A film-coated slow-release fertilizer based on protein capsule film

By coating urea particles with protein capsule membrane and forming modified polyurethane materials, the mechanical properties and environmental pollution problems of gelatin and polyurethane materials are solved, and a coating sustained-release fertilizer with excellent hydrophobicity and mechanical properties is prepared, reducing environmental pollution and Improves the efficiency of nitrogen utilization.

CN118652146BActive Publication Date: 2024-11-05YANTAI ZHONGDE GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411123912.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-05
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

In the prior art, gelatin, as a wrapping material, has poor mechanical properties and poor hydrophobicity, and the difficulty in degrading of polyurethane materials, resulting in environmental pollution, making it difficult to prepare a coated sustained release fertilizer with strong mechanical properties and hydrophobicity and environmental protection.

Method used

The protein capsule film is used to coat urea particles, and the modified polyurethane material is formed through two coating processes, and the hydrophobicity and mechanical properties are improved by using dihydroxy-terminated fluorinated chain extender, modified polyol solids and isophorone diisocyanate. , reduce the amount of polyurethane and reduce environmental pollution.

Benefits of technology

The prepared slow-release fertilizer has good hydrophobicity, mechanical properties and thermodynamic properties, extends the material life cycle, reduces environmental pollution, and improves nitrogen nutrient utilization efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a coated slow-release fertilizer based on a protein capsule film, belongs to the technical field of fertilizers, and is used to solve the technical problems in the prior art that gelatin as a coating material has poor mechanical properties and poor hydrophobicity, and polyurethane as a coating material is difficult to degrade. The invention comprises the following steps: adding molten protein capsule film to urea particles to obtain a first film layer, dripping a dihydroxyl-terminated fluorinated chain extender solution, a modified polyol solid and isophorone diisocyanate into the first film layer to obtain a second film layer, and modifying gelatin with citric acid, trace metal elements and quaternary ammonium salt methyltrialkylammonium chloride to enrich the nutritional elements of the protein capsule film and improve the slow-release performance, and using a polyfluorinated chain extender and a modified polyol solid with multiple functional groups and multiple cross-linking sites to improve the hydrophobicity and mechanical properties of a prepared polyurethane film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fertilizers, and in particular to a film-coated slow-release fertilizer based on a protein capsule film. Background Art

[0002] Slow-release fertilizers can be divided into coated slow-release fertilizers, encapsulated slow-release fertilizers and other categories. Among them, coated slow-release fertilizers are those in which one or more layers of thin film are sprayed on the surface of fertilizer particles to form a dense low-permeability membrane, which can control the rate at which water enters the fertilizer core and the rate at which nutrient solution diffuses from the inside of the membrane to the outside, thereby slowing down the release rate of nutrients in the fertilizer. Polyurethane, as a functional polymer material, has a strong modifiability due to the diversity of monomer types required for its polymerization and the flexibility of the synthesis process. Therefore, it can be used in the fertilizer field. However, as a difficult-to-degrade material, polyurethane is prone to cause environmental pollution.

[0003] The patent application with publication number CN103387452A discloses a method for preparing a slow-release fertilizer. Formaldehyde is added to a gelatin solution as a cross-linking agent, and then ferrous sulfate and a chelating agent are added to prepare a composite colloidal solution containing chelated iron salts. The colloidal solution is then coated on the surface of urea particles to obtain a coating layer containing urea-complexed iron salts. However, compared with polyurethane materials, gelatin has technical defects such as poor mechanical properties and poor hydrophobicity, which affect the slow-release effect and stability of the coated slow-release fertilizer.

[0004] Patent application with publication number CN100475750C discloses a composite coated slow-release fertilizer, wherein the film layer includes a high-barrier organic film layer, a thermosetting polymer and a sulfur-containing thermosetting polymer. The thermosetting polymer may be a polyurethane epoxy resin, etc. The release period of the slow-release fertilizer is increased by multi-layer coating. However, each film layer of the above-mentioned prior art is a difficult-to-degrade material and is highly polluting to the soil environment.

[0005] Therefore, how to prepare a film-coated slow-release fertilizer with strong mechanical properties and hydrophobicity and little environmental pollution is a technical problem that needs to be solved urgently. Summary of the invention

[0006] The purpose of the present invention is to provide a coated slow-release fertilizer based on a protein capsule membrane, which is used to solve the technical problems in the prior art that gelatin as a coating material has poor mechanical properties and poor hydrophobicity, and polyurethane as a coating material is difficult to degrade.

