heading steel wire rod and a manufacturing method thereof. Background Art

[0002] Bolts, screws and other fasteners are the most applicable and basic mechanical connection parts with a wide range of applications. In recent years, with the rapid development of new energy vehicles, higher strength grade fasteners are conducive to reducing the weight of the vehicle body and improving the driving range of new energy vehicles. Therefore, the performance requirements for the raw material cold heading steel wire rod for fasteners have also increased. At present, the existing fastener strength grade is mainly 10.9~12.9, and is produced and manufactured using a medium and low carbon alloying component system. Fasteners with higher strength grades need to add more strengthening alloy elements for research and development and manufacturing, such as:

[0003] Patent CN114058974B discloses a 15 .9 grade corrosion-resistant high-strength bolt steel and its production method and heat treatment method adopt C-Si-Mn-Cr-Mo-V-Nb-Ti-B-Ni-Cu-Al composition design, combined with billet rolling, high-temperature heating rough rolling, medium rolling, low-temperature sizing and slow cooling on a cooling bed for excellent rod rolling, to obtain pearlite + ferrite, hot-rolled structure without bainite, martensite and other hard phase structures, further through reheating deformation heat treatment and high-frequency tempering heat treatment to obtain tempered troostite + dispersed carbide structure, but first, the material contains high content of Si, Cr, Mo, also contains V, Nb, Ti and other micro-alloy components, V has a high alloy content, which brings a significant increase in material cost. For the purpose of reducing material cost, omitting alloy components or reducing alloy content will lead to loss of steel strength, and it is difficult to achieve 15.9 grade performance level in subsequent quenching and tempering processing; second, the high alloying component system brings increased hardenability, aggravates rolling The risk of precipitation of abnormal structures such as martensite and bainite that deteriorate the drawing performance during the post-cooling process will lead to brittle fracture during the coiling, transportation or uncoiling of the wire rod, causing a decrease in the yield rate. In order to reduce the risk of abnormal structure precipitation, round steel is used to avoid brittle fracture during coiling, but it is impossible to directly obtain wire rods with smaller diameters through high-wire rolling, which is not conducive to the production of small-sized fasteners. The use of controlled rolling and controlled cooling followed by offline heat treatment to optimize the structure will increase the process and cost, affecting production efficiency; third, the addition of more strengthening alloy elements greatly weakens the plasticity and cold working properties of the material. Before drawing and cold heading in the manufacturing of fasteners, multiple spheroidizing annealing processes are required to improve the cold working performance. At the same time, it brings problems such as increased manufacturing processes, emissions, energy consumption and costs of fasteners. It is even impossible to meet the plasticity requirements through annealing, causing processing cracking. Therefore, in order to save the annealing process, the development of hot-rolled cold heading steel wire rods for corresponding 15.9-grade fasteners brings greater challenges.

[0004] Carbon is a necessary and economical element for fastener steel to obtain high strength. Replacing alloy elements is beneficial to reducing steel costs. However, the high-carbon steel used in the prior art mainly improves the drawing performance by increasing the troostite content in the organization. It is used in the fields of cords, bridge cables, etc. The technical difficulties and causes of its difficulty in applying to the manufacture of cold heading steel wire rods are: First, with the increase of carbon content, due to the limitation of the Stelmor air cooling control method after rolling and spinning, increasing the cooling rate will aggravate the temperature difference of the wire rod, aggravate the precipitation of abnormal organization and increase the wire rod. Brittleness, the risk of the plasticity of the wire rod decreasing too quickly, the existing high carbon steel will use low-speed or heat preservation cooling to reduce the risk of low-temperature microstructure precipitation, prolong the time of the wire rod in the troostite phase area to increase the proportion of troostite, but the low-speed cooling will make the wire rod stay in the precipitation interval of secondary cementite for a longer time, produce serious network carbides and affect the uniformity of the organization, especially significantly deteriorate the plasticity and toughness performance, cause the risk of cracking, and cannot meet the requirement of no annealing; second, the increase in carbon content increases the difficulty of improving plasticity, and it is directly used after spinning. Low-speed or heat-insulating cooling is difficult to produce a large degree of supercooling, and the resulting troostite lamellae are coarse. After adding strengthening elements such as Mn to the material, the activity of C is suppressed, which slows down the diffusion, and the cementite precipitation becomes coarser, making it more difficult to soften. At the same time, during the continuous cooling process, the wire rod is already in a low-temperature state after being inoculated with troostite, and the driving force is insufficient, and it is ultimately unable to soften. The resulting tissue has a high dislocation density, causing drawing hardening or cold heading cracking, and it is even more impossible to meet the requirements of annealing-free; Third, although some annealing-free cold heading steel wire rods are increased in the organization The ferrite content is used to improve the plasticity of the wire rod, but the strength of the wire rod will be excessively deteriorated. In the process of strengthening the bolts by large surface reduction drawing, the plasticity loss is large, which will aggravate the risk of cold heading cracking. Fourth, although the V element is added to improve the comprehensive performance of the wire rod by utilizing the grain refinement and precipitation strengthening effects of the microalloy, the driving force of the precipitation phase is small during the low-speed or heat-insulated continuous cooling process after spinning, and it is difficult to precipitate or the precipitation coarsening causes the utilization rate of V to decrease, resulting in the loss of strengthening effect, or the need to increase the amount of V and bring cost pressure. Summary of the invention

[0005] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a 15.9-grade annealing-free hot-rolled high-carbon vanadium-containing cold heading steel wire rod and a manufacturing method thereof, which can improve the utilization value of carbon and vanadium, reduce material costs, achieve wire rod structure regulation and strength-plasticity matching, and especially significantly improve the plasticity of the wire rod. It can be used to manufacture 15.9-grade fasteners without the annealing process, reduce the risk of cracking, and improve the yield rate and manufacturing efficiency.

[0006] The technical solution adopted by the present invention to solve its technical problem is:

[0007] A 15.9 grade annealing-free hot-rolled high-carbon vanadium-containing cold heading steel wire rod, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.86%-0.90%, Si: 0.70%-0.82%, Mn: 0.50%-0.70%, V: 0.03%-0.05%, P≤0.015%, S≤0.015%, the rest is Fe and unavoidable impurities, and the microstructure thereof includes a mixed structure consisting of tempered pearlite accounting for 55%-65% by volume, tempered troostite accounting for 34%-40% by volume, and the rest is quasi-spheroidized carbides.

