A tin-silver alloy bump and preparation method thereof
By using electroplating method of components such as thiol-containing compounds, amino acids, nonylphenol polyoxyethylene ether and fluorine-containing surfactant in the electroplating solution, the problem of uncontrollable silver content and high unevenness of Sn-Ag alloy bumps is solved. , realizes high-quality preparation of tin-silver alloy bumps, and improves the coplanarity and packaging reliability of bumps.
Patent Information
- Application Number
- CN202411096821.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-12
AI Technical Summary
When preparing Sn-Ag alloy bumps by the existing electroplating method, the silver content is uncontrollable and the height is uneven, which affects the coplanarity of the bumps and the packaging reliability.
Using electroplating solution containing thiol compounds, amino acids, nonylphenol polyoxyethylene ether and fluorine-containing surfactant, tin silver alloy bumps are prepared through electroplating and reflux processes to improve the uniformity of silver content and the co-blocks. Faceness.
The uniformity and coplanarity of the silver content of the tin-silver alloy bumps are significantly improved, ensuring high quality and packaging reliability of the bumps.
Smart Images

Figure CN118639288B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor integrated circuit packaging, and in particular relates to a tin-silver alloy bump and a preparation method thereof. Background Art
[0002] Bumping technology is to make bumps on the chip pad interface. By making metal bumps on the chip surface, a "point" interface for chip electrical interconnection is provided. It is widely used in advanced packaging such as FC, WLP, CSP, and 3D. Bumps are interconnects with metallic conductive properties that grow directionally on the chip surface and are directly or indirectly connected to the chip pad. The bumping process is between the front-end integrated circuit manufacturing and back-end packaging testing of the industrial chain, and is one of the core technologies of advanced packaging. Bumps are mainly divided into gold, copper, copper-nickel, tin, etc. according to their materials. Bumps of different metal materials are used in different chip product packages. Tin-based bumps have the advantages of easy welding, good wettability, and excellent conductivity, and are widely used. Tin-based bumps mainly include binary and ternary alloy bumps such as Sn-Pb, Sn-Cu, Sn-In, Sn-Ag, and Sn-Ag-Cu. Sn-Ag alloy bumps have the characteristics of good creep resistance, high strength, good thermal fatigue resistance, superior mechanical properties, and high melting point. As a solder, its applicable temperature in wafer-level packaging is slightly higher than the solder used in subsequent packaging, which can effectively avoid the reliability problems caused by repeated reflow to the packaging. Sn-Ag alloy solder is a relatively ideal solder for wafer-level packaging.
[0003] Sn-Ag alloy bumps are generally produced by nail head method, template printing, evaporation / sputtering, and electroplating. Each method has its advantages and disadvantages. The most common method is electroplating, which can be divided into two methods: step-by-step electroplating of Sn and Ag and simultaneous electroplating of Sn-Ag. The electroplating method has a low production cost, and the height and size can be controlled when manufacturing bumps with a diameter of less than 100μm. However, one of the challenges of the electroplating method is how to use the plating solution to achieve electrochemical co-deposition of different metals Sn and Ag, and stably control the Ag content and the uniformity of the height of all bumps on the wafer surface. Summary of the invention
[0004] In view of the problems of poor uniformity in height of Sn-Ag alloy bumps prepared by electroplating method in the above-mentioned prior art and uncontrollable silver content of the bumps, the present invention provides a method for preparing tin-silver alloy bumps.
[0005] To achieve the above purpose, the following technical solutions are specifically included:
[0006] A method for preparing a tin-silver alloy bump comprises the following steps:
[0007] S1: providing a wafer to be electroplated, wherein a metal pad and a metallization layer prepared on the metal pad are present on the chip;
[0008] S2: Cleaning the wafer to be electroplated by gas plasma;
[0009] S3: Placing the wafer in a plating solution for electroplating, and then cleaning and removing the photoresist; the plating solution comprises the following components in mass concentration: 30-150 g / L stannous methanesulfonate, 0.1-5 g / L silver methanesulfonate, 95-400 g / L methanesulfonic acid, 0.1-0.5 g / L antioxidant, 50-150 g / L 1,3-dimethylthiourea, 0.2-5 g / L thiol-containing compound, 0.5-15 g / L amino acid, 5-15 g / L benzaldehyde, 1-3 g / L methacrylic acid, 3-15 g / L nonylphenol polyoxyethylene ether, and 0.15-1.5 g / L fluorinated surfactant;
[0010] The thiol-containing compound is at least one of 5-thiol-3-amino-1,2,4-triazole, 1-(2-dimethylaminoethyl)-5-thioltetrazole, and 3-thiol-4-phenyl-1,2,4-triazole;
[0011] S4: After the reflow process, tin-silver alloy bumps are obtained on the metallization layer of the wafer.
