A TMs / cBN catalyst and its preparation method and application

By loading double transition metal on hexagonal boron nitride and inducing phase transition under high pressure, TMs/cBN catalyst is formed, which solves the problem that the structural and performance changes of BN catalysts are difficult to regulate under high pressure, and achieves efficient degradation of organic pollutants in water Effect.

CN118649700BActive Publication Date: 2024-11-05HEFEI INSTITUTE OF PHYSICAL SCIENCE CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411112314.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-05
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

As a solid-phase catalyst, the existing BN is a solid-phase catalyst due to uneven distribution of active sites on the surface and high ion leaching rate, which leads to unstable catalytic effect. The phase change under high pressure leads to difficult to regulate the changes in crystal structure and performance, which affects its application effect.

Method used

By loading a double transition metal on hexagonal boron nitride (hBN), it is converted into cubic boron nitride (cBN) by high-pressure induced phase change, forming a TMs/cBN catalyst, improving its conductivity and catalytic activity. The method involves hydrothermal reaction to form a precursor, and then performs a high pressure reaction in a diamond-to-anvil press with a pressure of 10-20 GPa and a temperature of 1300-1800 K, and a double transition metal loaded by boron nitride.

Benefits of technology

The electron transfer efficiency and catalytic activity of the catalyst are improved, the degradation effect on organic pollutants in water is enhanced, and the degradation rate reaches more than 94%, which significantly improves the stability and performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118649700B_ABST
    Figure CN118649700B_ABST
Patent Text Reader

Abstract

The invention discloses a TMs / cBN catalyst and a preparation method and application thereof, belonging to the field of water treatment technology. The TMs / cBN catalyst is constructed by high-pressure induced phase change, comprising the following steps: adding a double transition metal salt solution to a hexagonal boron nitride dispersion, stirring and mixing evenly, and then performing a hydrothermal reaction, and obtaining a precursor powder after centrifugation, washing, and drying; placing the precursor powder in a reaction device for high-pressure reaction for 1-5 hours, wherein the pressure of the high-pressure reaction is 10-20GPa and the temperature is 1300-1800K, and a TMs / cBN catalyst is obtained. The present invention loads double transition metals on hBN, and adopts a high-pressure reaction to make hBN undergo a phase change to form a new phase cBN, and utilizes phase change to regulate the electronic structure, enhance interfacial electron transfer, improve the conductivity and active sites of the catalyst, greatly improve the degradation ability of the catalyst to pollutants, and can effectively degrade organic pollutants in water bodies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of water treatment catalysts, and in particular relates to a TMs / cBN catalyst constructed by high pressure induced phase change, and a preparation method and application thereof. Background Art

[0002] In recent years, due to the widespread use of antibiotics, the water environment has been seriously polluted. People have tried various methods to treat antibiotics in water, including physical adsorption, photocatalysis, electrochemistry and advanced oxidation processes. Among them, advanced oxidation treatment technology, as a highly efficient and promising wastewater treatment technology, can be used to treat a variety of polluted water bodies. Among them, the Fenton-like process, as one of the most promising ways to treat organic wastewater, has been widely studied in recent years. The Fenton-like process is a process that generates oxidative active species such as hydroxyl radicals (·OH), sulfate radicals (·SO4) through the reaction of solid-phase catalysts and peroxides (such as hydrogen peroxide (H2O2), permonosulfate (PMS), peroxydisulfate (PDS), etc.). − ), superoxide radicals (·O2 − ) and singlet oxygen ( 1 O2), thereby achieving the oxidation degradation of pollutants into small molecules and even carbon dioxide, water and inorganic salts, achieving the purpose of sewage treatment. 2+ , Mn 2+ 、Co 2+ 、Ni 2+ Solid phase catalysts such as , can effectively activate peroxides to produce a large number of free radicals and non-free radicals.