[0008] The chemical composition and mass percentage design basis of the above-mentioned cold heading steel high carbon wire rod include:

[0009] (1) Carbon: Carbon is the most economical and effective element for solid solution strengthening and precipitation strengthening. It is the main added element in the present invention. It is used to ensure that the wire rod can reach the tensile strength and yield strength of the 15.9 grade fastener after quenching and tempering. At the same time, as an austenite-forming element, it can expand the austenite phase region and inhibit the formation of ferrite, but it also increases the decarburization sensitivity and the risk of cementite being distributed in a network along the grain boundary. If the C content is too high, the resulting tissue layer in the medium temperature range will be thicker, which will increase the difficulty of softening the wire rod and is not conducive to the control of the matrix structure. Therefore, based on material cost considerations, facilitating tissue control, ensuring the cold deformation performance of the cold heading steel wire rod without annealing, and meeting the final performance level requirements of the 15.9 grade bolt, the mass percentage of C is controlled to be 0.86%~0.90%.

[0010] (2) Silicon: Si is the main deoxidizing element in the smelting process. It can improve the tensile strength, yield strength and hardness of cold heading steel. At the same time, increasing the Si content can increase the C activity during online salt bath strong tempering, inhibit the precipitation of cementite, make the cementite thinner, and reduce the difficulty of carbide transformation to spheroidized structure during high-temperature molten salt isothermal process, which is convenient for structure softening and improves the plasticity of wire rod. Compared with Mo element which can inhibit the precipitation of cementite, Si is cheaper, which is beneficial to cost control. However, excessive silicon will increase the brittle inclusions and surface decarburization sensitivity, causing cold heading cracking during cold heading deformation. As a ferrite-forming element, Si is too high, which is not conducive to the inhibition of ferrite precipitation during pearlite transformation. Therefore, the mass percentage of Si is controlled to be 0.70%~0.82%.

[0011] (3) Manganese: Mn is often used as a deoxidizer in steel. Mn and Fe form a solid solution, which can improve the strength and hardenability of steel. At the same time, as an austenite-forming element, it can expand the austenite phase region and inhibit the formation of ferrite. It can also refine pearlite in steel. However, too high Mn content will aggravate the segregation during the solidification process of the steel billet, reduce the activity of carbon and the diffusion rate of carbon, which is not conducive to the spheroidization of carbides, increase the overheating sensitivity of steel and the risk of abnormal structure. Too high Mn content will also increase material costs. Therefore, the mass percentage of Mn is controlled to be 0.50%~0.70%.

[0012] (4) V: As a microalloying element, V can promote the formation of pearlite and inhibit the formation of bainite. The solid solution temperature of V is lower than that of Nb. It can prevent the grain growth of wire rod by dispersion precipitation in the medium temperature range of the online salt bath strong tempering stage, greatly improving the strength and hydrogen embrittlement resistance of the material. However, the price of V is relatively high. Excessive addition is not conducive to controlling the cost of cold heading steel wire rod and has the risk of coarsening. Therefore, based on the role of V and cost considerations, the mass percentage of V is controlled to be 0.03%~0.05%.

[0013] (5) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.

[0014] The above-mentioned cold heading steel wire rod adopts the high carbon and vanadium-containing composition design of C-Si-Mn-V, and C is used to replace the addition of alloy components such as Cr, Ni, Nb, B, and Mo. Si, Mn, and V are less than the existing 15.9 grade fastener steel, which can effectively reduce the material cost, and strengthen the composition system and hardenability of the material to ensure that the final performance level can be achieved after quenching and tempering. The microstructure includes most of the tempered pearlite, a small part of the tempered troostite and a small amount of quasi-spheroidized carbide, and cooperates with the austenite forming elements C and Mn to expand the austenite phase area and inhibit the precipitation of ferrite. The interlamellar spacing of pearlite is larger than that of troostite, the plasticity is higher than that of troostite, and the strength is higher than that of ferrite. The pearlite is transformed into tempered pearlite after tempering. The tempered pearlite can retain the moderate strength of pearlite and further improve the organizational stress and dislocation density. The interlamellar spacing of troostite is smaller than that of pearlite, the strength is higher than that of pearlite, and the plasticity is better than that of bainite and martensite. After troostite is transformed into tempered troostite after tempering, the tempered troostite can retain the better strength of troostite and further reduce the dislocation density of troostite. Si is combined to increase the C activity and inhibit the precipitation of cementite, so that the carbides in pearlite and troostite are easier to be transformed into quasi-spheroidized carbides. After the carbides of V are dispersed and precipitated, they can be evenly distributed on the plastic matrix.

[0015] Therefore, compared with the existing low-medium carbon hot-rolled cold-heading steel structure composed of pearlite + ferrite, the cold-heading steel wire rod can be regulated by tempering pearlite and tempering bainite structure, and cooperate with carbon solid solution strengthening and alum precipitation strengthening to obtain higher matrix strength, making up for the strength loss caused by eliminating alloys and reducing alloy content. Compared with the existing high-carbon steel wire rod with high bainite rate, the cold-heading steel wire rod can obtain a significantly softened matrix structure by regulating the tempering structure state, and significantly improve the plasticity of the wire rod without excessively deteriorating the strength of the wire rod. Compared with the hot-rolled cold-heading steel wire rod containing bainite, it can effectively avoid brittle fracture of coiling, and is more suitable for manufacturing 15.9 grade fasteners to avoid wire breakage and cold heading cracking when annealing process is omitted.

[0016] The finer the lamellar spacing of the tempered pearlite and the tempered bainite, the higher the strength of the wire rod and the lower the plasticity. However, too coarse lamellar spacing is not conducive to drawing and cold heading. In a preferred embodiment, the lamellar spacing of the tempered pearlite is 160~200nm, and the lamellar spacing of the tempered bainite is 70~110nm.

[0017] In a preferred embodiment, the network carbide of the cold heading steel wire rod is level 0, which can effectively suppress the influence of the network carbide and enhance the strengthening effect of the carbon element.

[0018] In a preferred embodiment, the diameter of the cold heading steel wire rod is 8.0~15.0mm, the tensile strength is 1320~1370MPa, and the cross-sectional shrinkage rate is 45%~50%. Compared with round steel manufacturing, cold heading steel wire rods with smaller diameters are more convenient for manufacturing fasteners with smaller specifications. The wire rod has a higher tensile strength and does not require deep drawing to strengthen it to approach the 15.9 performance level, avoiding the risk of cracking caused by excessive loss of wire rod plasticity during drawing and cold heading. The wire rod has significantly improved plasticity, which is manifested as a higher cross-sectional shrinkage rate. The annealing process in the fastener manufacturing process can be omitted, and 15.9-grade fasteners can be manufactured through drawing, cold heading and tempering treatment, simplifying the manufacturing process.