[0012] The invention improves the coplanarity of the tin-silver alloy bumps obtained by electroplating with the electroplating solution and the uniformity of the silver content by cooperating the thiol-containing compound, amino acid, nonylphenol polyoxyethylene ether, fluorine-containing surfactant and other components.
[0013] Preferably, the mass ratio of the thiol-containing compound to the amino acid is 1:(0.5-4).
[0014] More preferably, the mass ratio of the thiol-containing compound to the amino acid is 1:(2-4).
[0015] The 1,3-dimethylthiourea, the thiol-containing compound and the amino acid in the electroplating solution of the present invention can be used as a complexing agent and a stabilizer to complex with silver, thereby shortening the potential difference between tin and silver ions to ensure the completion of co-deposition and maintain the stability of the electroplating solution. The thiol-containing compound can also refine the grains of the electroplated tin-silver alloy, making the tin-silver alloy more dense and uniform.
[0016] Preferably, the amino acid includes at least one of glycine, glutamic acid and leucine.
[0017] Preferably, the fluorine-containing surfactant includes at least one of potassium perfluorooctane sulfonate, potassium perfluorohexane sulfonate and potassium perfluoropropyl sulfonate.
[0018] Preferably, the mass ratio of the nonylphenol polyoxyethylene ether to the fluorinated surfactant is (2-55):1.
[0019] More preferably, the mass ratio of the nonylphenol polyoxyethylene ether to the fluorinated surfactant is (2.7-17):1.
[0020] More preferably, the mass ratio of the nonylphenol polyoxyethylene ether to the fluorinated surfactant is (5-10):1.
[0021] The nonylphenol polyoxyethylene ether and fluorine-containing surfactant in the electroplating solution of the present invention serve as dispersants to disperse the components of the electroplating system, improve the uniformity of the plated alloy Ag of the electroplated alloy layer, make the layer flat and dense, and improve the coplanarity of the bumps.
[0022] Preferably, the antioxidant comprises at least one of catechol and potassium salt of 2,5-dihydroxybenzenesulfonate.
[0023] Preferably, the current density of the electroplating is 1-10 ASD, the time of the electroplating is 30-200 min, and the temperature of the electroplating is 25-35°C.
[0024] Preferably, the temperature of the reflow process is 220-260°C.
[0025] Preferably, in the wafer to be electroplated, the wafer metal pad includes a metallization layer and a photoresist layer on its surface, the photoresist layer has micropores to expose the metallization layer, the diameter of the micropores is 30-120μm, the thickness of the photoresist is 50-150μm, the metallization layer is Ti and Cu thin film layers from bottom to top, and the metallization layer exposed by the micropores also includes a 1-10μm thick Ni metal layer.
[0026] Preferably, the diameter of the micropores is 30-120 μm, the thickness of the photoresist is 50-150 μm, the metallization layers are Ti and Cu thin film layers from bottom to top, and the metallization layer exposed by the micropores also includes a 1-10 μm thick Ni metal layer.
[0027] The electroplating solution solvent of the present invention is water.
[0028] Compared with the prior art, the present invention has the following beneficial effects: the electroplating solution of the present invention contains mercapto compounds, amino acids, nonylphenol polyoxyethylene ether, and fluorine-containing surfactants, which can significantly improve the coplanarity of tin-silver alloy bumps and increase the uniformity of the silver content in the alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The present invention is a flow chart of the method for preparing the tin-silver alloy bump. DETAILED DESCRIPTION
[0030] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below through specific examples. The test methods used in the examples and / or comparative examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial channels unless otherwise specified.