[0007] The object of the present invention can be achieved by the following technical scheme: a film-coated slow-release fertilizer based on a protein capsule film, comprising urea particles, wherein the urea particles are sequentially coated with a first film layer and a second film layer from the inside to the outside;

[0008] The preparation method of the first film layer is:

[0009] 10-20 g of protein capsule membrane is melted to obtain a melted protein capsule membrane; 500 g of urea granules are placed in a drum granulator, preheated at 50-60° C. for 10 min, and the melted protein capsule membrane is added to the urea granules, and stirred evenly to obtain a first film layer;

[0010] The preparation method of the second film layer is:

[0011] Add 5g of dihydroxy-terminated fluorinated chain extender solution, 5g of modified polyol solid and 10-20g of isophorone diisocyanate to the protein capsule film, mix, stir and react; the above adding process is carried out twice to obtain the second film layer.

[0012] Urea is coated with a protein capsule film and a polyurethane emulsion in sequence to obtain secondary coated urea, and the secondary coated urea is vacuum dried to obtain a coated slow-release fertilizer based on the protein capsule film, wherein a modified polyol solid, a dihydroxy-terminated fluorinated chain extender solution and isophorone diisocyanate react on the surface of the urea after the primary coating to obtain a secondary coating film, thereby preparing a coated slow-release fertilizer based on the protein capsule film.

[0013] Furthermore, the method for preparing the protein capsule membrane comprises the following steps:

[0014] A1, citric acid, gelatin and deionized water are mixed, and the mixture is swollen at 50°C for 3-5 hours with mechanical stirring; and then the mixture is statically swollen at 80°C for 1-2 hours to obtain hydrolyzed gelatin;

[0015] After gelatin is hydrolyzed with citric acid, hydrolyzed gelatin can be obtained;

[0016] A2, copper sulfate pentahydrate, manganese sulfate monohydrate and deionized water are mixed and stirred to obtain a mixed metal solution;

[0017] A3, mixing hydrolyzed gelatin, citric acid and deionized water, reacting at 80-90°C for 2-3h to obtain a reactant; adding a mixed metal solution to the reactant, reacting at 50-60°C for 30min, then heating to 110-120°C, reacting until all the deionized water solvent is completely evaporated, to obtain a metal salt composite gelatin;

[0018] The amino functional groups in the hydrolyzed gelatin can react with the carboxyl groups of citric acid, and the excess hydroxyl and carboxyl functional groups in the hydrolyzed gelatin and the excess hydroxyl and carboxyl functional groups in the citric acid can adsorb metal ions, thereby preparing a metal salt composite gelatin modified with citric acid that adsorbs metal salts;

[0019] A4, metal salt composite gelatin and deionized water are mixed evenly, and stirred at 50-60°C for 40-50 minutes; then methyl trialkyl ammonium chloride is added, and mixed and reacted at 60°C for 40-50 minutes to obtain a product; the product is allowed to stand at room temperature for 2-4 hours, and then vacuum dried at 60-70°C for 1-2 hours to obtain a protein capsule membrane;

[0020] Furthermore, in step A1, the dosage ratio of citric acid, gelatin and deionized water is 1-5g:30g:200mL, and the speed of mechanical stirring is 100r / min; in step A2, the dosage ratio of copper sulfate pentahydrate, manganese sulfate monohydrate and deionized water is 1-5g:1-5g:50mL; the mixing and stirring temperature is 60-70°C, and the mixing and stirring time is 30min.

[0021] Furthermore, in step A3, the dosage ratio of hydrolyzed gelatin, citric acid and deionized water is 50-60g:20-30mL:200mL, and the dosage of mixed metal liquid is 50mL; in step A4, the dosage ratio of metal salt composite gelatin, deionized water and methyltrialkylammonium chloride is 50g:50mL:10-20g.

[0022] Further, the dihydroxy-terminated fluorinated chain extender solution is prepared by the following steps:

[0023] 3-Mercapto-1,2-propanediol, N-ethyl perfluorooctane sulfonamidoethyl acrylate and benzoyl peroxide are mixed and reacted at 100-110° C. for 3-5 hours to obtain a mixture; the mixture is heated to 120-130° C. and reacted until the 3-mercapto-1,2-propanediol solvent is completely evaporated to obtain a dihydroxy-terminated fluorinated chain extender solution.

