A biaxially oriented polypropylene matte film and its preparation method and application
The matt layer and the homopolymerized polypropylene intermediate layer are composed of high-density polyethylene, random copolymerized polypropylene and ethylene-5-norbornene-2-acetate block copolymer in a biaxially oriented polypropylene matt film. , solves the problems of longitudinal lines, wrinkles and insufficient surface tension, improves stiffness and tension durability, avoids corona treatment again, and is suitable for high-speed automated production and ultra-thin film applications.
Patent Information
- Application Number
- CN202411131890.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-19
AI Technical Summary
Existing biaxially oriented polypropylene matt films are prone to vertical lines and wrinkles during production and application, and have insufficient surface tension retention, resulting in the need for corona treatment again. They are unable to adapt to high-speed automated production, especially with regard to film thickness. Unwinding the roll is difficult in smaller cases.
It uses a matting layer composed of high-density polyethylene, random copolymerized polypropylene and ethylene-5-norbornene-2-acetate block copolymer, combined with an intermediate layer of homopolymerized polypropylene, and improves the performance by designing the molecular chain structure. Durable stiffness and surface tension, avoids corona treatment again, suitable for ultra-thin matting films.
It improves the flatness and surface tension durability of the film roll, ensures the adhesion between the functional coating layer and the matting layer, and is suitable for high-speed automated production, especially for ultra-thin film applications.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of matt films, in particular to a biaxially oriented polypropylene matt film and a preparation method and application thereof. Background Art
[0002] Biaxially oriented polypropylene (BOPP) matte film is usually a BOPP film with matte on one side and glossy on the other side or matte on both sides. It mainly achieves the matte effect by scattering light, which can improve the grade of printed outer packaging. Since the matte film can give people a soft, fashionable and elegant high-end feeling and eliminate eye fatigue, BOPP matte film is increasingly used in the packaging field, especially suitable for deep processing industries and fields such as coating and lamination.
[0003] The BOPP matte film currently used for functional coating still has the following shortcomings: First, the substrate stiffness is not enough, which leads to the problem of film flatness such as longitudinal lines and wrinkles on the film roll during the production and downstream application of BOPP matte film. The longitudinal lines and wrinkles will affect the quality of the film surface after functional coating; second, the surface tension retention of the matte layer used for functional coating is not enough, which leads to the need for corona treatment on the surface of the matte layer before functional coating (for example: functional coating to form an anti-scratch layer). However, the re-corona treatment can only be used for thicker matte films. This method is prone to problems such as difficulty in winding and unwinding and wrinkling of the film roll when used for thin matt films (usually below 20μm), and cannot meet the requirements of high-speed automated production. Summary of the invention
[0004] Based on this, the object of the present invention is to provide a biaxially oriented polypropylene matte film and a preparation method and application thereof. The biaxially oriented polypropylene matte film has the advantages of high stiffness and lasting surface tension. On the one hand, it can improve the problem of film roll flatness such as longitudinal lines and wrinkles in the film roll during production and downstream applications. On the other hand, it can be used for functional coating without further corona treatment and ensure the adhesion between the formed functional coating layer and the upper surface layer (i.e., the matte layer).
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A biaxially stretched polypropylene matte film comprises an upper surface layer, an intermediate layer and a lower surface layer which are arranged in sequence; the upper surface layer is a matte layer, comprising 40-50wt% of high-density polyethylene, 42-47wt% of random copolymerized polypropylene and 3-8wt% of ethylene-5-norbornene-2-acetate block copolymer; the intermediate layer is a stiffness control layer, comprising homopolypropylene; the molecular chain of the homopolypropylene is formed by connecting a first segment component with a melting temperature T1∈[136, 175]°C and a second segment component with a melting temperature T2∈(175, 180]°C; the second segment component accounts for 5-15wt% of the homopolypropylene.
[0007] The biaxially oriented polypropylene matte film of the present invention improves the properties of the biaxially oriented polypropylene matte film, such as stiffness and surface tension durability, by designing the components of the upper surface layer and the middle layer. On the one hand, the problem of film roll flatness caused by longitudinal lines and wrinkles in the film roll during production and downstream application can be improved. On the other hand, the adhesion between the functional coating layer formed during functional coating and the upper surface layer (matte layer) can be ensured without the need for further corona treatment.
[0008] The biaxially oriented polypropylene matte film of the present invention adopts 40-50wt% of high-density polyethylene, 42-47wt% of random copolymerized polypropylene and 3-8wt% of ethylene-5-norbornene-2-acetate block copolymer in the upper surface layer, i.e., the matte layer, so that the upper surface layer of the biaxially oriented polypropylene matte film has the properties of uniform matte, lasting surface tension and high stiffness, and improves the problem of film roll flatness of the biaxially oriented polypropylene matte film, which is prone to longitudinal lines and wrinkles in the film roll during production and downstream application, and can ensure the adhesion between the functional layer formed during functional coating and the upper surface layer (matte layer) without the need for further corona treatment.