[0019] A method for manufacturing a 15.9 grade annealing-free hot-rolled high-carbon vanadium-containing cold heading steel wire rod, wherein the chemical composition of the 15.9 grade annealing-free hot-rolled high-carbon vanadium-containing cold heading steel wire rod described in any one of the above items is rolled to produce a wire rod, the wire rod is spun into a wire rod at a spinning temperature of ≥940°C, and then subjected to online salt bath strong tempering, so that the wire rod is first subjected to a front-stage molten salt treatment, the wire rod is cooled to a sorbite phase region at a cooling rate of ≥41°C / s, and a part of the austenite structure in the wire rod is transformed into a sorbite phase region. The steel wire rod is subjected to isothermal treatment to promote the transformation of the untransformed austenite structure in the wire rod into the pearlite structure, and at the same time promote the tempering softening and the precipitation of vanadium-containing carbides. Finally, it is slowly cooled by rollers to produce a cold heading steel wire rod with a microstructure including 55% to 65% tempered pearlite by volume, 34% to 40% tempered troostite by volume, and the rest being a mixed structure composed of quasi-spheroidized carbides.

[0020] The manufacturing method adopts a higher spinning temperature. On the one hand, it can avoid the precipitation of secondary cementite in the spinning stage, which is used to control the network carbon. On the other hand, it is beneficial to form a large undercooling degree and sorbite nucleation in the subsequent online salt bath strong tempering. After spinning, the online salt bath strong tempering is directly carried out. The wire rod first passes through the front section molten salt with a lower temperature than the rear section molten salt. On the one hand, compared with the existing low-speed cooling, insulation cooling and even strong air cooling control after spinning, the high heat exchange capacity of the molten salt can be used to quickly cool the wire rod, effectively shortening the residence time in the network carbon area, thereby avoiding the network carbide to the high carbon. On the other hand, it can quickly bypass the ferrite precipitation zone, form a large degree of supercooling, enter the troostite phase zone, promote the partial transformation of the high-temperature austenite structure in the wire rod into troostite, and regulate the troostite content of the wire rod matrix. At the same time, compared with air cooling, the increase in cooling rate will cause abnormal tissue precipitation due to the temperature difference of the wire rod. When the wire rod passes through the molten salt, the molten salt can wrap the surface of the wire rod for uniform heat transfer. There is no temperature difference problem between the windward side and the leeward side, which can reduce the fluctuation of mechanical properties, avoid the precipitation of abnormal tissue, and make organizational preparations for subsequent tempering regulation.

[0021] The wire rod is then subjected to the temperature increase control of the molten salt in the latter stage. On the one hand, compared with the existing continuous cooling process such as heat preservation after spinning, it can be heated to the pearlite phase region, promoting the transformation of the untransformed structure in the wire rod into the pearlite structure with a larger interlamellar spacing than that of the troostite, and can cooperate with the austenite forming elements C and Mn to inhibit the precipitation of ferrite, and regulate the strength and plasticity of the matrix; on the other hand, it can keep the wire rod and the molten salt temperature consistent, so that the wire rod can be subjected to high-temperature isothermal treatment in the pearlite phase region for a longer time, instead of continuous cooling, and cooperate with Si to increase the C activity and inhibit the precipitation of cementite. The formed troostite and pearlite structures are tempered and softened, and the carbides therein are transformed into spheroidized structures, which soften the matrix, can reduce the organizational stress and dislocation density, and make it difficult for cracks to initiate and propagate. At the same time, in the precipitation temperature range of V-containing carbides, under the action of a long time, the driving force is greater, and nucleation can be formed inside the matrix to form a large number of fine interphase precipitations, thereby improving the utilization value of V dispersion strengthening, effectively improving the strength and hydrogen embrittlement resistance of the material, and due to sufficient organizational transformation, it can also avoid the generation of abnormal organizations in the subsequent roller slow cooling process.

[0022] When the wire rod is finally slowly cooled by the roller, the high temperature state of the wire rod after passing through the molten salt in the latter stage can be used to further soften the matrix, thereby achieving final microstructure regulation and strength-plasticity matching of the wire rod. Since the brittle fracture of coiling can be avoided, smaller wire rods can be directly obtained through high-wire rolling, and the manufacturing of round steel can save processes such as blanking and forging. Since wire rods with higher plasticity can be obtained directly, the offline heat treatment process after coiling can be saved, thereby simplifying the process and improving manufacturing efficiency and yield rate.

[0023] A higher heating furnace temperature and a longer time in the furnace are selected to promote uniform composition of the steel billet before rolling and avoid the risk of decarburization caused by too long a time. In a preferred embodiment, the heating furnace temperature is controlled to be 1050-1100°C before rolling, and the time in the furnace is 3-5h.

[0024] Since a higher spinning temperature is selected, the limitation of low-temperature spinning on low-temperature rolling can be broken, and a higher rolling temperature is selected to improve rolling efficiency, reduce the deformation resistance of the steel billet and the wear of the rolling line. Therefore, a higher initial rolling temperature can be selected to start rolling, and a larger initial rolling reduction can be used to refine the original austenite grains. In a preferred embodiment, during the rolling, the initial rolling temperature is controlled to be 1030~1080℃, and the initial rolling reduction is 28%~35%.

[0025] In a preferred embodiment, during the rolling, the heavy-load finishing rolling temperature is ≥960°C, the finishing rolling reduction is 8%~18%, and a larger finishing rolling reduction is selected to promote recrystallization of steel in austenite, refine the wire grains, and strengthen the matrix.

[0026] In a preferred embodiment, the molten salt temperature of the front-stage molten salt is 520~550℃, and the processing time is 30~40s. The lower the molten salt temperature of the front-stage molten salt and the longer the processing time, the greater the degree of supercooling, the finer the sorbite lamellae spacing, the more sorbite transformation, the higher the proportion of tempered sorbite, the higher the strength of the wire rod and the lower the plasticity. However, if the molten salt temperature is too low, the sorbite lamellae are too fine, and there is even a risk of bainite structure, which will significantly affect the plasticity of the wire rod. On the contrary, if the molten salt temperature is higher and the processing time is shorter, the sorbite lamellae spacing becomes coarser, the proportion of tempered sorbite decreases, the strength of the wire rod decreases, and the plasticity increases. However, if the molten salt temperature is too high, it is not conducive to controlling the nucleation of network carbides and sorbite. Therefore, the molten salt temperature and processing time of the front-stage molten salt can be further regulated to prepare the organization for the rear-stage molten salt treatment.