[0003] Boron nitride (BN) is a typical two-dimensional material. As a solid-phase catalyst substrate, it has many advantages, such as high chemical and thermal stability, high mechanical strength, excellent thermal conductivity, electrical insulation, large specific surface area and porous structure, and adjustable surface chemical properties. This makes it have broad application prospects in various catalytic reactions. However, BN as a solid-phase catalyst substrate has an uneven distribution of active sites on its surface and a high ion leaching rate, resulting in unstable catalytic effect. At the same time, BN can undergo phase change under high pressure, resulting in significant changes in its crystal structure and performance, which provides a new idea for regulating the performance of solid-phase catalysts based on BN. Summary of the invention

[0004] The purpose of the present invention is to provide a TMs / cBN catalyst constructed by high pressure induced phase change and a preparation method and application thereof, so as to improve the catalytic degradation activity thereof.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] The first object of the present invention is to provide a method for preparing a TMs / cBN catalyst, comprising the following steps:

[0007] S11, precursor preparation: adding a double transition metal salt solution to a hexagonal boron nitride dispersion, stirring and mixing evenly, and then performing a hydrothermal reaction, and obtaining a precursor powder after centrifugation, washing, and drying;

[0008] S12. High-pressure induced phase change to construct TMs / cBN catalyst: The precursor powder is placed in a reaction device for high-pressure reaction for 1-5 hours. The pressure of the high-pressure reaction is 10-20 GPa and the temperature is 1300-1800 K to obtain a TMs / cBN catalyst.

[0009] In the present application, the precursor powder generated by the hydrothermal reaction is hexagonal boron nitride loaded double transition metal powder (abbreviated as TMs / hBN), and then hBN is transformed into cBN under high pressure to generate cubic boron nitride loaded double transition metal (abbreviated as TMs / cBN).

[0010] Centrifugation, washing and drying of the product of the hydrothermal reaction are conventional operations, and specific conditions can be selected according to actual conditions. In this application, washing is performed 3-4 times with water and ethanol respectively; the drying temperature is 60-70°C and the drying time is 10-12 hours.

[0011] In a further embodiment, the double transition metal in the double transition metal salt solution in step S11 is a mixture of two transition metals selected from Ti, V, Cr, Mn, Fe, Co, Ni and Cu, and the molar ratio of the two transition metals is 1:5-0.2.

[0012] In a further embodiment, the metal salt solution in the double transition metal salt solution in step S11 is an aqueous solution of chloride, nitrate or sulfate, and its concentration is 0.01-0.21 mol / L.

[0013] The transition metal salt solution is selected from chlorides, nitrates or sulfates soluble in a solvent, wherein the solvent is water or ethanol, such as titanium nitrate, cobalt nitrate, nickel nitrate, vanadium nitrate, chromium nitrate, iron nitrate, copper nitrate, iron chloride, manganese chloride, copper sulfate, manganese sulfate, ferrous sulfate, etc. The double transition metal salt solution in the present invention is preferably selected from Co(NO3)2, Ni(NO3)2, Fe(NO3)3, Mn(NO3)2, etc.

[0014] In a further embodiment, the hexagonal boron nitride dispersion in step S11 is a dispersion formed by dispersing hexagonal boron nitride in water, and its concentration is 0.1-3 mol / L.

[0015] In a further embodiment, the stirring and mixing time in step S11 is 20-40 minutes, and the temperature of the hydrothermal reaction is 100-200° C. and the time is 10-18 hours.

[0016] In a further embodiment, the reaction equipment in step S12 is a diamond anvil press.

[0017] The diamond anvil cell press (DAC) in the present invention is an existing device, which is the main device for generating static extreme high pressure. It holds the highest record for generating static pressure in the world and can generate pressures ranging from tens of thousands to millions of atmospheres. The present application uses it to subject the precursor hexagonal boron nitride loaded double transition metal powder to high pressure to transform hBN into cBN, generate cubic boron nitride loaded double transition metal, and improve its conductivity and catalytic activity.

[0018] The second object of the present invention is to provide a TMs / cBN catalyst prepared by the above preparation method.

[0019] The third object of the present invention is to provide an application of the above TMs / cBN catalyst for catalytic degradation of organic pollutants in water.

[0020] In a further embodiment, the method for using the TMs / cBN catalyst to catalytically degrade organic pollutants in water comprises the following steps:

[0021] S21, adding TMs / cBN catalyst into sewage and dispersing by ultrasonic;

[0022] S22. Add peroxide to carry out catalytic degradation reaction to remove organic pollutants in sewage.

[0023] In a further embodiment, the concentration of organic pollutants in the sewage is 20-100 mg / L;

[0024] Based on the volume of sewage, the amount of TMs / BN catalyst added is 50-500 mg / L, and the amount of peroxide added is 20-300 mg / L.