[0009] Wherein, the ethylene-5-norbornene-2-acetate block copolymer is a block copolymer with ethylene and 5-norbornene-2-acetate as synthetic monomers, including a relatively soft polyethylene part and a relatively hard 5-norbornene-2-acetate part. The ethylene-5-norbornene-2-acetate block copolymer is synthesized by gradient copolymerization using metallocene catalysis, and has a wide molecular weight distribution (PDI is 1.3-1.6). The ethylene-5-norbornene-2-acetate block copolymer is a crystalline copolymer. Due to the presence of a low content of norbornene molecular chains in the ethylene-5-norbornene-2-acetate block copolymer, the relatively soft polyethylene part exhibits crystallinity, so that the ethylene-5-norbornene-2-acetate block copolymer has a certain degree of crystallinity. On the one hand, the crystalline part (polyethylene part) in the ethylene-5-norbornene-2-acetate block copolymer cooperates with the rigid ring structure in the ethylene-5-norbornene-2-acetate block copolymer, which is beneficial to improving the stiffness of the matte layer without affecting the matte effect, and cooperates with the intermediate layer to jointly improve the overall stiffness of the film; on the other hand, the polar ester group in the ethylene-5-norbornene-2-acetate block copolymer is beneficial to the high surface tension after corona treatment, and the rigid ring structure in the ethylene-5-norbornene-2-acetate block copolymer is beneficial to slowing down the surface tension decay speed and improving the durability of the surface tension of the matte layer after corona treatment. The two functions work together to improve the problem of failure due to severe surface tension decay, and the adhesion between the functional coating layer and the upper surface layer (matte layer) of the film in subsequent functional coating applications can be guaranteed without corona treatment again, which is particularly suitable for the coating of ultra-thin matte films.
[0010] The biaxially oriented polypropylene matte film of the present invention, the homopolypropylene used in the intermediate layer, its molecular chain is formed by connecting a first segment component with a melting temperature of T1∈[136, 175]°C and a second segment component with a melting temperature of T2∈(175, 180]°C; the second segment component accounts for 5-15wt% of the homopolypropylene. The homopolypropylene is a semi-crystalline polymer, and the chain structure and lamella size in the molecule are distributed to a certain extent. The molecular chain of the homopolypropylene is analyzed by a continuous self-nucleation annealing method and a thermal classification method. In the process of melting at elevated temperature and crystallization at reduced temperature, two melting peaks of different sizes will appear on the melting curve of homopolymer polypropylene after the final crystallization is complete. The higher the melting temperature, the thicker the crystal. The two melting peaks are composed of the first segment component with low melting point and thin crystal thickness (melting temperature T1 is 136-175℃, including 175℃; that is, melting temperature T1∈[136,175]℃) and the second segment component with high melting point and thick crystal thickness (melting temperature T2 is 175-180℃, excluding 175℃; that is, melting temperature T2∈(17 5, 180] ℃). The present invention adopts the homopolymer polypropylene formed by connecting the first segment component with melting temperature T1∈[136, 175] ℃ and the second segment component with melting temperature T2∈(175, 180] ℃ in the molecular chain to improve the stiffness of the intermediate layer, and cooperates with the component design of the upper surface layer to jointly improve the stiffness of the biaxially oriented polypropylene matte film. The second segment component accounts for 5-15wt% of the homopolymer polypropylene, that is, the second segment component with high melting point and thick lamella thickness (melting temperature T2∈(175 When the proportion of the second segment component with a melting temperature T2∈(175, 180]℃ is less than 5wt%, it is not conducive to improving the stiffness of the film, resulting in the overall softness of the film. When the proportion of the second segment component with a melting temperature of 175-180℃ is greater than 15wt%, the film is too stiff and not conducive to large-ratio biaxial stretching, and the film is easily broken. The present invention is beneficial to improving the smoothness of film production by controlling the proportion of the second segment component with a melting temperature T2∈(175, 180]℃ in the homopolymer polypropylene molecular chain.
[0011] Furthermore, in the upper surface layer, the melt index of the high-density polyethylene is 10-20 g / 10 min (melt index test conditions: 190°C, 21.6 kg), and the melt index of the copolymerized polypropylene is 7-10 g / 10 min (melt index test conditions: 230°C, 2.16 kg), which is conducive to obtaining a good matte effect. The copolymerized polypropylene is one or both of ethylene-propylene copolymer and ethylene-propylene-butene copolymer.
[0012] Furthermore, the content of 5-norbornene-2-acetate in the ethylene-5-norbornene-2-acetate block copolymer is 10-15 mol%. By limiting the content of 5-norbornene-2-acetate in the ethylene-5-norbornene-2-acetate block copolymer, the ethylene-5-norbornene-2-acetate block copolymer has moderate steric hindrance, ensuring suitable melt fluidity, ensuring the smoothness of biaxial stretching production, ensuring the matt uniformity, surface tension and durability of the matt layer, and improving the bonding force between the matt layer and the functional coating layer; if the content of 5-norbornene-2-acetate in the ethylene-5-norbornene-2-acetate block copolymer is less than 10 mol%, It is not conducive to further improving the adhesion between the matt layer and the functional coating layer; if the 5-norbornene-2-acetate content in the ethylene-5-norbornene-2-acetate block copolymer is greater than 15 mol%, then due to the high content of polar groups and cyclic structures, on the one hand, due to the excessive hydrogen bonding force between the molecular chains, the matt layer will be too brittle, which is not conducive to biaxial stretching, and cracks will be generated during production, which is not conducive to ensuring the bonding force between the matt layer and the intermediate layer. On the other hand, it will cause the surface adhesion of the matt layer after corona treatment to be too strong, which is not conducive to the smoothness of winding and unwinding during production and use.