[0027] In a preferred embodiment, the molten salt circulation rate of the front-stage molten salt is 50-150 t / h, and the molten salt temperature rise is controlled to be ≤12°C, which can control the processing accuracy of the wire rod passing through the front-stage molten salt and avoid abnormal tissue.

[0028] In a preferred embodiment, the molten salt temperature of the rear-stage molten salt is 580-620°C, and the processing time is 550-800s. The lower the molten salt temperature of the rear-stage molten salt, the smaller the spacing between the pearlite lamellae formed, which can provide more power for the precipitation of vanadium-containing carbides, form finer phase precipitation, increase the strength of the wire rod and decrease the plasticity, but the molten salt temperature is too low, which is not conducive to the pearlite phase transformation, the proportion of tempered pearlite, and the plasticity of the matrix, and is not conducive to the precipitation of vanadium-containing carbides in the medium temperature range; on the contrary, the higher the molten salt temperature, the coarser the spacing between the pearlite lamellae formed, which can provide more power for high-temperature isothermal tempering spheroidization and softening, reduce the strength of the wire rod and increase the plasticity, but the molten salt temperature is too high, and the pearlite lamellae are too coarse. Even ferrite may precipitate, which is detrimental to the strength of the matrix. The longer the treatment time of the latter molten salt, the better the softening effect. However, too long a treatment time will bring about problems of increased energy consumption and cost, and efficiency loss. At the same time, there is a risk of precipitation coarsening of vanadium-containing carbides and agglomeration of quasi-spheroidized carbides, which are detrimental to the strength and plasticity of the wire rod. On the contrary, the shorter the treatment time, the poorer the spheroidization and softening effects, the strength of the wire rod increases, and the plasticity decreases. However, if the treatment time is too short, the wire rod is not softened, and may not even be fully transformed into pearlite. The vanadium-containing carbides may not have time to disperse and precipitate in large quantities, and there is a risk of abnormal tissue precipitation, which is detrimental to the regulation of the strength and plasticity of the wire rod. Therefore, the molten salt temperature and treatment time of the latter molten salt can be further regulated to match the strength and plasticity of the wire rod.

[0029] Since the temperature difference between the front-stage molten salt and the rear-stage molten salt is small, the molten salt circulation rate can be appropriately reduced to reduce energy consumption while maintaining processing accuracy. In a preferred embodiment, the molten salt circulation rate of the rear-stage molten salt is 30~80t / h, and the molten salt temperature rise is controlled to be ≤8°C.

[0030] In a preferred embodiment, the roller slow cooling controls the wire rod to be cooled to below 500°C at a cooling rate of 2~5°C / s. The high temperature state of the wire rod after leaving the molten salt can be utilized to avoid the precipitation and coarsening of vanadium-containing carbides at a slightly higher cooling rate, thereby speeding up the production rhythm and avoiding too long online time caused by too low cooling rate. After that, the wire rod is controlled to be cooled at a cooling rate of 0.3~0.7°C / s, and the cooling rate can be further reduced for slow cooling to promote further softening of the wire rod structure until it is coiled.

[0031] In a preferred embodiment, when the roller is slowly cooled, after the wire rod is cooled to below 500°C, the heat preservation cover is closed, and the wire rod's own heat can be used to slowly cool it, and the wire rod is controlled to be cooled at a cooling rate of 2~5°C / s. Then the heat preservation cover is closed to reduce the cooling rate of the wire rod, and the wire rod is controlled to be cooled at a cooling rate of 0.3~0.7°C / s to further soften the wire rod and facilitate rapid coiling at the coiling station.

[0032] Compared with the prior art, the beneficial effects of the present invention are at least:

[0033] (1) In view of the current situation that the material cost is relatively high due to the fact that the addition of more strengthening alloy elements greatly weakens the plasticity and cold working performance of the material, the cold heading steel wire rod of the present invention adopts a high carbon and alum-containing composition design of C-Si-Mn-V, which can effectively reduce the material cost. The microstructure includes most tempered pearlite, a small part of tempered troostite and a small amount of quasi-spheroidized carbides. The solid solution strengthening of carbon and the precipitation strengthening of alum can obtain a higher matrix strength. By regulating the tempering microstructure state, the quasi-spheroidized carbides can be evenly distributed on the plastic matrix, further reducing the microstructure stress and dislocation density, realizing the microstructure regulation and strength-plasticity matching of the wire rod, especially significantly improving the plasticity of the wire rod, achieving a tensile strength of 1320-1370 MPa and a cross-sectional shrinkage of 45%-50%. It can be used to manufacture fasteners such as 15.9-grade bolts without the annealing process, reducing the risk of cracking and improving the yield rate, and has a good market application prospect.

[0034] (2) In view of the limited means of controlling cooling in the production of cold heading steel base materials for fasteners, it is difficult to control the microstructure and performance of hot rolled wire rods or there are many processes. The manufacturing method of the present invention adopts a high C-Si-Mn-V composition design, combined with online salt bath strong tempering and roller slow cooling technology process design. The higher wire drawing temperature can increase the supercooling of the wire rod in the subsequent online salt bath strong tempering treatment and effectively shorten the residence time in the carbon mesh area. The front-stage molten salt is used to control the content of the troostite microstructure of the wire rod matrix. The heated rear-stage molten salt is used to promote the transformation of the untransformed microstructure of the wire rod into the pearlite microstructure, and promote the high-temperature tempering softening and precipitation of vanadium-containing carbides of the wire rod microstructure to ensure the strength and plasticity matching of the wire rod. The microstructure and performance of the hot-rolled cold heading steel wire rod are regulated, and the offline heat treatment process after coiling can be omitted, thereby simplifying the process, improving the manufacturing efficiency and yield rate, and having good industrial adaptability.