[0031] Example 1
[0032] A method for preparing a tin-silver alloy bump, the flow chart is as shown in the attached Figure 1 As shown, the specific steps include:
[0033] S1: A silicon-based wafer to be electroplated is provided, wherein the metal pad of the wafer chip to be electroplated has been patterned, and a 100nm Ti and a 1-10μm copper film layer have been sputtered in the area to be electroplated as a metallization layer, and photoresist (PR) illumination and development have been performed on the metallization layer to prepare openings with a diameter of 80μm and a depth of 65μm. The spacing between adjacent openings is 150μm, and a 2μm thick Ni barrier layer is electroplated after the photolithography is completed;
[0034] S2: The chip wafer to be electroplated is soaked and rinsed with deionized water for 1 minute, then taken out and blown dry, and then cleaned with nitrogen and oxygen mixed gas plasma, and then electroplated with a platinum-titanium anode and the metal welding plate of the wafer to be electroplated as a cathode. The electroplating current density is 8ASD, the electroplating temperature is 30°C, and the electroplating time is 60 minutes. The electroplating solution consists of the following components: stannous methanesulfonate 80g / L, silver methanesulfonate 1g / L, methanesulfonic acid 150g / L, catechol 0.2g / L, 1,3-dimethylthiourea 100g / L, 5-mercapto-3-amino-1,2,4-triazole 1g / L, glycine 2g / L, benzaldehyde 6g / L, methacrylic acid 1.5g / L, nonylphenol polyoxyethylene ether (10EO) 5g / L, potassium perfluorooctane sulfonate 0.5g / L, and the solvent is deionized water.
[0035] S3: After the electroplating is completed, the photoresist is removed by cleaning and then using a degumming solution to obtain a tin-silver alloy bump;
[0036] S4: A thermal reflow process is then performed at a reflow temperature of 235° C. to obtain tin-silver alloy bumps on the metallization layer of the wafer.
[0037] Example 2-3
[0038] The difference between Example 2-3 and Example 1 is that the types of mercapto compounds contained in the electroplating solution are different, as shown in Table 1 for details.
[0039] Embodiment 4-6
[0040] The difference between Examples 4-6 and Example 1 is that the concentrations of the thiol compound and glycine in the electroplating solution are different, as shown in Table 1 for details.
[0041] Embodiment 7-8
[0042] The difference between Example 7-8 and Example 1 is that the types of amino acids in the electroplating solution are different, as shown in Table 1.
[0043] Examples 9-10
[0044] The difference between Example 9-10 and Example 1 is that the types of fluorinated surfactants in the electroplating solution are different, as shown in Table 1 for details.
[0045] Examples 11-14
[0046] The difference between Examples 11-14 and Example 1 is that the concentrations of the fluorinated surfactant and nonylphenol polyoxyethylene ether in the electroplating solution are different, as shown in Table 1 for details.
[0047] Comparative Example 1
[0048] The difference between this comparative example and Example 1 is that there is no 5-mercapto-3-amino-1,2,4-triazole in the electroplating solution, as shown in Table 1 for details.
[0049] Comparative Example 2
[0050] The difference between this comparative example and Example 1 is that there is no glycine in the electroplating solution, as shown in Table 1 for details.
[0051] Comparative Example 3
[0052] The difference between this comparative example and Example 1 is that there is no nonylphenol polyoxyethylene ether in the electroplating solution, as shown in Table 1 for details.
[0053] Comparative Example 4
[0054] The difference between this comparative example and Example 1 is that there is no potassium perfluorooctane sulfonate in the electroplating solution, as shown in Table 1 for details.
[0055] Comparative Example 5
[0056] The difference between this comparative example and Example 1 is that the electroplating solution does not contain 5-mercapto-3-amino-1,2,4-triazole, glycine, nonylphenol polyoxyethylene ether and potassium perfluorooctane sulfonate, as shown in Table 1 for details.
[0057] WID is used to characterize the coplanarity within the wafer, and AOI (Automated Optical Inspection) is used to test WID. Where WID% = 1 / 2 × [(H 最大高度 -H 最小高度 ) / H 平均高度 ]×100, where H最大高度 is the height of the tallest pillar of the pillar array electroplated on the substrate, measured at the highest part of the pillar; H 最小高度 is the height of the shortest pillar of the pillar array electroplated on the substrate, measured at the highest part of the pillar; H 平均高度 It is the average height of all columns electroplated on the substrate; when WID<15%, it is considered qualified.
[0058] The tin-silver alloy bumps on the chip are divided into 5 areas, and the average silver mass percentage (Agwt.%) in the tin-silver alloy bumps in each area is measured. The silver content in the tin-silver alloy bumps is detected by an element analyzer. The results show that the silver content in the tin-silver alloy bumps is 0.4-3%. Then the standard deviation of the silver content in the tin-silver alloy bumps on the metal solder pad of the overall chip wafer is calculated as the uniformity of the silver content in the tin-silver alloy bumps (%); when the uniformity of the silver content in the tin-silver alloy bumps is ≤10%, it is considered qualified.