[0013] Furthermore, the crystallinity of the ethylene-5-norbornene-2-acetate block copolymer is 10-25%. Limiting the crystallinity of the ethylene-5-norbornene-2-acetate block copolymer to 10-25% is conducive to improving the stiffness of the matt layer while ensuring the matt effect of the matt layer; if the crystallinity of the ethylene-5-norbornene-2-acetate block copolymer is too low, on the one hand, it is not conducive to improving the stiffness of the matt layer, and on the other hand, the macromolecular chain of the ethylene-5-norbornene-2-acetate block copolymer is too rigid, which will greatly reduce the toughness of the matt layer and is not conducive to biaxial stretching film forming; if the crystallinity of the ethylene-5-norbornene-2-acetate block copolymer is too high, it may have an adverse effect on the matt effect of the matt layer (it may affect the crystallization of high-density polyethylene, thereby affecting the formation of the "sea island structure" and affecting the final matt effect), and due to the high crystallinity, the cyclic structure and ester group content in the molecular chain of the ethylene-5-norbornene-2-acetate block copolymer are too low, which will lead to difficulty in stretching and easy film breakage.
[0014] Furthermore, the melting point of the ethylene-5-norbornene-2-acetate block copolymer is 108-120° C., and the number average molecular weight of the ethylene-5-norbornene-2-acetate block copolymer is (2.5-5)×10 4Controlling the melting point and number average molecular weight of the ethylene-5-norbornene-2-acetate block copolymer within the above range is beneficial to matching the fluidity of the matte layer melt, facilitating the biaxial stretching process and ensuring the matte effect.
[0015] Furthermore, the middle layer also includes 1-5wt% of antistatic masterbatch; by adding 1-5wt% of antistatic masterbatch into the middle layer, the antistatic performance of the biaxially oriented polypropylene matte film is improved.
[0016] Furthermore, the crystallinity of the first segment component is 40-50%; the crystallinity of the second segment component is 5-10%. By limiting the crystallinity of the first segment component with low melting point and thin lamella thickness (melting temperature T1∈[136, 175]℃) to 40-50%, and the crystallinity of the second segment component with high melting point and thick lamella thickness (melting temperature T2∈(175, 180]℃) to 5-10%, the Young's modulus (longitudinal direction) of the homopolymer polypropylene after stretching is 3000-4000MPa, so that the homopolymer polypropylene has both stiffness and flexibility, which is beneficial to the overall stiffness of the film and the smoothness of production. If the crystallinity of the second segment component with a high melting point and thick lamellar thickness (melting temperature T2∈(175, 180]℃) is less than 5%, it is not conducive to improving the stiffness of the film, resulting in the overall softness of the film (the Young's modulus (longitudinal) of the film after stretching is 1000-2000MPa). If the crystallinity of the second segment component with a high melting point and thick lamellar thickness (melting temperature T2∈(175, 180]℃) is greater than 10%, the film will be too stiff and not conducive to large-ratio biaxial stretching, and the film will easily break.
[0017] Furthermore, the crystallinity of the homopolypropylene is 45-55%. When the crystallinity of the homopolypropylene is controlled to be 45-55%, the stiffness of the obtained biaxially oriented polypropylene matte film is optimal. When the overall crystallinity of the homopolypropylene is lower than 45%, the film is too soft and cannot provide the stiffness and flatness required for coating, and is not conducive to winding; when the overall crystallinity of the homopolypropylene is higher than 55%, the film is easily broken and the thickness uniformity is affected during the production process, which is not conducive to the smoothness of production and affects the production efficiency of the product.
[0018] Furthermore, the total thickness of the biaxially oriented polypropylene matte film is 12-18 μm, and the thickness of the upper surface layer is 1.5-2.0 μm. The biaxially oriented polypropylene matte film of the present invention is suitable for the above-mentioned thinner matte film (usually below 20 μm), has the advantages of durable surface tension and high stiffness, and can ensure the adhesion between the functional coating layer and the matte layer of the film in subsequent functional coating applications without the need for further corona treatment, and is particularly suitable for ultra-thin matte films.
[0019] Furthermore, the biaxially oriented polypropylene matte film of the present invention further comprises a compatibilizing layer, which is disposed between the upper surface layer and the middle layer; the compatibilizing layer comprises homopolypropylene, 1-2wt% maleic anhydride grafted polypropylene and 2-4wt% propylene-norbornene copolymer. The provision of the compatibilizing layer improves the bonding strength between the upper surface layer and the middle layer.
[0020] Furthermore, in the compatibilization layer, the melt index of the homopolypropylene is 2.5-3.5 g / 10min (measurement conditions: 230°C, 2.16 KG); the grafting rate of maleic anhydride in the maleic anhydride grafted polypropylene is 0.5-1wt%; the melt index of the propylene-norbornene copolymer is 1-4 g / 10min (measurement conditions: 230°C, 2.16 KG). By providing a compatibilization layer, it is beneficial to further ensure the bonding force between the upper surface layer and the middle layer, and it is less likely to be delaminated during production and use. Preferably, the thickness of the compatibilization layer is 1-2μm.
[0021] As a preferred solution of this embodiment, the lower surface layer is a bright layer, including homopolypropylene and 1-5wt% anti-adhesion masterbatch. By setting the lower surface layer as a bright layer and adding the anti-adhesion masterbatch in the bright layer, it is beneficial to improve the smoothness of the winding and unwinding of the biaxially oriented polypropylene matte film during production and use. Preferably, the homopolypropylene is isotactic polypropylene with an isotacticity of 95-97% and a melt index of 2.5-3.5g / 10min (measurement conditions: 230°C, 2.16KG). In other solutions, those skilled in the art can specifically choose to set the lower surface layer according to actual needs, for example, the lower surface layer can also be set as a matte layer.