[0035] (3) The manufacturing method of the present invention can break the limitation of low-temperature wire laying on low-temperature rolling, select a higher rolling temperature to improve rolling efficiency and reduce the wear of the steel billet on the rolling line. The roller slow cooling can be carried out by first air cooling to slightly increase the cooling speed, and then insulation cooling to reduce the cooling speed, so as to further soften the wire rod and facilitate rapid coiling at the coiling station, which is beneficial to improving manufacturing efficiency and has good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0037] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;

[0038] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;

[0039] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION

[0040] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:

[0041] A preferred embodiment of the manufacturing method of the 15.9 grade annealing-free hot-rolled high-carbon vanadium-containing cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.87%, Si: 0.7%, Mn: 0.5%, V: 0.03%, P: 0.012%, S: 0.012%, and the rest is Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of rolling → spinning → online salt bath strong tempering → roller slow cooling → coiling, specifically:

[0042] The rolling is used to heat steel billets with a specification of 180mm×180mm through a heating furnace to promote uniform composition of the steel billets and avoid the risk of decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billets coming out of the heating furnace are rolled through a rolling line, and are successively subjected to initial rolling, intermediate rolling and heavy-load finishing rolling to be wires with a diameter specification of 8mm. A higher rolling temperature and reduction are used to improve the rolling efficiency, reduce the wear on the rolling line, and refine the grains of the wires. Specifically: the heating furnace temperature is controlled to be 1050°C, the furnace time is 3h, the initial rolling temperature is 1030°C, the initial rolling reduction is 35%, the heavy-load finishing temperature is 960°C, and the finishing reduction is 18%.

[0043] The spinning process is used to convert the wire rods coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers to avoid the precipitation of secondary cementite in the spinning stage, which is beneficial to the formation of a large undercooling degree and sorbite nucleation in the subsequent online salt bath strong tempering. Specifically, the spinning temperature is controlled to be 940°C.

[0044] The online salt bath strong tempering adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, i.e., the front molten salt, and is quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 43°C / s, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, and is cooled to the troostite phase region, and controls part of the austenite structure in the wire rod to be transformed into the troostite structure. The wire rod passing through the front molten salt is then conveyed by a roller to pass through the second salt bath tank, i.e., the rear molten salt, and is heated to the pearlite phase through the rear molten salt. Isothermal treatment is carried out in the zone to promote the transformation of the untransformed austenite structure in the wire rod into the pearlite structure, and at the same time promote the tempering softening of troostite and pearlite, the transformation of carbides to spheroidization and the precipitation of vanadium-containing carbides, reduce the organizational stress and dislocation density. Specifically: the molten salt temperature of the front section molten salt is 520°C, the treatment time is 40s, the molten salt circulation volume is 150t / h, and the molten salt temperature rise is controlled to be ≤12°C; the molten salt temperature of the rear section molten salt is 580°C, the treatment time is 750s, the molten salt circulation volume is 30t / h, and the molten salt temperature rise is controlled to be ≤8°C.

[0045] The roller slow cooling process uses rollers to convey the wire rods coming out of the second salt bath tank for slow cooling treatment, which promotes further softening of the wire rods and facilitates rapid coiling at the coiling station. Specifically, the heat preservation cover is first opened to control the wire rods to cool to 490°C at a cooling rate of 4.2°C / s, and then the heat preservation cover is closed to control the wire rods to cool at a cooling rate of 0.58°C / s until they are coiled. The coiling process is used to coil the wire rods into coils through the coiling drum of the coiling station. The coiling temperature is 290°C. After packaging and storage, the finished cold heading steel wire rods are obtained. The metallographic structure diagram is as shown below. Figure 1 shown.

[0046] Comparative Example 1:

[0047] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of rolling → spinning → Stelmor insulation slow cooling, specifically: controlling the heating furnace temperature to 1030°C, the furnace time to 4h, the initial rolling temperature to 1010°C, the heavy load finishing rolling temperature to 920°C, the spinning temperature to 900°C, the Stelmor insulation slow cooling adopts closing all fans and insulation hoods, and conveying the wire rod with rollers. The wire rod completes phase change in the hood at a cooling rate of 1.2°C / s, and the finished wire rod is obtained after it comes off the line.

[0048] Comparative Example 2:

[0049] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of rolling → spinning → air cooling → insulation and slow cooling, specifically: controlling the heating furnace temperature to 1020°C, the furnace time to 4.5h, the initial rolling temperature to 990°C, the heavy-load finishing rolling temperature to 870°C, the spinning temperature to 850°C, the air cooling adopts opening the insulation cover to cool the wire rod to 695°C at a cooling rate of 2.1°C / s, the insulation and slow cooling adopts closing all fans and insulation covers to complete the phase change of the wire rod in the cover at a cooling rate of 0.9°C / s, and obtaining the finished wire rod after it comes off the line.

[0050] Comparative Example 3:

[0051] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of rolling → spinning → Stelmor rapid cooling → roller slow cooling, specifically: controlling the heating furnace temperature to 1045°C, the furnace time to 3.5h, the initial rolling temperature to 1015°C, the heavy-load finishing rolling temperature to 935°C, the spinning temperature to 910°C, the Stelmor rapid cooling adopts opening 1~6# fans at 40%, so that the wire rod is cooled to 678°C at a cooling rate of 4.3°C / s, the roller slow cooling adopts closing all fans and insulation covers, so that the wire rod completes phase change in the cover at a cooling rate of 1°C / s, and the finished wire rod is obtained after going offline.

[0052] The wire rods obtained in the above-mentioned Example 1 and Comparative Examples 1 to 3 were subjected to organization and performance testing: the tensile test was conducted using "GB-T228.1-2021 Metal Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:

[0053] Table 1. Comparison of wire rod structure and properties by different manufacturing methods

[0054]

[0055] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with the troostite + ferrite structure obtained under low-temperature spinning and insulation cooling, although the strength is higher, serious network carbides are produced, which affects the uniformity of the structure, especially significantly deteriorates the plasticity and toughness properties. The obtained structure has a high dislocation density, which is easy to cause drawing hardening or cold heading cracking. The present invention can effectively shorten the residence time in the network carbon area, avoid the adverse effects of network carbides on high carbon components, and isothermally treat the molten salt in the later stage by heating it to the pearlite phase region to promote the transformation of the untransformed austenite structure in the wire rod into the pearlite structure, while promoting tempering softening and the precipitation of vanadium-containing carbides, which can improve the utilization value of carbon and vanadium, realize the wire rod structure regulation and strength-plasticity matching, especially significantly improve the plasticity of the wire rod.

[0056] From the comparison results of Example 1 and Comparative Example 2, it can be seen that compared with the pearlite + ferrite structure obtained by appropriately increasing the spinning temperature and then air cooling + insulation cooling, there is still serious network carbide, and the strength of the wire rod will be excessively deteriorated. The dislocation density of the obtained structure is relatively high, and the improvement of plasticity is limited. The present invention can obtain a significantly softened matrix structure by regulating the tempering structure state, and significantly improve the plasticity of the wire rod without excessively deteriorating the strength of the wire rod.