[0024] The mercapto group of mercapto-1,2-propylene glycol reacts with the double bond of N-ethyl perfluorooctane sulfonamidoethyl acrylate to generate mercaptoimine, thereby obtaining a dihydroxy-terminated fluorinated chain extender. In the above-mentioned free radical addition reaction, benzoyl peroxide is used as an initiator to accelerate the reaction rate.

[0025] The reaction formula of mercapto-1,2-propanediol and N-ethyl perfluorooctane sulfonamidoethyl acrylate is as follows:

[0026] Furthermore, the usage ratio of 3-mercapto-1,2-propylene glycol, N-ethyl perfluorooctane sulfonamidoethyl acrylate and benzoyl peroxide is 200 mL:60 g:1-3 g.

[0027] Further, the modified polyol solid is prepared by the following steps:

[0028] A 0.1 mol / L NaOH solution and chloral hydrate are mixed and stirred to obtain a premixed solution; the premixed solution is placed under a nitrogen atmosphere, 2-chloro-4-hydroxybenzaldehyde is added, and the mixture is reacted at 85-95° C. for 10-12 hours, and then filtered to obtain a solid; the solid is washed three times with deionized water to obtain a modified polyol solid.

[0029] The phenolic hydroxyl group in chloral hydrate easily undergoes a nucleophilic substitution reaction with the chloride ion in 2-chloro-4-hydroxybenzaldehyde, thereby preparing a modified polyol solid.

[0030] The reaction formula of chloro-4-hydroxybenzaldehyde and chloral hydrate is as follows:

[0031] Furthermore, the usage ratio of NaOH solution, 2-chloro-4-hydroxybenzaldehyde and chloral hydrate is 200mL:50g:10-20g.

[0032] Furthermore, when preparing the first film layer, the stirring speed is 100-200 r / min and the stirring time is 10 min; when preparing the second film layer, the mixing and stirring speed is 100 r / min and the reaction time is 10-20 min.

[0033] The present invention has the following beneficial effects:

[0034] 1. The slow-release fertilizer prepared by the present invention uses urea granules as core material, and is coated with a protein capsule film to obtain once-coated urea; gelatin is a protein macromolecular compound composed of 18 kinds of amino acids linked by peptide bonds, and after being hydrolyzed by citric acid, the hydrolyzed gelatin can expose more amino, carboxyl, hydroxyl and other functional groups; in addition, the hydrolyzed gelatin improves its own reaction activity by reducing its own molecular weight. Copper and manganese are trace elements required by crops. Copper sulfate pentahydrate, manganese sulfate monohydrate and deionized water are evenly mixed, and the obtained mixed metal solution can be regarded as a water-soluble fertilizer of trace elements. Citric acid is an organic acid. In the early stage, it mainly participates in cell respiration and photosynthesis. In the later stage, its function is mainly to participate in physiological metabolic activities such as absorption, transportation, distribution and metabolic detoxification of heavy metals. The hydrolyzed gelatin uses its own amino group to react with citric acid. The hydrolyzed gelatin and citric acid use their own hydroxyl and carboxyl functional groups to react with the mixed metal solution for adsorption and complexation, thereby obtaining a mixed metal solution and citric acid-modified gelatin. The metal salt composite gelatin is then modified with methyltrialkylammonium chloride, and quaternary ammonium salt is used to improve the hydrophobicity and adsorption of the protein capsule membrane, further improving the sustained release of the prepared protein capsule membrane. In addition, urea is released into the soil through the protein capsule membrane, and the ammonia produced by the hydrolysis of urea can combine with the carboxylic acid of citric acid, thereby interfering with the effective inhibition of nitrogen volatilization loss and improving the nitrogen nutrient utilization efficiency.