[0022] The present invention also provides a method for preparing any of the above-mentioned biaxially oriented polypropylene matte films, comprising the following steps:
[0023] Step 1: Batching and plasticization: The proportion of each layer of raw materials is set in the control system of the biaxial stretch film production line, and then the batching system will automatically transport the dried raw materials of each layer to the corresponding extruders according to the input ratio. After melting and plasticizing in the extruders of each layer, the melt enters the die head through the runner and distributor;
[0024] Step 2: Slice casting: After being extruded through the die, the melt immediately contacts the cooling roller to form a thick sheet;
[0025] Step 3: Longitudinal stretching: The thick sheet is heated to the set temperature by multiple sets of preheating rollers, and then longitudinal stretching is started, and then shaping is performed;
[0026] Step 4: Horizontal stretching: After preheating the thick sheet after longitudinal stretching to the set temperature, start horizontal stretching, and then perform shaping and cooling treatment after horizontal stretching;
[0027] Step 5: Traction and rewinding: The multi-layer film from the horizontal pulling unit enters the traction unit, and after thickness measurement and corona treatment, enters the rewinding unit to obtain a parent roll;
[0028] Step 6: Slitting: Slitting the aged mother roll to obtain film rolls of specified width and length.
[0029] Furthermore, in the above process, the melt extrusion temperature of the matte layer is 200-260°C; the melt extrusion temperature of the middle layer and the lower surface layer is 230-260°C; in the process of the melt contacting the cooling roller, the temperature of the chilling water and the chilling roller is 15-50°C; the temperature of the longitudinal stretching zone is 90-130°C; the temperature of the transverse stretching zone is 155-165°C; the longitudinal stretching ratio is 4.5-5.5 times; the transverse stretching ratio is 8-10 times; the corona power factor of the matte layer is 20-25W·min / m. Preferably, when the biaxially oriented polypropylene matte film includes the compatibilizing layer, the above preparation method is adopted; in its process, the melt extrusion temperature of the compatibilizing layer is 230-260°C.
[0030] The present invention also provides an application of any of the above-mentioned biaxially oriented polypropylene matte films in functional coating, wherein the film is coated on the surface of the upper surface layer to form a matte film product with a functional coating layer. The biaxially oriented polypropylene matte film of the present invention can be directly coated on the surface of the upper surface layer to form a functional coating layer without further corona treatment, and the formed functional coating layer has strong adhesion to the upper surface layer.
[0031] Compared with existing technology:
[0032] The biaxially oriented polypropylene matte film of the present invention has a long-lasting surface tension and high stiffness. By optimizing the material composition of the middle layer and the matte layer, the matte layer has improved surface tension, stiffness and other properties such as stiffness, which meets the coating process and can adapt to high-speed automated production. DETAILED DESCRIPTION
[0033] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein.
[0034] In the following examples or comparative examples:
[0035] The melting point was tested by DSC instrument under the conditions of 10K / min heating and cooling speed and 50mL / min N2 filling rate. The temperature was raised from 20℃ to 200℃, then kept at 200℃ for 2min, then cooled from 200℃ to 20℃, then kept at 20℃ for 2min, and finally raised from 20℃ to 200℃.
[0036] The content of the segment components was determined using the SSA heat treatment procedure in the DSC instrument. In a high-purity nitrogen atmosphere, the sample was heated from 30°C to 200°C at a rate of 20°C / min to eliminate the thermal history. After that, the sample was melt-crystallized continuously at the selected temperature with a temperature gradient of 4°C. Finally, it was heated to 200°C at a rate of 10°C / min to obtain the SSA melting curve after the final crystallization was perfected.
[0037] The melt index (melt mass flow rate MFR) is determined according to GB / T3682-2018.
[0038] In the following examples or comparative examples, the melt index of high-density polyethylene is 10 g / 10 min (190° C., 21.6 KG), and the melt index of random copolymer polypropylene is 7.5 g / 10 min (230° C., 2.16 KG).
[0039] Example 1
[0040] This embodiment provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0041] Among them, the formula of each layer is as follows:
[0042] Matt layer: 40wt% high-density polyethylene, 57wt% random copolymer polypropylene and 3wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 10mol%, crystallinity is 25%, melting point is 108℃, molecular weight is 2.5×10 4 );
[0043] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 52%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 5wt%, and the crystallinity is 5%; the first segment component content with melting temperature T1∈[136,175]℃ is 95wt%, and the crystallinity is 50%) and 1wt% antistatic masterbatch;
[0044] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0045] The total thickness of the biaxially oriented polypropylene matte film of this embodiment is 15 μm, the thickness of the upper surface layer is 1.8 μm, and the thickness of the lower surface layer is 1.0 μm.
[0046] This embodiment also provides a method for preparing a biaxially oriented polypropylene matte film, comprising the following steps:
[0047] Step 1: Batching and plasticization: The proportion of each layer of raw materials is set in the control system of the biaxial stretch film production line, and then the batching system will automatically transport the dried raw materials of each layer to the corresponding extruders according to the input ratio. After melting and plasticizing in the extruders of each layer, the melt enters the die head through the runner and distributor;
[0048] Step 2: Slice casting: After being extruded through the die, the melt immediately contacts the cooling roller to form a thick sheet;
[0049] Step 3: Longitudinal stretching: The thick sheet is heated to the set temperature by multiple sets of preheating rollers, and then longitudinal stretching is started, and then shaping is performed;
[0050] Step 4: Horizontal stretching: After preheating the thick sheet after longitudinal stretching to the set temperature, start horizontal stretching, and then perform shaping and cooling treatment after horizontal stretching;
[0051] Step 5: Traction and rewinding: The multi-layer film from the horizontal pulling unit enters the traction unit, and after thickness measurement and corona treatment, enters the rewinding unit to obtain a parent roll;
[0052] Step 6: Slitting: Slitting the aged mother roll to obtain film rolls of specified width and length.