[0025] In a further embodiment, the organic pollutants in the sewage include at least one of tetracycline, oxytetracycline hydrochloride, chlortetracycline hydrochloride, doxycycline and their derivatives;

[0026] The peroxide is permonosulfate (PMS), peroxydisulfate (PDS) or hydrogen peroxide (H2O2).

[0027] In a further embodiment, in step S22, the catalytic degradation reaction is carried out under stirring at 300-600 rpm, and the reaction time is 30-90 min.

[0028] Compared with the prior art, the catalyst provided by the present invention has the following significant advantages:

[0029] Hexagonal boron nitride (hBN) has a layered structure similar to graphite, with each layer consisting of a hexagonal lattice formed by BN bonds. The layers interact with each other through weak van der Waals forces and are easily peeled off. It also has a wide band gap (about 5.97 eV) and behaves as an insulator. Due to the wide band gap, the density of states of hBN near the Fermi level is very low, resulting in poor intrinsic electronic conductivity and catalytic activity.

[0030] Under high pressure, hexagonal boron nitride (hBN) transforms into cubic boron nitride (cBN), resulting in significant changes in its crystal structure and properties. Cubic boron nitride (cBN) has a cubic crystal structure similar to diamond, with B and N atoms arranged in sp 3 The hybrid bonds are arranged to form a three-dimensional network structure. Its band gap is narrow (about 1.6 eV), which belongs to a wide bandgap semiconductor, which makes cBN exhibit semiconductor properties under certain conditions. Its state density near the Fermi level is relatively high, which gives it better conductivity and potential catalytic activity.

[0031] BN is an excellent solid-phase catalyst carrier. Its catalytic performance is improved by loading transition metals on hBN. First, loading transition metals can introduce additional electronic states. The d electron bands of these metals interact with the electronic band structure of BN, resulting in an increase in the density of electronic states, especially near the Fermi level. This improves the electron transfer efficiency and promotes the catalytic reaction. Secondly, loading transition metals can regulate the electronic structure of hBN by changing its band gap, so that it exhibits better catalytic performance under specific reaction conditions. At the same time, after BN is loaded with transition metals, new electron transfer channels can be formed, thereby increasing the electron transfer rate.

[0032] The present invention places hexagonal boron nitride loaded with double transition metals (TMs / hBN) in a diamond anvil cell press (DAC) for high-pressure reaction, and utilizes the phase change process of hBN under high-pressure conditions to destroy the original lattice of hBN and transform it into a new phase cBN. Thereby, its atomic arrangement and electronic structure are changed, and its catalytic performance is improved. First, high pressure will cause the hBN lattice to compress, reduce the atomic distance, and this compression will change the degree of overlap of the atomic electron orbits, leading to the rearrangement of the electronic energy level. Secondly, the hBN phase change will induce changes in the electronic structure, and the new crystal structure usually has different electron distribution and energy band structure, thereby changing the electronic properties and catalytic performance of the material. Furthermore, the hBN surface is rich in defects, such as nitrogen vacancies. During the high-pressure induced phase change process, the surface transition metal elements may enter the cBN interface, forming a new bonding mode, providing a new path for interface electron transfer, and improving the electron transfer efficiency. Finally, high pressure can make the transition metal more evenly distributed on the cBN surface, thereby exposing more active sites.

[0033] Therefore, the TMs / cBN catalyst prepared under high pressure in the present invention increases the density of electronic states near the Fermi level of the catalyst by loading transition metals, thereby improving the conductivity and electron transfer ability of cBN. In addition, high pressure is used to induce phase transition, so that the transition metal generates a new coordination binding mode during the hBN phase transition process, thereby enhancing the localized state of electrons.

[0034] In addition, the use of double transition metals in the present application can also utilize synergistic effects to improve the efficiency of electron transfer and greatly enhance the catalytic effect, thereby being able to effectively reduce organic pollutants in water. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The following drawings, which constitute part of the present invention, are used to assist in understanding the present invention. The contents provided in the drawings and their related descriptions in the present invention can be used to explain the present invention, but do not constitute improper limitations on the present invention. In the drawings:

[0036] Figure 1 are scanning electron microscope images of the products, wherein a is a scanning electron microscope image of Co1Ni / BN-15G prepared in Example 1 of the present invention, and b is a scanning electron microscope image of Co1Ni / BN prepared in Comparative Example 1;