[0035] 2. The present invention drips a dihydroxy-terminated fluorinated chain extender solution, a modified polyol solid and an isophorone diisocyanate liquid onto the surface of the urea after the primary coating, and then reacts on the urea surface to form a polyurethane polymer material, thereby preparing the urea after the secondary coating, that is, the film-coated slow-release fertilizer based on the protein capsule membrane prepared by the present invention. The present invention uses 3-mercapto-1,2-propanediol and N-ethyl perfluorooctane sulfonamide ethyl acrylate as raw materials to synthesize a dihydroxy-terminated fluorinated chain extender to form a hydrophobic monomer, thereby improving the hydrophobicity of the prepared polyurethane; the present invention uses the reaction product of 2-chloro-4-hydroxybenzaldehyde and chloral hydrate as a polyol component, thereby introducing aldehyde groups, chloride ions, hydroxyl groups and other functional groups into the polyol component, and the above-mentioned various functional groups can react with isocyanate groups, and multiple active sites are cross-linked, so that the prepared modified polyurethane forms a multi-segment, network structure, thereby improving the mechanical properties and thermal stability of the modified polyurethane itself. The two layers of coating materials of the slow-release fertilizer prepared by the present invention have good hydrophobicity, mechanical properties and thermodynamics; in addition, the inner layer of the protein capsule film is rich in the nutrient elements required by the crops, enriching the nutritional function of the slow-release fertilizer. The double coating can not only form a secondary slow release of urea, but also extend the material life cycle of the slow-release fertilizer coating material; the double coating process can also reduce the amount of polyurethane used, thereby reducing the potential pollution to the environment without reducing the mechanical properties and hydrophobicity of the prepared coated slow-release fertilizer. DETAILED DESCRIPTION

[0036] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] This embodiment provides a method for preparing a protein capsule film for a film-coated slow-release fertilizer based on a protein capsule film, comprising the following steps:

[0039] 1. Add 1g of citric acid, 30g of gelatin and 200mL of deionized water into a 500mL beaker, then transfer the beaker to a water bath, set the temperature to 50°C, stir mechanically at 100r / min, and swell for 3-5h to obtain a mixed solution; then adjust the temperature of the water bath to 80°C, swell statically for 1h to obtain hydrolyzed gelatin;

[0040] 2. Add 1g of copper sulfate pentahydrate, 1g of manganese sulfate monohydrate and 50mL of deionized water to a 250mL three-necked flask, then fix the three-necked flask in a constant temperature bath, connect the three-necked flask to a stirrer, and stir at 100r / min for 30min at 60°C to obtain a mixed metal solution;

[0041] 3. Mix 50 g of hydrolyzed gelatin, 20 mL of citric acid and 200 mL of deionized water, add to a 500 mL beaker, transfer the beaker to a water bath, adjust the temperature of the water bath to 80 ° C, react for 2 hours, and mechanically stir at 100 r / min during the reaction to obtain a reactant; add 50 mL of mixed metal liquid to the reactant, stir at 100 r / min at 50 ° C for 30 minutes, then heat to 110 ° C, react until all the deionized water solvent is completely evaporated, and obtain a metal salt composite gelatin;

[0042] 4. Add 50 g of metal salt composite gelatin and 50 mL of deionized water into a three-necked flask, mix well, and stir at 50°C for 40 min; then add 10 g of methyltrialkylammonium chloride into the three-necked flask, mix and react at 60°C for 40 min to obtain a product; let the product stand at room temperature for 2 h, and then vacuum dry at 60°C for 1 h to obtain a protein capsule membrane.

[0043] Example 2

[0044] This embodiment provides a method for preparing a protein capsule film for a film-coated slow-release fertilizer based on a protein capsule film, comprising the following steps:

[0045] 1. Add 3g of citric acid, 30g of gelatin and 200mL of deionized water into a 500mL beaker, then transfer the beaker to a water bath, set the temperature to 50°C, stir mechanically at 100r / min, and swell for 4h to obtain a mixed solution; then adjust the temperature of the water bath to 80°C, swell statically for 1.5h to obtain hydrolyzed gelatin;

[0046] 2. Add 3g of copper sulfate pentahydrate, 3g of manganese sulfate monohydrate and 50mL of deionized water into a 250mL three-necked flask, then fix the three-necked flask into a constant temperature bath, connect the three-necked flask to a stirrer, stir at 100r / min for 30min at 60°C to obtain a mixed metal solution;