[0053] In the above process, the melt extrusion temperature of the matte layer is 235°C; the melt extrusion temperature of the middle layer and the lower surface layer is 250°C; in the process of the melt contacting the cooling roller, the temperature of the chilled water and the chilled roller is 40°C; the temperature of the longitudinal stretching zone is 125°C; the temperature of the transverse stretching zone is 160°C; the longitudinal stretching ratio is 5.3 times; the transverse stretching ratio is 8.5 times; the corona power factor of the matte layer is 23.5W•min / m.
[0054] Example 2
[0055] This embodiment provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0056] Among them, the formula of each layer is as follows:
[0057] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 12mol%, crystallinity is 15%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0058] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 45%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, crystallinity is 8%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, crystallinity is 45%) and 1wt% antistatic masterbatch;
[0059] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0060] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this embodiment are the same as those of embodiment 1.
[0061] The preparation method of the biaxially oriented polypropylene matte film of this embodiment is the same as that of embodiment 1.
[0062] Example 3
[0063] This embodiment provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0064] Among them, the formula of each layer is as follows:
[0065] Matt layer: 50wt% high-density polyethylene, 42wt% random copolymer polypropylene and 8wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 15mol%, crystallinity is 10%, melting point is 120℃, molecular weight is 5.0×10 4 );
[0066] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 55%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 15wt%, and the crystallinity is 10%; the first segment component content with melting temperature T1∈[136,175]℃ is 85wt%, and the crystallinity is 50%) and 1wt% antistatic masterbatch;
[0067] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0068] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this embodiment are the same as those of embodiment 1.
[0069] The preparation method of the biaxially oriented polypropylene matte film of this embodiment is the same as that of embodiment 1.
[0070] Example 4
[0071] This embodiment provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), a compatibilization layer, an intermediate layer and a lower surface layer which are arranged in sequence.
[0072] Among them, the formula of each layer is as follows:
[0073] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 12mol%, crystallinity is 15%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0074] Compatibilization layer: 96wt% homopolymer polypropylene (melt index is 3.0g / 10min, melt index test conditions: 230℃, 2.16KG), 2wt% maleic anhydride grafted polypropylene (maleic anhydride grafting rate is 0.5wt%), 2wt% propylene-norbornene copolymer (melt index: 2g / 10min, melt index measurement conditions: 230℃, 2.16KG);
[0075] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 53%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, and the crystallinity is 8%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, and the crystallinity is 50%) and 1wt% antistatic masterbatch;
[0076] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0077] The total thickness of the biaxially oriented polypropylene matte film of this embodiment is 16.2 μm, the thickness of the upper surface layer is 1.8 μm, the thickness of the lower surface layer is 1.0 μm, and the thickness of the volume-increasing layer is 1.2 μm.
[0078] The preparation method of the biaxially oriented polypropylene matte film of this embodiment is the same as that of Embodiment 1, wherein: the melt extrusion temperature of the compatibilization layer is 250°C.
[0079] Example 5
[0080] The present embodiment provides an application of a biaxially oriented polypropylene matte film in a functional coating. Specifically, a scratch-resistant coating is applied to the upper surface layer (matte layer) of the biaxially oriented polypropylene matte film of Embodiments 1 to 4, respectively, and a matte film product with a functional coating layer (i.e., an anti-scratch layer) is formed after molded with a plate film (24 μm thick corona-free matte film) and UV cured.
[0081] A functional coating layer was formed on the surface of the biaxially oriented polypropylene matte film of Example 1-4, and the adhesion between the functional coating layer and the upper surface layer (matte layer) was evaluated. Please refer to Table 1 for the results.