[0037] Figure 2 are X-ray diffraction patterns of the products, wherein a is the X-ray diffraction pattern of Co1Ni / BN-15G prepared in Example 1 of the present invention, and b is the X-ray diffraction pattern of Co1Ni / BN prepared in Comparative Example 1;

[0038] Figure 3 The effect diagram of TC degradation by the catalysts prepared in Examples 1-5 of the present invention and Comparative Examples 1-2 is shown. DETAILED DESCRIPTION

[0039] The present invention is further described below in conjunction with specific embodiments, but the essence of the present invention is not limited to the following embodiments. The methods are conventional methods unless otherwise specified, and the materials can be obtained from public commercial channels unless otherwise specified. Those skilled in the art should know that any simple transformation or substitution based on the essence of the present invention belongs to the protection scope claimed by the present invention.

[0040] Example 1

[0041] A method for preparing a TMs / cBN catalyst comprises the following steps:

[0042] (1) Preparation of precursor: 0.006 mol Co(NO3)2 and 0.006 mol Ni(NO3)2 were dissolved in 200 mL of water to obtain solution A, and then 0.01 mol hexagonal boron nitride (hBN) was dispersed in 100 mL of water to obtain dispersion B. Solution A and dispersion B were mixed and stirred for 30 min and then transferred to a reactor for hydrothermal reaction at 200 °C for 18 h. After the reaction was completed, the solid was separated by centrifugation, washed with water and ethanol for 3 times respectively, and dried at 60 °C for 12 h to obtain the precursor powder.

[0043] (2) Construction of Co-Ni / cBN catalyst by high-pressure induced phase transformation: The precursor powder was placed in a diamond anvil press (DAC), a pressure of 15 GPa was applied, and the pressure was maintained at 1800 K for 3 h to obtain the Co-Ni / cBN catalyst, which was denoted as Co1Ni / BN-15G.

[0044] Example 2

[0045] The preparation method is the same as that of Example 1, except that the amount of Co(NO3)2 added is adjusted to 0.003 mol. The prepared catalyst is recorded as Co 0.5 Ni / BN-15G.

[0046] Example 3

[0047] The preparation method of Example 1 was followed, except that the amount of Co(NO3)2 added was adjusted to 0.012 mol, and the prepared catalyst was recorded as Co2Ni / BN-15G.

[0048] Example 4

[0049] The catalyst prepared was prepared according to the preparation method of Example 1, except that the pressure was adjusted to 20 GPa, and was denoted as Co1Ni / BN-20G.

[0050] Example 5

[0051] The catalyst prepared was prepared according to the preparation method of Example 1, except that the pressure was adjusted to 10 GPa, and was denoted as Co1Ni / BN-10G.

[0052] Comparative Example 1

[0053] The CoNi / BN catalyst was synthesized without high pressure treatment, and the steps were as follows:

[0054] 0.006 mol Co(NO3)2 and 0.006 mol Ni(NO3)2 were dissolved in 200 mL of water to obtain solution A. Then 0.01 mol hexagonal boron nitride (hBN) was dispersed in 100 mL of water to obtain dispersion B. Solution A and dispersion B were mixed and stirred for 30 min and then transferred to a reactor for hydrothermal reaction at 200 °C for 18 h. After the reaction was completed, the solid was separated by centrifugation, washed with water and ethanol for 3 times respectively, and dried at 60 °C for 12 h to obtain the catalyst, which was recorded as Co1Ni / BN.

[0055] Comparative Example 2

[0056] The CoNi / BN catalyst was synthesized under low pressure by the following steps:

[0057] (1) Preparation of precursor: 0.006 mol Co(NO3)2 and 0.006 mol Ni(NO3)2 were dissolved in 200 mL of water to obtain solution A. Then 0.01 mol hexagonal boron nitride (hBN) was dispersed in 100 mL of water to obtain dispersion B. Solution A and dispersion B were mixed and stirred for 30 min and then transferred to a reactor for hydrothermal reaction at 200°C for 18 h. After the reaction was completed, the solid was separated by centrifugation, washed with water and ethanol for 3 times respectively, and dried at 60°C for 12 h to obtain the precursor powder.

[0058] (2) Construction of CoNi / BN catalyst by high-pressure induced phase transition: The precursor powder was placed in a diamond anvil press (DAC), a pressure of 5 GPa was applied, and it was maintained at 1800 K for 3 h to obtain the catalyst, which was recorded as Co1Ni / BN-5G.