[0047] 3. Mix 50g of hydrolyzed gelatin, 20mL of citric acid and 200mL of deionized water, add to a 500mL beaker, transfer the beaker to a water bath, adjust the temperature of the water bath to 85°C, react for 2.3h, and mechanically stir at 100r / min during the reaction to obtain a reactant; add 50mL of mixed metal liquid to the reactant, stir at 100r / min at 50°C for 30min, then heat to 110°C, and react until all the deionized water solvent is completely evaporated to obtain a metal salt composite gelatin;

[0048] 4. Add 50 g of metal salt composite gelatin and 50 mL of deionized water into a three-necked flask, mix well, and stir at 55°C for 45 min; then add 10 g of methyltrialkylammonium chloride into the three-necked flask, mix and react at 60°C for 43 min to obtain a product; let the product stand at room temperature for 3 h, and then vacuum dry at 65°C for 1.3 h to obtain a protein capsule membrane.

[0049] Example 3

[0050] This embodiment provides a method for preparing a protein capsule film for a film-coated slow-release fertilizer based on a protein capsule film, comprising the following steps:

[0051] 1. Add 5g of citric acid, 30g of gelatin and 200mL of deionized water into a 500mL beaker, then transfer the beaker to a water bath, set the temperature to 50°C, stir mechanically at 100r / min, and swell for 5h to obtain a mixed solution; then adjust the temperature of the water bath to 80°C, swell statically for 2h to obtain hydrolyzed gelatin;

[0052] 2. Add 5 g of copper sulfate pentahydrate, 5 g of manganese sulfate monohydrate and 50 mL of deionized water into a 250 mL three-necked flask, then fix the three-necked flask into a thermostatic bath, connect the three-necked flask to a stirrer, and stir at 100 r / min for 30 min at 60 ° C to obtain a mixed metal solution;

[0053] 3. Mix 50 g of hydrolyzed gelatin, 20 mL of citric acid and 200 mL of deionized water, add to a 500 mL beaker, transfer the beaker to a water bath, adjust the temperature of the water bath to 90 ° C, react for 3 hours, and mechanically stir at 100 r / min during the reaction to obtain a reactant; add 50 mL of mixed metal liquid to the reactant, stir at 100 r / min at 50 ° C for 30 minutes, then heat to 110 ° C, react until all the deionized water solvent is completely evaporated, and obtain a metal salt composite gelatin;

[0054] 4. Add 50 g of metal salt composite gelatin and 50 mL of deionized water into a three-necked flask, mix well, and stir at 60°C for 50 min; then add 10 g of methyltrialkylammonium chloride into the three-necked flask, mix and react at 60°C for 50 min to obtain a product; let the product stand at room temperature for 4 h, and then vacuum dry at 70°C for 2 h to obtain a protein capsule membrane.

[0055] Example 4

[0056] This embodiment provides a method for preparing a film-coated slow-release fertilizer based on a protein capsule film, comprising the following steps:

[0057] S1. In a 250 mL three-necked flask equipped with a condenser, add 200 mL of 3-mercapto-1,2-propylene glycol, 60 g of N-ethyl perfluorooctane sulfonamidoethyl acrylate and 1 g of benzoyl peroxide, transfer the three-necked flask to a water bath, adjust the temperature of the water bath to 100° C., stir mechanically at 100 r / min, and react for 3 h to obtain a mixture; heat the mixture to 120° C. and react until all 3-mercapto-1,2-propylene glycol is completely volatilized to obtain a dihydroxy-terminated fluorinated chain extender solution;

[0058] S2. Add 200 mL of 0.1 mol / L NaOH solution and 10 g of chloral hydrate solid to a 500 mL three-necked flask, stir at 100 r / min for 5 min to obtain a premixed solution; connect a condenser to one end of the three-necked flask, fill the three-necked flask with nitrogen until the three-necked flask is in a nitrogen atmosphere; then transfer the three-necked flask to a water bath, set the temperature of the water bath to 85° C., add 50 g of 2-chloro-4-hydroxybenzaldehyde to the three-necked flask, react for 10 h, and then filter to obtain a solid; wash the solid three times with deionized water to obtain a modified polyol solid;

[0059] S3, 500g of urea granules are placed in a drum granulator and preheated at 50°C for 10min; then 500g of urea is added to a beaker, and 10g of the protein capsule film prepared in Example 1 is heated to melt, added to the beaker, and stirred evenly with an electric stirrer to obtain urea after one coating; wherein the stirring rate is 100r / min and the stirring time is 10min; then 5g of dihydroxy-terminated fluorinated chain extender solution, 5g of modified polyol solid and 10g of isophorone diisocyanate are added to the beaker, accompanied by mechanical stirring at 100r / min, and the reaction is carried out for 10min. The above-mentioned feeding process is carried out twice to obtain urea after secondary coating; the urea after secondary coating is placed in a vacuum drying oven and dried at 30°C for 30min to prepare a coated slow-release fertilizer based on protein capsule film.