[0082] Comparative Example 1
[0083] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0084] Among them, the formula of each layer is as follows:
[0085] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 12mol%, crystallinity is 15%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0086] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 52%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 1wt%, and the crystallinity is 5%; the first segment component content with melting temperature T1∈[136,175]℃ is 99wt%, and the crystallinity is 50%) and 1wt% antistatic masterbatch;
[0087] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0088] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0089] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0090] Comparative Example 2
[0091] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0092] Among them, the formula of each layer is as follows:
[0093] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 12mol%, crystallinity is 15%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0094] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 52%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 30wt%, crystallinity is 5%; the first segment component content with melting temperature T1∈[136,175]℃ is 70wt%, crystallinity is 50%) and 1wt% antistatic masterbatch;
[0095] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0096] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0097] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0098] Comparative Example 3
[0099] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0100] Among them, the formula of each layer is as follows:
[0101] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 12mol%, crystallinity is 15%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0102] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 40%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, and the crystallinity is 1%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, and the crystallinity is 50%) and 1wt% antistatic masterbatch;
[0103] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0104] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0105] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0106] Comparative Example 4
[0107] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0108] Among them, the formula of each layer is as follows:
[0109] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 12mol%, crystallinity is 15%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0110] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 55%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, and the crystallinity is 30%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, and the crystallinity is 50%) and 1wt% antistatic masterbatch;
[0111] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0112] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0113] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0114] Comparative Example 5
[0115] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0116] Among them, the formula of each layer is as follows:
[0117] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-norbornene copolymer (norbornene content is 12mol%, molecular weight is 3.5×10 4 );
[0118] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 45%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, crystallinity is 8%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, crystallinity is 45%) and 1wt% antistatic masterbatch;
[0119] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0120] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0121] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0122] Comparative Example 6
[0123] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0124] Among them, the formula of each layer is as follows:
[0125] Matt layer: 50wt% high-density polyethylene and 50wt% random copolymer polypropylene;
[0126] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 45%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, crystallinity is 8%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, crystallinity is 45%) and 1wt% antistatic masterbatch;
[0127] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0128] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0129] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0130] Comparative Example 7
[0131] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0132] Among them, the formula of each layer is as follows:
[0133] Matt layer: 40wt% high-density polyethylene, 45wt% random copolymer polypropylene and 15wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 12mol%, crystallinity is 15%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0134] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 45%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, crystallinity is 8%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, crystallinity is 45%) and 1wt% antistatic masterbatch;
[0135] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0136] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0137] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0138] Comparative Example 8
[0139] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0140] Among them, the formula of each layer is as follows:
[0141] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 30mol%, crystallinity is 15%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0142] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 45%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, crystallinity is 8%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, crystallinity is 45%) and 1wt% antistatic masterbatch;
[0143] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0144] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0145] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0146] Comparative Example 9
[0147] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0148] Among them, the formula of each layer is as follows:
[0149] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 3mol%, crystallinity is 15%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0150] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 45%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, crystallinity is 8%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, crystallinity is 45%) and 1wt% antistatic masterbatch;
[0151] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0152] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0153] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0154] Comparative Example 10
[0155] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0156] Among them, the formula of each layer is as follows:
[0157] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 12mol%, crystallinity is 40%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0158] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 45%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, crystallinity is 8%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, crystallinity is 45%) and 1wt% antistatic masterbatch;
[0159] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0160] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0161] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0162] Comparative Example 11
[0163] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0164] Among them, the formula of each layer is as follows:
[0165] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (non-crystalline) (5-norbornene-2-acetate content is 12mol%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0166] Middle layer: 99wt% homopolypropylene (melt index is 2.5g / 10min, melt index test conditions: 230℃, 2.16KG, crystallinity is 45%; homopolypropylene is 100%, of which the second segment component content with melting temperature T2∈(175,180]℃ is 10wt%, crystallinity is 8%; the first segment component content with melting temperature T1∈[136,175]℃ is 90wt%, crystallinity is 45%) and 1wt% antistatic masterbatch;
[0167] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0168] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0169] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0170] Comparative Example 12
[0171] This comparative example provides a biaxially oriented polypropylene matte film, comprising an upper surface layer (matte layer), an intermediate layer and a lower surface layer which are arranged in sequence.
[0172] Among them, the formula of each layer is as follows:
[0173] Matt layer: 47wt% high-density polyethylene, 47wt% random copolymer polypropylene and 6wt% ethylene-5-norbornene-2-acetate block copolymer (5-norbornene-2-acetate content is 12mol%, crystallinity is 15%, melting point is 113℃, molecular weight is 3.5×10 4 );
[0174] Middle layer: 9.9wt% homopolypropylene (melting temperature T2∈(175, 180]℃, crystallinity 8%), 89.1wt% homopolypropylene (melting temperature T1∈[136, 175]℃, crystallinity 45%) and 1wt% antistatic masterbatch;
[0175] Lower surface layer: 97wt% homopolymer polypropylene (isotacticity is 96%, melt index is 3.0 g / 10min, melt index test conditions: 230°C, 2.16 KG) and 3wt% anti-blocking masterbatch.
[0176] The total thickness and thickness of each layer of the biaxially oriented polypropylene matte film of this comparative example are the same as those of Example 1.
[0177] The preparation method of the biaxially oriented polypropylene matte film of this comparative example is the same as that of Example 1.
[0178] Comparative Example 13
[0179] The present comparative example provides an application of a biaxially oriented polypropylene matte film in a functional coating. Specifically, a scratch-resistant coating is applied to the upper surface layer (matte layer) of the biaxially oriented polypropylene matte film of comparative examples 1 to 12, respectively, and a matte film product with a functional coating layer (i.e., an anti-scratch layer) is formed after plate film (24 μm thick corona-free matte film) molding and UV curing.
[0180] A functional coating layer is formed on the surface of the biaxially stretched polypropylene matte film of Comparative Examples 1-12. A functional coating layer is formed on the surface of the biaxially stretched polypropylene matte film of Comparative Examples 1-12. The adhesion between the functional coating layer and the upper surface layer (matte layer) is evaluated. Please refer to Table 1 for the results.
[0181] Performance Testing
[0182] The following performance tests were performed on the biaxially oriented polypropylene matte films of Examples 1-4 and Comparative Examples 1-12 respectively:
[0183] Matting effect:
[0184] ① Glossiness: According to GB / T8807-88, tested at a 45° angle.
[0185] ② Haze: Tested according to GB / T2410-2008.
[0186] Surface tension and durability:
[0187] ① Surface tension: tested according to GB / T2913.
[0188] ② Durability: Test the surface tension of the film after aging treatment for 0 days, 30 days, 60 days and 90 days.
[0189] Stiffness:
[0190] ① Young's modulus: tested according to GB / T1040.1-2018.
[0191] Production smoothness (qualitative): whether there is stratification, film breaking, and smoothness of winding and unwinding.