[0059] Test Example 1

[0060] The catalysts prepared in the above Examples 1-5 or Comparative Examples 1-2 were subjected to relevant performance tests, and the test methods were as follows:

[0061] The morphology of the catalysts was characterized using a FEI-Quanta 200 scanning electron microscope (SEM).

[0062] Use PANalytical X-ray diffractometer to characterize the crystal form and structural characteristics of the material;

[0063] The concentration of antibiotics in the treated water samples was measured using an Agilent 1220 high performance liquid chromatograph.

[0064] The specific test objects and test results are as follows:

[0065] (1) Figure 1 In the figure, a is a scanning electron microscope image of Co1Ni / BN-15G prepared in Example 1 of the present invention, and b is a scanning electron microscope image of Co1Ni / BN prepared in Comparative Example 1.

[0066] from Figure 1 It can be seen that the catalyst of Example 1 treated with high pressure presents a three-dimensional lamellar shape, indicating that the supported substrate is cubic boron nitride (cBN); while the catalyst not treated with high pressure (Comparative Example 1) presents a spherical and blocky disordered morphology, indicating that the supported substrate is hexagonal boron nitride (hBN).

[0067] (2) Figure 2 In the figure, a is the X-ray diffraction pattern of Co1Ni / BN-15G prepared in Example 1, and b is the X-ray diffraction pattern of Co1Ni / BN prepared in Comparative Example 1.

[0068] According to the comparison of PDF standard cards, it can be seen from the XRD spectrum that the diffraction peaks of the Co1Ni / BN-15G prepared in Example 1 appear in the diffraction peaks of the XRD spectrum standard card (PDF#51-0779) of cubic boron nitride (cBN), indicating that the high pressure treatment of Example 1 successfully transforms the hexagonal BN into cubic BN, that is, cubic boron nitride-supported double transition metals are generated. The diffraction peaks of Co1Ni / BN in Comparative Example 1 are consistent with the diffraction peaks of the XRD spectrum standard card (PDF#45-0893) of hexagonal boron nitride (hBN), indicating that the catalyst prepared in Comparative Example 1 is hexagonal boron nitride-supported double transition metals.

[0069] In addition, the same detection shows that the Co1Ni / BN-5G catalyst prepared in Comparative Example 2 has diffraction peaks of both cubic boron nitride and hexagonal boron nitride, indicating that part of the hexagonal BN is converted into cubic BN.

[0070] Test Example 2

[0071] Taking tetracycline (TC) as a pollutant, the degradation effects of the catalysts prepared in Examples 1-5 and Comparative Examples 1-2 on tetracycline (TC) were tested.

[0072] The specific operations are as follows:

[0073] Prepare a TC aqueous solution with a TC concentration of 20 mg / L, denoted as C0; then divide it into seven equal portions, each of 50 mL, as test water samples;

[0074] Weigh 5 mg of Co1Ni / BN-15G and Co0.5 Ni / BN-15G, Co2Ni / BN-15G, Co1Ni / BN-20G, Co1Ni / BN-10G, Co1Ni / BN, and Co1Ni / BN-5G catalysts were added to a test water sample respectively, and the catalyst was fully dispersed by ultrasound to obtain seven treated samples;

[0075] Each treated sample was placed on a stirring table, and 1 mL of a 1000 mg / L monosulfate (PMS) solution was added, stirred at 350 rpm, and the catalytic degradation reaction was carried out at room temperature (the pH of the mixed solution was about 6.4 at this time, and no additional adjustment was required). Water samples were taken at 0, 2, 5, 10, 20, and 30 minutes during the degradation reaction, and the TC concentration in the water samples was detected by Agilent 1220 high performance liquid chromatography, recorded as C.

[0076] The degradation test results of the above treatment samples are as follows: Figure 3 As shown in the figure, the vertical axis C / C0 represents the removal rate of TC. Specifically, when the value of C / C0 is smaller, the removal rate (or degradation rate) of TC is greater; conversely, when the value of C / C0 is larger, the removal rate of TC is smaller.