[0060] Example 5

[0061] This embodiment provides a method for preparing a film-coated slow-release fertilizer based on a protein capsule film, comprising the following steps:

[0062] S1. In a 250 mL three-necked flask equipped with a condenser, add 200 mL of 3-mercapto-1,2-propylene glycol, 60 g of N-ethyl perfluorooctane sulfonamidoethyl acrylate and 2 g of benzoyl peroxide, transfer the three-necked flask to a water bath, adjust the temperature of the water bath to 105° C., stir mechanically at 150 r / min, and react for 4 h to obtain a mixture; heat the mixture to 123° C. and react until all 3-mercapto-1,2-propylene glycol is completely volatilized to obtain a dihydroxy-terminated fluorinated chain extender solution;

[0063] S2. Add 200 mL of 0.1 mol / L NaOH solution and 16 g of chloral hydrate solid to a 500 mL three-necked flask, stir at 100 r / min for 5 min to obtain a premixed solution; connect a condenser to one end of the three-necked flask, fill the three-necked flask with nitrogen until the three-necked flask is in a nitrogen atmosphere; then transfer the three-necked flask to a water bath, set the temperature of the water bath to 90° C., add 50 g of 2-chloro-4-hydroxybenzaldehyde to the three-necked flask, react for 11 h, and then filter to obtain a solid; wash the solid three times with deionized water to obtain a modified polyol solid;

[0064] S3, 500g of urea granules are placed in a drum granulator and preheated at 55°C for 10min; then 500g of urea is added to a beaker, and 15g of the protein capsule film prepared in Example 2 is melted, added to the beaker, and stirred evenly with an electric stirrer to obtain urea after a single coating; wherein the stirring rate is 150r / min and the stirring time is 10min; then 5g of a dihydroxy-terminated fluorinated chain extender solution, 5g of a modified polyol solid and 15g of isophorone diisocyanate are added to a beaker, accompanied by mechanical stirring at 100r / min, and the reaction is carried out for 15min. The above-mentioned feeding process is carried out twice to obtain urea after a secondary coating; the urea after the secondary coating is placed in a vacuum drying oven and dried at 35°C for 30min to prepare a coated slow-release fertilizer based on the protein capsule film.

[0065] Example 6

[0066] This embodiment provides a method for preparing a film-coated slow-release fertilizer based on a protein capsule film, comprising the following steps:

[0067] S1. In a 250 mL three-necked flask equipped with a condenser, add 200 mL of 3-mercapto-1,2-propylene glycol, 60 g of N-ethyl perfluorooctane sulfonamidoethyl acrylate and 3 g of benzoyl peroxide, transfer the three-necked flask to a water bath, adjust the temperature of the water bath to 110° C., stir mechanically at 200 r / min, and react for 5 h to obtain a mixture; heat the mixture to 130° C. and react until all 3-mercapto-1,2-propylene glycol is completely volatilized to obtain a dihydroxy-terminated fluorinated chain extender solution;

[0068] S2. Add 200 mL of 0.1 mol / L NaOH solution and 20 g of chloral hydrate solid to a 500 mL three-necked flask, mix and stir at 100 r / min for 5 min to obtain a premixed solution; connect a condenser to one end of the three-necked flask, fill the three-necked flask with nitrogen until the three-necked flask is in a nitrogen atmosphere; then transfer the three-necked flask to a water bath, set the temperature of the water bath to 95° C., add 50 g of 2-chloro-4-hydroxybenzaldehyde to the three-necked flask, react for 12 h, and then filter to obtain a solid; wash the solid three times with deionized water to obtain a modified polyol solid;

[0069] S3, 500g of urea granules are placed in a drum granulator and preheated at 60°C for 10min; then 500g of urea is added to a beaker, and 20g of the protein capsule film prepared in Example 3 is melted, added to the beaker, and stirred evenly with an electric stirrer to obtain urea after one coating; wherein, the stirring rate is 200r / min and the stirring time is 10min; then 5g of dihydroxy-terminated fluorinated chain extender solution, 5g of modified polyol solid and 20g of isophorone diisocyanate are added to the beaker, accompanied by mechanical stirring at 100r / min, and the reaction is carried out for 20min. The above-mentioned feeding process is carried out twice to obtain urea after secondary coating; the urea after secondary coating is placed in a vacuum drying oven and dried at 40°C for 30min to prepare a coated slow-release fertilizer based on protein capsule film.