[0057] It can be seen from the comparison results of Example 1 and Comparative Example 3 that, compared with the wire rod containing bainite obtained by increasing the air cooling rate, the present invention can avoid the precipitation of abnormal tissues, effectively avoid brittle fracture of coiling, and is more suitable for manufacturing 15.9 grade fasteners when annealing process is omitted, avoiding wire breakage during drawing and cracking during cold heading. Embodiment 2:

[0058] A preferred embodiment of the manufacturing method of the 15.9 grade annealing-free hot-rolled high-carbon vanadium-containing cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.86%, Si: 0.8%, Mn: 0.7%, V: 0.039%, P: 0.015%, S: 0.013%, and the rest are Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of rolling → spinning → online salt bath strong tempering → roller slow cooling → coiling, specifically:

[0059] The rolling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote uniform composition of the steel billet and avoid the risk of decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter specification of 15mm through a rolling line, and is successively subjected to initial rolling, intermediate rolling and heavy-load finishing rolling. A higher rolling temperature and reduction are used to improve the rolling efficiency, reduce the wear on the rolling line, and refine the grains of the wire. Specifically: the heating furnace temperature is controlled to be 1100°C, the furnace time is 5h, the initial rolling temperature is 1080°C, the initial rolling reduction is 28%, the heavy-load finishing temperature is 975°C, and the finishing reduction is 8%.

[0060] The spinning process is used to convert the wire rods coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers to avoid the precipitation of secondary cementite in the spinning stage, which is beneficial to the formation of a large degree of undercooling and sorbite nucleation in the subsequent online salt bath strong tempering. Specifically, the spinning temperature is controlled to be 955°C.

[0061] The online salt bath strong tempering adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, i.e., the front molten salt, and is quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 41°C / s, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, and is cooled to the troostite phase region, and controls part of the austenite structure in the wire rod to be transformed into the troostite structure. The wire rod passing through the front molten salt is then conveyed by a roller to pass through the second salt bath tank, i.e., the rear molten salt, and is heated to the pearlite phase through the rear molten salt. Isothermal treatment is carried out in the zone to promote the transformation of the untransformed austenite structure in the wire rod into the pearlite structure, and at the same time promote the tempering softening of troostite and pearlite, the transformation of carbides to spheroidization and the precipitation of vanadium-containing carbides, reduce the organizational stress and dislocation density. Specifically: the molten salt temperature of the front section molten salt is 542°C, the treatment time is 32s, the molten salt circulation volume is 50t / h, and the molten salt temperature rise is controlled to be ≤12°C; the molten salt temperature of the rear section molten salt is 602°C, the treatment time is 800s, the molten salt circulation volume is 35t / h, and the molten salt temperature rise is controlled to be ≤8°C.

[0062] The roller slow cooling process uses rollers to convey the wire rods coming out of the second salt bath tank for slow cooling treatment, which promotes further softening of the wire rods and facilitates rapid coiling at the coiling station. Specifically: first open the heat preservation cover, control the wire rod to cool to 480°C at a cooling rate of 5°C / s, then close the heat preservation cover, control the wire rod to cool at a cooling rate of 0.45°C / s until coiling; the coiling process is used to coil the wire rod into a coil through the coiling drum of the coiling station, the coiling temperature is 300°C, and after packaging and storage, a cold heading steel wire rod product is obtained, and its metallographic structure diagram is as follows Figure 2 shown.

[0063] Comparative Example 4:

[0064] A method for manufacturing a wire rod, which differs from that of Example 2 in that the heating furnace temperature is controlled to be 1035°C, the furnace time is 5.5h, the initial rolling temperature is 1020°C, the heavy-load finishing rolling temperature is 940°C, the wire-spinning temperature is 920°C, and the wire rod after spinning is subjected to a front-stage molten salt to cool the wire rod at a cooling rate of 36°C / s, and a finished wire rod is obtained after it comes off the line.

[0065] Comparative Example 5:

[0066] A method for manufacturing wire rod, which differs from Example 2 in that the molten salt temperature of the front-stage molten salt is 574°C, the processing time is 20s, and the wire rod after spinning is passed through the front-stage molten salt to cool the wire rod at a cooling rate of 37°C / s, and the finished wire rod is obtained after it comes off the line.

[0067] Comparative Example 6:

[0068] A method for manufacturing wire rod, which differs from Example 2 in that the molten salt temperature of the front-stage molten salt is 500°C, the processing time is 45s, the molten salt circulation volume of the front-stage molten salt is 300t / h, and the molten salt circulation volume of the rear-stage molten salt is 130t / h. The wire rod after spinning passes through the front-stage molten salt, so that the wire rod is cooled at a cooling rate of 45°C / s, and the finished wire rod is obtained after it comes off the line. Embodiment 3:

[0069] A preferred embodiment of the manufacturing method of the 15.9 grade annealing-free hot-rolled high-carbon vanadium-containing cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.88%, Si: 0.82%, Mn: 0.55%, V: 0.046%, P: 0.012%, S: 0.013%, and the rest is Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of rolling → wire laying → online salt bath strong tempering → roller slow cooling → coiling, specifically:

[0070] The rolling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote uniform composition of the steel billet and avoid the risk of decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter specification of 10mm through a rolling line, and is successively subjected to initial rolling, intermediate rolling and heavy-load finishing rolling. A higher rolling temperature and reduction are used to improve the rolling efficiency, reduce the wear on the rolling line, and refine the grains of the wire. Specifically: the heating furnace temperature is controlled to be 1075°C, the furnace time is 4h, the initial rolling temperature is 1050°C, the initial rolling reduction is 32%, the heavy-load finishing temperature is 960°C, and the finishing reduction is 14%.

[0071] The spinning process is used to convert the wire rods coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers to avoid the precipitation of secondary cementite in the spinning stage, which is beneficial to the formation of a large degree of undercooling and sorbite nucleation in the subsequent online salt bath strong tempering. Specifically, the spinning temperature is controlled to be 945°C.