[0192] Evaluation of adhesion between functional coating layer and upper surface layer (matt layer):
[0193] Use 3M 610 tape with a length of about 7.5 cm to stick it on the functional coating layer (the film sample size is 50*50 cm and has been aged for 90 days), then press evenly with a force of about 3 kg, press back and forth six times, quickly pull the tape at a 60-degree angle, and observe the coating shedding. No shedding or slight shedding (shedding area ≤5%) is qualified.
[0194] The performance test results of the biaxially oriented polypropylene matte films of Examples 1-4 and Comparative Examples 1-12 are shown in Table 1:
[0195] Table 1 Performance test results of biaxially oriented polypropylene matte films of Examples 1-4 and Comparative Examples 1-12
[0196]
[0197] The biaxially oriented polypropylene matte films of Examples 1-4 of the present invention have good matte effect, high surface tension, good durability, and high stiffness. They are not easy to delaminate or break during the production process, and the film can be smoothly rolled up and unrolled. After the functional coating is applied, the functional coating layer has strong adhesion to the upper surface layer (matt layer), and the functional coating layer is not easy to fall off.
[0198] In the biaxially oriented polypropylene matte film of Comparative Example 1, in the homopolymerized polypropylene segment of the middle layer, the content of the second segment component with a melting temperature T2∈(175, 180]°C is too low, the Young's modulus is low, the film stiffness is too low, and the film is overall soft.
[0199] In the biaxially oriented polypropylene matte film of Comparative Example 2, in the homopolymerized polypropylene segment of the middle layer, the content of the second segment component with a melting temperature T2∈(175, 180]°C is too high, the Young's modulus is high, and the film stiffness is too high, which is not conducive to biaxial stretching during the production process and increases film breakage.
[0200] In the biaxially oriented polypropylene matte film of Comparative Example 3, in the homopolymerized polypropylene segment of the middle layer, the second segment component with a melting temperature T2∈(175, 180]°C has low crystallinity, low Young's modulus, low film stiffness, and the film is overall soft.
[0201] In the biaxially oriented polypropylene matte film of Comparative Example 4, in the homopolymerized polypropylene segment of the middle layer, the crystallinity of the second segment component with a melting temperature T2∈(175, 180]°C is too high; the Young's modulus is high, and the film stiffness is too high, which is not conducive to biaxial stretching during the production process, and the film breakage increases.
[0202] The biaxially oriented polypropylene matte film of Comparative Example 5 uses ethylene-norbornene copolymer in the upper surface layer (matt layer) instead of the ethylene-5-norbornene-2-acetate block copolymer of the present invention. The film of Comparative Example 5 has a low initial surface tension, which decreases to 39 dyn / cm after 90 days, and cannot effectively guarantee the adhesion between the upper surface layer (matt layer) and the functional coating layer in subsequent applications of the film. In the evaluation of the adhesion between the functional coating layer and the upper surface layer (matt layer), the coating (referring to the functional coating layer) falls off, and the falling area is 8%.
[0203] The biaxially oriented polypropylene matte film of Comparative Example 6 contains only high-density polyethylene and random copolymerized polypropylene in the upper surface layer (matt layer), and no ethylene-5-norbornene-2-acetate block copolymer is added to the upper surface layer (matt layer). The Young's modulus of the film of Comparative Example 6 is lower than that of the embodiment, and the initial surface tension of the film is low, and it decreases to 38 dyn / cm after 90 days. It is also impossible to effectively guarantee the adhesion between the upper surface layer (matt layer) and the functional coating layer of the film in subsequent applications. In the evaluation of the adhesion between the functional coating layer and the upper surface layer (matt layer), the coating (referring to the functional coating layer) has fallen off, and the falling off area is 10%.
[0204] In the biaxially oriented polypropylene matte film of Comparative Example 7, the content of ethylene-5-norbornene-2-acetate block copolymer in the upper surface layer (matt layer) is too high, and the overall matte effect of the film is poor; the surface tension of the film is too high, and the surface adhesion is too strong, which is not conducive to the smoothness of winding and unwinding during production and use; the bonding force between the upper surface layer (matt layer) and the middle layer is poor, and it is easy to delaminate; the Young's modulus is relatively high, the matt layer is brittle, which is not conducive to biaxial stretching, and cracks will occur during production.
[0205] In the biaxially oriented polypropylene matte film of Comparative Example 8, the content of 5-norbornene-2-acetate in the ethylene-5-norbornene-2-acetate block copolymer used in the upper surface layer (matt layer) is too high. Since the content of polar groups (ester groups) and rigid cyclic structures (norbornene) in the upper surface layer (matt layer) is too high, on the one hand, the hydrogen bonding force between the molecular chains is too large, which will cause the matt layer to be too brittle, which is not conducive to biaxial stretching, and cracks will be generated during production. It is also not conducive to ensuring the bonding force between the matt layer and the middle layer, and it is easy to delaminate; on the other hand, the surface tension of the matt layer after corona treatment is too high, and the adhesion is too strong, which is not conducive to the smoothness of winding and unwinding during production and use. On the other hand, the overall matt effect of the film is deteriorated.
[0206] In the biaxially oriented polypropylene matte film of Comparative Example 9, the content of 5-norbornene-2-acetate in the ethylene-5-norbornene-2-acetate block copolymer used in the upper surface layer (matt layer) is too low, and the initial surface tension of the film is low, and it decreases to 38 dyn / cm after 90 days, which is not conducive to improving the bonding strength between the upper surface layer (matt layer) and the functional coating layer in subsequent applications. In the evaluation of the adhesion between the functional coating layer and the upper surface layer (matt layer), the coating (referring to the functional coating layer) has fallen off, and the falling off area is 10%.