[0077] from Figure 3 It can be seen that the degradation effect of Co1Ni / BN-20G prepared in Example 4 is the best, with a degradation rate of 94%; while the degradation effect of Co1Ni / BN in Comparative Example 1 is the worst, with a degradation rate of only about 49%; the degradation effect of Co1Ni / BN-5G prepared in Comparative Example 2 is better than that of Comparative Example 1. It shows that high-pressure treatment has a significant effect on the degradation effect of the catalyst, and the greater the pressure of high-pressure treatment, the better the degradation effect. Therefore, the pressure of high-pressure treatment in this application is preferably 10-20 GPa.

[0078] Co1Ni / BN-15G, Co 0.5 The degradation effects of Ni / BN-15G and Co2Ni / BN-15G are basically the same, indicating that simply changing the dosage between the double transition metals has no obvious benefit on the catalytic effect.

[0079] Embodiment 6:

[0080] A method for preparing a TMs / cBN catalyst comprises the following steps:

[0081] (1) Preparation of precursor: 0.004 mol FeCl3 and 0.02 mol MnCl2 were dissolved in 200 mL water to obtain solution A, and then 0.1 mol hexagonal boron nitride (hBN) was dispersed in 100 mL water to obtain dispersion B. Solution A and dispersion B were mixed and stirred for 20 min and then transferred to a reactor for hydrothermal reaction at 100 °C for 10 h. After the reaction was completed, the solid was separated by centrifugation, washed with water and ethanol for 4 times, and dried at 70 °C for 10 h to obtain the precursor powder.

[0082] (2) High-pressure induced phase transformation to construct Co-Ni / cBN catalyst: The precursor powder was placed in a diamond anvil press (DAC), a pressure of 15 GPa was applied, and the pressure was maintained at 1300 K for 5 h to obtain the catalyst, which was recorded as Mn5Fe / BN.

[0083] The Mn5Fe / BN catalyst prepared in this example was tested for removing organic pollutants from sewage as follows:

[0084] Prepare 100 mL of chlortetracycline hydrochloride aqueous solution, wherein the concentration of chlortetracycline hydrochloride is 50 mg / L, add 50 mg of the Mn5Fe / BN catalyst prepared in this example, and disperse it fully by ultrasound; then add 10 mL of peroxydisulfate solution with a concentration of 1000 mg / L; stir at 600 rpm at room temperature, and carry out catalytic degradation reaction for 90 minutes.

[0085] After testing, the degradation rate of chlortetracycline hydrochloride by Mn5Fe / BN prepared in this example reached 89.5%.

[0086] Embodiment 7:

[0087] A method for preparing a TMs / cBN catalyst comprises the following steps:

[0088] (1) Preparation of precursor: 0.035 mol of CuSO4 and 0.007 mol of FeSO4 were dissolved in 200 mL of water to obtain solution A, and then 0.3 mol of hexagonal boron nitride (hBN) was dispersed in 100 mL of water to obtain dispersion B. Solution A and dispersion B were mixed and stirred for 40 min and then transferred to a reactor for hydrothermal reaction at 150 °C for 15 h. After the reaction was completed, the solid was separated by centrifugation, washed with water and ethanol for 3 times respectively, and dried at 65 °C for 12 h to obtain the precursor powder.

[0089] (2) High-pressure induced phase transformation to construct Co-Ni / cBN catalyst: The precursor powder was placed in a diamond anvil press (DAC), a pressure of 20 GPa was applied, and the pressure was maintained at 1500 K for 1 h to obtain the catalyst, which was recorded as Cu5Fe / BN.

[0090] The Mn5Fe / BN catalyst prepared in this example was tested for removing organic pollutants from sewage as follows:

[0091] Prepare 100 mL of oxytetracycline hydrochloride aqueous solution, wherein the concentration of oxytetracycline hydrochloride is 100 mg / L, add 5 mg of the Mn5Fe / BN catalyst prepared in this example, and disperse it fully by ultrasound; then add 1 mL of hydrogen peroxide solution with a concentration of 300 mg / L; stir at 300 rpm at room temperature, and carry out catalytic degradation reaction for 60 min.

[0092] According to the test, the degradation rate of oxytetracycline hydrochloride by Cu5Fe / BN prepared in this embodiment reaches 80%.

[0093] Embodiment 8:

[0094] The same as Example 1, except that the double transition metal solution is vanadium nitrate and chromium nitrate.

[0095] The same test as in Test Example 2 was performed. The catalyst prepared in this example was tested for degradation (30 min) of doxycycline contained in the test water sample, and the degradation rate was 79%.