[0070] Comparative Example 1

[0071] The difference between this comparative example and Example 6 is that in step S3, during the preparation of the protein capsule membrane, citric acid is not used to modify the hydrolyzed gelatin.

[0072] Comparative Example 2

[0073] The difference between this comparative example and Example 6 is that in step S3, the molten protein capsule membrane is not added and the urea is not coated once.

[0074] Comparative Example 3

[0075] The difference between this comparative example and Example 6 is that step S2 is eliminated, and in step S3, ethylene glycol is used instead of modified polyol.

[0076] Comparative Example 4

[0077] The difference between this comparative example and Example 6 is that step S1 is eliminated, and in step S3, 3-mercapto-1,2-propanediol is used to replace the dihydroxy-terminated fluorinated chain extender solution.

[0078] Performance Test:

[0079] 1. The film-coated slow-release fertilizer based on the protein capsule membrane prepared in Examples 4-6 and Comparative Examples 1-4 was subjected to thermogravimetric testing; the test was performed using a TG analysis thermogravimeter at a heating rate of 10°C / min from room temperature to 700°C in a nitrogen atmosphere.

[0080] 2. The water contact angle of the film-coated slow-release fertilizer based on the protein capsule membrane prepared in Examples 4-6 and Comparative Examples 1-4 was tested; an optical contact angle tester was used, and the test was performed three times to obtain the average value.

[0081] 3. According to GB / T23348-2009, the nitrogen release rate of the protein capsule film-coated slow-release fertilizers prepared in Examples 4-6 and Comparative Examples 1-4 was measured at 25°C for 30 days and 40 days.

[0082] The performance test data is shown in Table 1.

[0083] Table 1 Performance test data of the sample

[0084] Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Quality retention rate / (%) 83 84 87 86 79 72 85 Water contact angle / (°) 91.56 92.19 93.42 93.16 95.12 93.12 83.16 Nitrogen release rate value at 30 days / (%) 68 64 62 60 73 64 63 Nitrogen release rate value at 40 days / (%) 75 73 72 69 81 72 74

[0085] Data Analysis:

[0086] Comparative analysis of the data in Table 1 shows that the film-coated slow-release fertilizers based on the protein capsule membranes prepared in Examples 4-6 of the present invention all have excellent thermal stability, which is manifested in a high value of the quality retention rate;

[0087] The coated slow-release fertilizers based on the protein capsule membrane prepared in Examples 4-6 of the present invention all have excellent hydrophobicity and slow-release ability, as shown by large water contact angle values ​​and stable release rates of nitrogen at 30 days and 40 days;

[0088] However, in Comparative Example 2, urea was not coated once, which reduced its slow-release performance, as shown by the faster nitrogen release rate at 30 days and 40 days;

[0089] In Comparative Example 3, the same mass of ethylene glycol was used to replace the modified polyol solid, which reduced the cross-linking sites between itself and isophorone diisocyanate and reduced its own cross-linking degree, which was manifested as a decrease in quality retention rate;

[0090] In Comparative Example 4, 3-mercapto-1,2-propanediol was used to replace the dihydroxy-terminated fluorinated chain extender solution, which reduced the fluorine content in the secondary coating material, thereby reducing its own hydrophobicity, which is manifested as a decrease in the water contact angle.