[0072] The online salt bath strong tempering adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, i.e., the front molten salt, and is quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 42°C / s, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, and is cooled to the troostite phase region, and controls part of the austenite structure in the wire rod to be transformed into the troostite structure. The wire rod passing through the front molten salt is then conveyed by a roller to pass through the second salt bath tank, i.e., the rear molten salt, and is heated to the pearlite phase through the rear molten salt. Isothermal treatment is carried out in the zone to promote the transformation of the untransformed austenite structure in the wire rod into the pearlite structure, and at the same time promote the tempering softening of troostite and pearlite, the transformation of carbides to spheroidization and the precipitation of vanadium-containing carbides, reduce the organizational stress and dislocation density. Specifically: the molten salt temperature of the front section molten salt is 527°C, the treatment time is 36s, the molten salt circulation volume is 120t / h, and the molten salt temperature rise is controlled to be ≤12°C; the molten salt temperature of the rear section molten salt is 610°C, the treatment time is 615s, the molten salt circulation volume is 80t / h, and the molten salt temperature rise is controlled to be ≤8°C.

[0073] The roller slow cooling process uses rollers to convey the wire rods coming out of the second salt bath tank for slow cooling treatment, which promotes further softening of the wire rods and facilitates rapid coiling at the coiling station. Specifically: first open the heat preservation cover, control the wire rod to cool to 470°C at a cooling rate of 3.5°C / s, then close the heat preservation cover, control the wire rod to cool at a cooling rate of 0.3°C / s until coiling; the coiling process is used to coil the wire rod into a coil through the coiling drum of the coiling station, the coiling temperature is 295°C, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 3 shown.

[0074] Comparative Example 7:

[0075] A method for manufacturing a wire rod, which differs from Example 3 in that the molten salt temperature of the rear-stage molten salt is 560° C., the processing time is 500 s, and the finished wire rod is obtained after going offline.

[0076] Comparative Example 8:

[0077] A method for manufacturing wire rod, which differs from Example 3 in that the molten salt temperature of the rear-stage molten salt is 560°C, the processing time is 500s, the molten salt circulation rate is 130t / h, and the finished wire rod is obtained after going offline. Embodiment 4:

[0078] A preferred embodiment of the manufacturing method of the 15.9 grade annealing-free hot-rolled high-carbon vanadium-containing cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.9%, Si: 0.75%, Mn: 0.69%, V: 0.05%, P: 0.014%, S: 0.015%, and the rest is Fe and unavoidable impurities. The manufacturing method is manufactured according to the process flow of rolling → spinning → online salt bath strong tempering → roller slow cooling → coiling, specifically:

[0079] The rolling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote uniform composition of the steel billet and avoid the risk of decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter specification of 12mm through a rolling line, and is successively subjected to initial rolling, intermediate rolling and heavy-load finishing rolling. A higher rolling temperature and reduction are used to improve the rolling efficiency, reduce the wear on the rolling line, and refine the grains of the wire. Specifically: the heating furnace temperature is controlled to be 1080°C, the furnace time is 4.5h, the initial rolling temperature is 1060°C, the initial rolling reduction is 30%, the heavy-load finishing temperature is 970°C, and the finishing reduction is 10%.

[0080] The spinning process is used to convert the wire rods coming out of the rolling line into wire rods through a spinning mechanism. The wire rods are spread on the rollers and transported along the rollers to avoid the precipitation of secondary cementite in the spinning stage, which is beneficial to the formation of a large degree of undercooling and sorbite nucleation in the subsequent online salt bath strong tempering. Specifically, the spinning temperature is controlled to be 950°C.

[0081] The online salt bath strong tempering adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, i.e., the front molten salt, and is quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 41°C / s, and quickly passes through the precipitation temperature range of secondary cementite, eliminates the network carbon deterioration phase caused by excessive carbon element, and is cooled to the troostite phase region, and controls part of the austenite structure in the wire rod to be transformed into the troostite structure. The wire rod passing through the front molten salt is then conveyed by a roller to pass through the second salt bath tank, i.e., the rear molten salt, and is heated to the pearlite phase through the rear molten salt. Isothermal treatment is carried out in the zone to promote the transformation of the untransformed austenite structure in the wire rod into the pearlite structure, and at the same time promote the tempering softening of troostite and pearlite, the transformation of carbides to spheroidization and the precipitation of vanadium-containing carbides, reduce the organizational stress and dislocation density. Specifically: the molten salt temperature of the front section molten salt is 550°C, the treatment time is 30s, the molten salt circulation volume is 100t / h, and the molten salt temperature rise is controlled to be ≤12°C; the molten salt temperature of the rear section molten salt is 620°C, the treatment time is 550s, the molten salt circulation volume is 65t / h, and the molten salt temperature rise is controlled to be ≤8°C.

[0082] The roller slow cooling process uses rollers to transport the wire rods coming out of the second salt bath tank for slow cooling treatment, which promotes further softening of the wire rods and facilitates rapid coiling at the coiling station. Specifically: the heat preservation cover is not closed tightly at first, and the wire rod is controlled to be cooled to 465°C at a cooling rate of 2°C / s. Then the heat preservation cover is closed and the wire rod is controlled to be cooled at a cooling rate of 0.7°C / s until it is coiled. The coiling process is used to coil the wire rod into a coil through the coiling drum of the coiling station. The coiling temperature is 285°C. After packaging and storage, the finished cold heading steel wire rod is obtained.

[0083] Comparative Example 9:

[0084] A method for manufacturing wire rod, which differs from Example 4 in that the roller slow cooling process adopts an open heat preservation cover to control the wire rod to be cooled to 285°C at a cooling rate of 3°C / s, and the finished wire rod is obtained after it comes off the line.

[0085] The wire rods obtained in the above-mentioned Examples 2 to 4 and Comparative Examples 4 to 9 were subjected to organizational and performance tests: the tensile test was conducted according to GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method to obtain tensile strength and cross-sectional shrinkage, and the organizational test was conducted according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 2 below:

[0086] Table 2. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods

[0087]

[0088] It can be seen from the results of Examples 1 to 4 that the present invention adopts a high C-Si-Mn-V component design, combined with an online salt bath strong tempering and roller slow cooling technology process design, and the microstructure includes a large part of tempered pearlite, a small part of tempered troostite and a small amount of quasi-spheroidized carbide, achieving a tensile strength of 1320-1370 MPa and a cross-sectional shrinkage of 45%-50%. It can be used to manufacture fasteners such as 15.9 grade bolts without the annealing process, effectively reducing material costs, improving the yield rate, and has good market application prospects.