[0096] Comparative Example 3:

[0097] Same as Example 1, except that the pressure of 15 GPa was applied and then maintained at 1000 K for 3 h.

[0098] The same test as in Experimental Example 2 shows that the degradation rate of tetracycline by the catalyst prepared in this comparative example is only 66%, indicating that the temperature of the high-pressure reaction is 1300-1800 K. A lower temperature is not conducive to the transformation of hexagonal BN to cubic BN, thereby affecting its degradation effect on organic pollutants.

[0099] Comparative Example 4:

[0100] Same as Example 1, except that 0.012 mol Co(NO3)2 was dissolved in 200 mL water to obtain solution A.

[0101] The same test as in Experimental Example 2 showed that the degradation rate of tetracycline by the catalyst prepared in this embodiment was 70%. This indicates that the degradation effect of the single metal-loaded catalyst on organic pollutants is poor, and further proves that the double transition metal-loaded catalyst used in this application has a synergistic effect, greatly enhancing its catalytic effect, thereby being able to efficiently reduce organic pollutants in water.

[0102] Finally, it should be noted that the above embodiments are only preferred implementations of the present invention and are only used to explain the present invention, not to limit the present invention. For those skilled in the art, they can still modify the technical solutions recorded in the above embodiments, or replace some of the technical features therein with equivalents. Any changes, replacements and modifications made within the spirit and principles of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a TMs / cBN catalyst, characterized in that: The following steps are involved: S11, precursor preparation: adding a double transition metal salt solution to a hexagonal boron nitride dispersion, stirring and mixing evenly, and then performing a hydrothermal reaction, and obtaining a precursor powder after centrifugation, washing, and drying; S12. High-pressure induced phase change to construct TMs / cBN catalyst: The precursor powder is placed in a reaction device for high-pressure reaction for 1-5 hours. The pressure of the high-pressure reaction is 10-20 GPa and the temperature is 1300-1800 K to obtain a TMs / cBN catalyst.

2. The preparation method according to claim 1, characterized in that: In step S11, the double transition metal in the double transition metal salt solution is a mixture of two transition metals selected from Ti, V, Cr, Mn, Fe, Co, Ni and Cu, and the molar ratio of the two transition metals is 1:5-0.

2.

3. The preparation method according to claim 1, characterized in that: The metal salt solution in the double transition metal salt solution in step S11 is a chloride, nitrate or sulfate solution, and its concentration is 0.01-0.21 mol / L.

4. The preparation method according to claim 1, characterized in that: The hexagonal boron nitride dispersion in step S11 is a dispersion formed by dispersing hexagonal boron nitride in water, and its concentration is 0.1-3 mol / L.

5. The preparation method according to claim 1, characterized in that: The stirring and mixing time in step S11 is 20-40 minutes, and the temperature of the hydrothermal reaction is 100-200° C. and the time is 10-18 hours.

6. The preparation method according to claim 1, characterized in that: The reaction equipment in step S12 is a diamond anvil press.

7. A TMs / cBN catalyst prepared by the preparation method according to any one of claims 1 to 6.

8. The use of the TMs / BN catalyst as claimed in claim 7, characterized in that: It is used to catalyze the degradation of organic pollutants in water.

9. The use according to claim 8, characterized in that: The method for using the TMs / cBN catalyst to catalytically degrade organic pollutants in water comprises the following steps: S21, adding TMs / cBN catalyst into sewage and dispersing by ultrasonic; S22. Add peroxide to carry out catalytic degradation reaction to remove organic pollutants in sewage.

10. The use according to claim 9, characterized in that: The concentration of organic pollutants in the sewage is 20-100 mg / L; Based on the volume of sewage, the amount of TMs / cBN catalyst added is 50-500 mg / L, and the amount of peroxide added is 20-300 mg / L.

11. The use according to claim 9, characterized in that: The organic pollutants in the sewage include at least one of tetracycline, oxytetracycline hydrochloride, chlortetracycline hydrochloride, doxycycline and their derivatives; The peroxide is peroxymonosulfate, peroxydisulfate or hydrogen peroxide.

12. The use according to claim 9, characterized in that: In step S22, the catalytic degradation reaction is carried out under stirring at 300-600 rpm, and the reaction time is 30-90 min.