[0091] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0092] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0093] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A film-coated slow-release fertilizer based on a protein capsule film, characterized in that: The urea granules are covered with a first film layer and a second film layer in sequence from the inside to the outside; The preparation method of the first film layer is: 10-20 g of protein capsule membrane is melted to obtain a melted protein capsule membrane; 500 g of urea granules are placed in a drum granulator, preheated at 50-60° C. for 10 min, and the melted protein capsule membrane is added to the urea granules, and stirred evenly to obtain a first film layer; The preparation method of the second film layer is: Add 5 g of dihydroxy-terminated fluorinated chain extender solution, 5 g of modified polyol solid and 10-20 g of isophorone diisocyanate to the protein capsule film, mix, stir and react; the above-mentioned adding process is carried out twice to obtain a second film layer; The preparation method of the protein capsule film comprises the following steps: A1, citric acid, gelatin and deionized water are mixed, and the mixture is swollen at 50°C for 3-5 hours with mechanical stirring; and then the mixture is statically swollen at 80°C for 1-2 hours to obtain hydrolyzed gelatin; A2, copper sulfate pentahydrate, manganese sulfate monohydrate and deionized water are mixed and stirred to obtain a mixed metal solution; A3, mixing hydrolyzed gelatin, citric acid and deionized water, reacting at 80-90°C for 2-3h to obtain a reactant; adding a mixed metal solution to the reactant, reacting at 50-60°C for 30min, then heating to 110-120°C, reacting until all the deionized water solvent is completely evaporated, to obtain a metal salt composite gelatin; A4, metal salt composite gelatin and deionized water are mixed evenly, and stirred at 50-60°C for 40-50 minutes to obtain intermediate A; intermediate A and methyltrialkylammonium chloride are mixed and reacted at 60°C for 40-50 minutes to obtain a product; the product is allowed to stand at room temperature for 2-4 hours, and then vacuum dried at 60-70°C for 1-2 hours to obtain a protein capsule membrane.

2. The film-coated slow-release fertilizer based on protein capsule film according to claim 1, characterized in that: In step A1, the dosage ratio of citric acid, gelatin and deionized water is 1-5g:30g:200mL, and the speed of mechanical stirring is 100r / min; in step A2, the dosage ratio of copper sulfate pentahydrate, manganese sulfate monohydrate and deionized water is 1-5g:1-5g:50mL.

3. The film-coated slow-release fertilizer based on protein capsule film according to claim 1, characterized in that: In step A3, the usage ratio of hydrolyzed gelatin, citric acid and deionized water is 50-60g:20-30mL:200mL, and the usage ratio of mixed metal liquid is 50mL; in step A4, the usage ratio of metal salt composite gelatin, deionized water and methyltrialkylammonium chloride is 50g:50mL:10-20g.

4. The film-coated slow-release fertilizer based on protein capsule film according to claim 1, characterized in that: The dihydroxy terminated fluorinated chain extender solution is prepared by the following steps: 3-Mercapto-1,2-propanediol, N-ethyl perfluorooctane sulfonamidoethyl acrylate and benzoyl peroxide are mixed and reacted at 100-110° C. for 3-5 hours to obtain a mixture; the mixture is heated to 120-130° C. and reacted until the 3-mercapto-1,2-propanediol solvent is completely evaporated to obtain a dihydroxy-terminated fluorinated chain extender solution.

5. The film-coated slow-release fertilizer based on protein capsule film according to claim 4, characterized in that: The usage ratio of 3-mercapto-1,2-propanediol, N-ethyl perfluorooctane sulfonamidoethyl acrylate and benzoyl peroxide is 200mL:60g:1-3g.

6. The film-coated slow-release fertilizer based on protein capsule film according to claim 1, characterized in that: The modified polyol solid is prepared by the following steps: A 0.1 mol / L NaOH solution and chloral hydrate are mixed and stirred to obtain a premixed solution; the premixed solution is placed under a nitrogen atmosphere, 2-chloro-4-hydroxybenzaldehyde is added, and the mixture is reacted at 85-95° C. for 10-12 hours, and then filtered to obtain a solid; the solid is washed three times with deionized water to obtain a modified polyol solid.

7. The film-coated slow-release fertilizer based on protein capsule film according to claim 6, characterized in that: The dosage ratio of NaOH solution, 2-chloro-4-hydroxybenzaldehyde and chloral hydrate is 200mL:50g:10-20g.

8. The film-coated slow-release fertilizer based on protein capsule film according to claim 1, characterized in that: When preparing the first film layer, the stirring speed is 100-200r / min and the stirring time is 10min; when preparing the second film layer, the mixing and stirring speed is 100r / min and the reaction time is 10-20min.