[0207] In the biaxially oriented polypropylene matte film of Comparative Example 10, the ethylene-5-norbornene-2-acetate block copolymer used in the upper surface layer (matt layer) has a high crystallinity, which has an adverse effect on the matt effect of the matt layer. In addition, it is difficult to stretch the film during the production process, and the film is easily broken, resulting in an increase in film breakage.
[0208] In the biaxially oriented polypropylene matte film of Comparative Example 11, the ethylene-5-norbornene-2-acetate block copolymer used in the upper surface layer (matt layer) is non-crystalline and has a low Young's modulus, which is not conducive to improving the stiffness of the matt layer.
[0209] The biaxially oriented polypropylene matte film of Comparative Example 12 is a mixture of two homopolypropylenes, i.e., a mixture of a homopolypropylene having a melting temperature T2∈(175, 180]°C and a homopolypropylene having a melting temperature T1∈[136, 175]°C, rather than the homopolypropylene of the present invention formed by connecting two segment components having different melting temperatures on the same molecular chain (i.e., the molecular chain of the homopolypropylene of the present invention is formed by connecting a first segment component having a melting temperature T1∈[136, 175]°C and a second segment component having a melting temperature T2∈(175, 180]°C). The film of Comparative Example 12 has impurities, which affects the application of the film.
[0210] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and the present invention is also intended to include these modifications and modifications.
Claims
1. A biaxially oriented polypropylene matte film, Features: The invention comprises an upper surface layer, an intermediate layer and a lower surface layer which are arranged in sequence; the upper surface layer is a matte layer, comprising 40-50wt% of high-density polyethylene, 42-57wt% of random copolymerized polypropylene and 3-8wt% of ethylene-5-norbornene-2-acetate block copolymer; the content of 5-norbornene-2-acetate in the ethylene-5-norbornene-2-acetate block copolymer is 10-15mol%; the crystallinity of the ethylene-5-norbornene-2-acetate block copolymer is 10-25%; the intermediate layer is a stiffness control layer, comprising homopolymerized polypropylene; the molecular chain of the homopolymerized polypropylene in the intermediate layer is composed of a melting temperature T 1 ∈[136, 175]℃ first segment components and melting temperature T 2 The second segment component is connected with the homopolypropylene at ∈(175, 180]℃; the second segment component accounts for 5-15wt% of the homopolypropylene; the crystallinity of the second segment component is 5-10%.
2. The biaxially oriented polypropylene matte film according to claim 1, Features: The melting point of the ethylene-5-norbornene-2-acetate block copolymer is 108-120° C., and the number average molecular weight of the ethylene-5-norbornene-2-acetate block copolymer is (2.5-5)×10 4 .
3. The biaxially oriented polypropylene matte film according to claim 1, Features: The middle layer also includes 1-5wt% antistatic masterbatch.
4. The biaxially oriented polypropylene matte film according to claim 1, Features: The crystallinity of the first segment component is 40-50%; the crystallinity of the homopolypropylene in the middle layer is 45-55%.
5. The biaxially oriented polypropylene matte film according to claim 1, Features: The total thickness of the biaxially oriented polypropylene matte film is 12-18 μm, and the thickness of the upper surface layer is 1.5-2.0 μm.
6. The biaxially oriented polypropylene matte film according to claim 1, Features: It also includes a compatibilization layer, which is arranged between the upper surface layer and the middle layer; the compatibilization layer includes homopolypropylene, 1-2wt% maleic anhydride grafted polypropylene and 2-4wt% propylene-norbornene copolymer; the homopolypropylene of the compatibilization layer has a melting index of 2.5-3.5 g / 10min under the measuring conditions of 230°C and 2.16KG; the grafting rate of maleic anhydride in the maleic anhydride grafted polypropylene is 0.5-1wt%; the melting index of the propylene-norbornene copolymer under the measuring conditions of 230°C and 2.16 KG is 1-4 g / 10min.
7. A method for preparing the biaxially oriented polypropylene matte film according to any one of claims 1 to 6, Features: The following steps are involved: Step 1: Batching and plasticization: The proportion of each layer of raw materials is set in the control system of the biaxial stretch film production line, and then the batching system will automatically transport the dried raw materials of each layer to the corresponding extruders according to the input ratio. After melting and plasticizing in the extruders of each layer, the melt enters the die head through the runner and distributor; Step 2: Slice casting: After being extruded through the die, the melt immediately contacts the cooling roller to form a thick sheet; Step 3: Longitudinal stretching: The thick sheet is heated to the set temperature by multiple sets of preheating rollers, and then longitudinal stretching is started, and then shaping is performed; Step 4: Horizontal stretching: After preheating the thick sheet after longitudinal stretching to the set temperature, start horizontal stretching, and then perform shaping and cooling treatment after horizontal stretching; Step 5: Traction and rewinding: The multi-layer film from the horizontal pulling unit enters the traction unit, and after thickness measurement and corona treatment, enters the rewinding unit to obtain a parent roll; Step 6: Slitting: Slitting the aged mother roll to obtain film rolls of specified width and length.
8. Use of the biaxially oriented polypropylene matte film according to any one of claims 1 to 6 in functional coating, Features: The surface of the upper surface layer is coated to form a matte film product with a functional coating layer.