[0089] From the comparison results of Example 2 and Comparative Example 4, it can be seen that the selection of a higher spinning temperature can avoid the precipitation of secondary cementite in the spinning stage, which is beneficial to the formation of a larger degree of supercooling and troostite nucleation in the subsequent online salt bath strong tempering; from the comparison results of Example 2 and Comparative Example 5, it can be seen that the higher the molten salt temperature and the shorter the treatment time, the coarser the troostite lamellae spacing, the lower the proportion of tempered troostite, the lower the strength of the wire rod and the increase in plasticity, but the molten salt temperature is too high, which is not conducive to the control of network carbides and troostite nucleation; from the comparison results of Example 2 and Comparative Example 6, it can be seen that the lower the molten salt temperature and the longer the treatment time, the finer the tempered troostite lamellae and the higher the proportion, the higher the strength of the wire rod and the decrease in plasticity, and the molten salt temperature and treatment time of the front-stage molten salt can be further regulated to prepare the organization for the rear-stage molten salt treatment.

[0090] From the comparison results of Example 3 and Comparative Example 7, it can be seen that the lower the molten salt temperature of the rear-stage molten salt and the shorter the treatment time, the smaller the spacing between the pearlite lamellae formed, and a finer interphase precipitation is formed, but if the treatment time is too short, the spheroidization and softening effects are poor, the strength of the wire rod increases, and the plasticity decreases; from the comparison results of Example 3 and Comparative Example 8, it can be seen that the higher the molten salt temperature of the rear-stage molten salt and the longer the treatment time, more power can be provided for high-temperature isothermal tempering spheroidization and softening, but if the treatment time is too long, there is a risk of precipitation coarsening of vanadium-containing carbides and agglomeration of quasi-spheroidized carbides, which are not conducive to the strength and plasticity of the wire rod; therefore, the molten salt temperature and treatment time of the rear-stage molten salt can be further adjusted to adjust the strength and plasticity matching of the wire rod.

[0091] From the comparison results of Example 4 and Comparative Example 9, it can be seen that the roller slow cooling uses the heat of the wire rod itself to slowly cool it, and then closing the insulation cover to further reduce the cooling speed of the wire rod, which can promote further softening of the wire rod and facilitate rapid coiling at the coiling station.

[0092] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.86%-0.90%, Si: 0.70%-0.82%, Mn: 0.50%-0.70%, V: 0.03%-0.05%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities. Its microstructure includes a mixed structure consisting of tempered pearlite accounting for 55%-65% by volume, tempered troostite accounting for 34%-40% by volume, and the rest is quasi-spheroidized carbides. Its manufacturing method includes: According to the chemical composition of the 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod, the wire rod is rolled to produce a wire rod. After the wire rod is spun into a wire rod at a spinning temperature of ≥940°C, an online salt bath strong tempering is performed, so that the wire rod is first subjected to a front-stage molten salt treatment, and the wire rod is cooled to the sorbite phase region at a cooling rate of ≥41°C / s, and part of the austenite structure in the wire rod is transformed into the sorbite structure, and then the wire rod is heated to the pearlite phase region through the rear-stage molten salt for isothermal treatment to promote the untransformed wire rod in the wire rod. The austenite structure is transformed into the pearlite structure, while promoting tempering softening and precipitation of vanadium-containing carbides, and finally slowly cooled by rollers to produce a cold heading steel wire rod with a mixed structure consisting of tempered pearlite, tempered troostite and quasi-spheroidized carbides; the molten salt temperature of the front section molten salt is 520-550°C, and the processing time is 30-40s; the molten salt temperature of the rear section molten salt is 580-620°C, and the processing time is 550-800s.

2. The 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 160-200 nm, the interlamellar spacing of the tempered troostite is 70-110 nm, and the network carbide of the cold heading steel wire rod is level 0.

3. The 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod according to claim 1, characterized in that: The cold heading steel wire rod has a diameter of 8.0-15.0 mm, a tensile strength of 1320-1370 MPa, and a cross-sectional shrinkage of 45%-50%.

4. A method for manufacturing a 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod, characterized in that: According to the chemical composition of the 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod as claimed in claim 1, the wire rod is spun into a wire rod at a spinning temperature of ≥940°C, and then subjected to online salt bath strong tempering, so that the wire rod is first subjected to a front-stage molten salt treatment, and the wire rod is cooled to the troostite phase region at a cooling rate of ≥41°C / s, and part of the austenite structure in the wire rod is transformed into the troostite structure, and then the wire rod is heated to the pearlite phase region through the rear-stage molten salt for isothermal treatment, so as to promote the transformation of the untransformed austenite structure in the wire rod into the pearlite structure , while promoting tempering softening and precipitation of vanadium-containing carbides, and finally slowly cooling through a roller to produce a cold heading steel wire rod having a microstructure including 55% to 65% by volume of tempered pearlite, 34% to 40% by volume of tempered troostite, and the rest being a mixed structure of quasi-spheroidized carbides; the molten salt temperature of the front section molten salt is 520 to 550°C, and the processing time is 30 to 40s; the molten salt temperature of the rear section molten salt is 580 to 620°C, and the processing time is 550 to 800s.

5. The method for manufacturing 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod according to claim 4, characterized in that: Before the rolling, the heating furnace temperature is controlled to be 1050-1100° C., and the time in the furnace is 3-5 hours.

6. The method for manufacturing the 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod according to claim 4, characterized in that: During the rolling, the initial rolling temperature is controlled to be 1030-1080° C., the initial rolling reduction is 28%-35%, the heavy-load finishing rolling temperature is ≥960° C., and the finishing rolling reduction is 8%-18%.

7. The method for manufacturing 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod according to claim 4, characterized in that: The molten salt circulation rate of the front-stage molten salt is 50-150 t / h, and the molten salt temperature rise is controlled to be ≤12°C; the molten salt circulation rate of the rear-stage molten salt is 30-80 t / h, and the molten salt temperature rise is controlled to be ≤8°C.

8. The method for manufacturing 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod according to claim 4, characterized in that: The roller slow cooling controls the wire rod to be cooled to below 500°C at a cooling rate of 2-5°C / s, and then controls the wire rod to be cooled at a cooling rate of 0.3-0.7°C / s until it is coiled.

9. The method for manufacturing 15.9 grade annealing-free hot-rolled high carbon vanadium-containing cold heading steel wire rod according to claim 8, characterized in that: When the roller is slowly cooled, after the wire rod is cooled to below 500° C., the heat preservation cover is closed.

Citation Information

Patent Citations

  • A 15.9 grade corrosion-resistant high-strength bolt steel, its production method and heat treatment method thereof.

    CN114058974B

  • Non-quenching and tempering double-phase cold heading steel for high-strength fastener and method for manufacturing same

    CN101220439A

  • Wire rod for high-carbon steel cut wire shot and production method thereof

    CN105002417A

  • Wire rod for high-carbon steel wire and preparation method of wire rod