[0059] Table 1
[0060]
[0061] It can be seen from Examples 1-14 and Comparative Examples 1-5 that the mercapto compounds, amino acids, nonylphenol polyoxyethylene ethers and fluorine-containing surfactants in the electroplating solution of the present invention can significantly improve the coplanarity of the silver alloy bumps and the uniformity of the silver content in the alloy.
[0062] It can be seen from Examples 1 and 4-6 that as the concentration ratio of the thiol-containing compound to the amino acid increases, the coplanarity of the silver alloy bumps and the uniformity of the silver content are better, and the optimal concentration ratio is 0.75:2.25.
[0063] It can be seen from Examples 1 and 11-14 that the concentration ratio of nonylphenol polyoxyethylene ether and fluorinated surfactant has a complex effect on the coplanarity of the silver alloy bump and the uniformity of the silver content. At a smaller ratio, for example, when the concentration ratio of nonylphenol polyoxyethylene ether and fluorinated surfactant is (2-5):1, the tin-silver alloy bump has better coplanarity and uniformity of the silver content.
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a tin-silver alloy bump, It is characterized in that The steps include: S1: providing a wafer to be electroplated, wherein a metal pad, a metallization layer prepared on the metal pad and a photoresist layer on the surface thereof are present on the chip; S2: Cleaning the wafer to be electroplated by gas plasma; S3: Placing the wafer in a plating solution for electroplating, and then cleaning and removing the photoresist layer; the plating solution comprises the following components in mass concentration: 30-150 g / L stannous methanesulfonate, 0.1-5 g / L silver methanesulfonate, 95-400 g / L methanesulfonic acid, 0.1-0.5 g / L antioxidant, 50-150 g / L 1,3-dimethylthiourea, 0.2-5 g / L thiol-containing compound, 0.5-15 g / L amino acid, 5-15 g / L benzaldehyde, 1-3 g / L methacrylic acid, 3-15 g / L nonylphenol polyoxyethylene ether, and 0.15-1.5 g / L fluorinated surfactant; The thiol-containing compound is at least one of 5-thiol-3-amino-1,2,4-triazole, 1-(2-dimethylaminoethyl)-5-thioltetrazole, and 3-thiol-4-phenyl-1,2,4-triazole; S4: After the reflow process, tin-silver alloy bumps are obtained on the metallization layer of the wafer.
2. The method for preparing the tin-silver alloy bump according to claim 1, It is characterized in that The mass ratio of the thiol-containing compound to the amino acid is 1:(0.5-4).
3. The method for preparing the tin-silver alloy bump according to claim 1, It is characterized in that The amino acid includes at least one of glycine, glutamic acid and leucine.
4. The method for preparing the tin-silver alloy bump according to claim 1, It is characterized in that The fluorine-containing surfactant includes at least one of potassium perfluorooctane sulfonate, potassium perfluorohexane sulfonate and potassium perfluoropropyl sulfonate.
5. The method for preparing the tin-silver alloy bump according to claim 1, It is characterized in that The mass ratio of the nonylphenol polyoxyethylene ether to the fluorine-containing surfactant is (2-55):
1.
6. The method for preparing the tin-silver alloy bump according to claim 5, It is characterized in that The mass ratio of the nonylphenol polyoxyethylene ether to the fluorine-containing surfactant is (2.7-17):
1.
7. The method for preparing the tin-silver alloy bump according to claim 1, It is characterized in that The antioxidant includes at least one of catechol and 2,5-dihydroxybenzenesulfonic acid potassium salt.
8. The method for preparing the tin-silver alloy bump according to claim 1, It is characterized in that The current density of the electroplating is 1-10 ASD, the time of the electroplating is 30-200 min, and the temperature of the electroplating is 25-35° C.
9. The method for preparing the tin-silver alloy bump according to claim 1, It is characterized in that The temperature of the reflow process is 220-260°C; In the wafer to be electroplated, the photoresist layer undergoes a development process to expose micropores in the metallization layer, the diameter of the micropores is 30-120 μm, the thickness of the photoresist layer is 50-150 μm, the metallization layers are Ti and Cu films from bottom to top, and the metallization layer exposed by the micropores also includes a 1-10 μm thick Ni metal layer.
10. A tin-silver alloy bump made by the method for making a tin-silver alloy bump according to any one of claims 1 to 9.
Citation Information
Patent Citations
Plating bath and electroplating method
CN103361685A
Tin-based electroplating solution for solder bumps including perfluoroalkyl surfactant
CN105316711A
Method for ultrasonically electroplating Sn-Ag bumps under high current density
CN116005214A
High-stability Sn-Ag alloy electroplating solution as well as preparation method and application thereof
CN117626367A