Composite material for preparing powdered polycarboxylate water reducer, powdered polycarboxylate water reducer and preparation method thereof
The composite material prepared by copolymerizing modified silica gel and unsaturated monomers works synergistically with inorganic salts to quickly cure the polycarboxylic acid water reducer, solving the problem of complex manufacturing process and high energy consumption of powder polycarboxylic acid water reducer, realizing the It provides efficient and low-cost powder water reducing agent production, provides internal curing effect and reduces concrete cracking.
Patent Information
- Application Number
- CN202411146655.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing powder polycarboxylic acid water-reducing agent is complex in manufacturing process, high energy consumption, and difficult to produce on a large scale, resulting in high product prices. The spray drying method requires large equipment and high energy consumption. The high-temperature process provides polycarboxylic acid water-reducing agents. The performance is unfavorable, the traditional method is cumbersome to operate, the environmental pollution is severe, and the product is prone to stickiness and difficult to store.
Copolymerization of modified silica gel, unsaturated small monomer, unsaturated salt monomer, chain transfer agent, and initiator is used to prepare composite materials, and synergistically work with inorganic salts that can generate crystal hydrates to quickly cure the polycarboxylic acid water reducer aqueous solution , form a highly absorbent powder water reducing agent, improve mechanical strength and powder forming properties, and reduce the high energy consumption and reaction out-of-control problems of the spray drying process.
It realizes rapid curing and high mechanical strength of polycarboxylic acid water reducing agent, reduces production costs, avoids high energy consumption of spray drying, provides internal curing effect, reduces concrete cracking, and has excellent finished product performance and is suitable for large-scale production.
Smart Images

Figure CN118652396B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water reducers, and particularly relates to a composite material for preparing a powdered polycarboxylic acid water reducer, a powdered polycarboxylic acid water reducer and a preparation method. Background Art
[0002] Polycarboxylate water reducers can be divided into two forms: liquid and solid. Liquid polycarboxylate water reducers have excellent properties such as low dosage, high water reduction rate, significant strength improvement, green and pollution-free, simple synthesis process and low cost. However, they have problems such as high storage and transportation costs and limited application scope. Therefore, solid polycarboxylate water reducers have developed rapidly in recent years. They are easy to transport and store, and can also be widely used in grouting materials, dry-mixed mortar and other fields.
[0003] At present, the production and preparation process of solid polycarboxylic acid water reducer is mainly based on spray drying, but spray drying consumes a lot of energy and has high cost, and the addition of anti-caking agent will also affect the product performance to a certain extent. In addition, bulk polymerization is also one of the hot research directions of solid water reducer, but the bulk polymerization temperature is high, the viscosity of the polymerization system increases, and it is easy to cause double bond destruction, low conversion rate, or local implosion, and reaction out of control. Therefore, it still remains in the laboratory research stage and is difficult to carry out large-scale production.
[0004] The Chinese patent with publication number CN101824125A discloses a method for preparing a powdered polycarboxylic acid high-performance water-reducing agent, wherein the polycarboxylic acid water-reducing agent solution is thrown out at high speed through the centrifugal disk of a centrifugal spray dryer to form droplets, and dried under the conditions of an inlet air temperature of 180-230°C, an outlet air temperature of 80-120°C, and adding an anti-sticking agent to the air inlet duct, thereby obtaining a powdered polycarboxylic acid high-performance water-reducing agent. However, the spray drying method requires large equipment, high energy consumption during the drying process, and the high temperature process has an adverse effect on the performance of the polycarboxylic acid water-reducing agent.
[0005] The Chinese patent with publication number CN102372828A discloses a method for synthesizing a solid polycarboxylate water-reducing agent, and the technical scheme is to use a monomer containing an unsaturated group to react in an organic solvent, add an alkaline substance to neutralize it after the reaction, and prepare the polycarboxylate water-reducing agent through centrifugal separation, and then dry the prepared polycarboxylate water-reducing agent to obtain a solid polycarboxylate water-reducing agent. The main disadvantages of this preparation method are that the organic solvent consumption is large, the production process is complicated, and the environmental pollution is serious.
[0006] The Chinese patent with publication number CN103554382A discloses a method for solid phase synthesis of polycarboxylate water reducer, and the polymerization reaction is completed in a ball mill or a colloid mill. Add polyether monomer, initiator and a small amount of water to the ball mill or colloid mill, start the machine to mix for 10 minutes, and then add a mixture of small molecule monomer, reducing agent, chain transfer agent and water of the same mass as the small molecule monomer to the ball mill or colloid mill in several times. After all are added, continue to react for 1 hour to obtain a solid or paste polycarboxylate water reducer. This method not only has cumbersome operating steps and is difficult to process production, but also requires the addition of a certain amount of water. The final product may be a paste. Even if it is a solid, it is easy to become sticky due to residual moisture and is not easy to store.
[0007] In summary, the existing powdered polycarboxylic acid water-reducing agent has a complex manufacturing process, high energy consumption, and is difficult to mass produce, resulting in a high product price. Summary of the invention
[0008] In order to solve the above technical problems, the present invention provides a composite material for preparing a powdered polycarboxylate water-reducing agent and a preparation method thereof. The composite material has high water absorption. When used as a raw material for the powdered polycarboxylate water-reducing agent, it can synergistically act with an inorganic salt that can form a crystalline hydrate, so that the polycarboxylate water-reducing agent aqueous solution is rapidly solidified, thereby preparing the powdered polycarboxylate water-reducing agent, while ensuring the initial dispersion performance of the water-reducing agent, providing an internal curing effect, and reducing concrete cracking.
[0009] The present invention also provides a powdered polycarboxylate water-reducing agent and a preparation method thereof. The powdered polycarboxylate water-reducing agent uses the composite material for preparing the powdered polycarboxylate water-reducing agent provided by the present invention, the polycarboxylate water-reducing agent, and an inorganic salt capable of forming a crystalline hydrate as raw materials. The composite material and the inorganic salt capable of forming a crystalline hydrate synergistically absorb moisture in an aqueous solution of the polycarboxylate water-reducing agent to rapidly solidify the aqueous solution, thereby preparing the powdered polycarboxylate water-reducing agent.
[0010] The technical solution adopted by the present invention is as follows:
[0011] The present invention provides a composite material for preparing a powdered polycarboxylate water reducer, wherein the composite material has the structural formula:
[0012] Wherein, R1 represents H or CH3; a=0 or 1, R2 represents COOCH2CH2CH2; R3 represents COOH or CONH2; Represents silica gel; x:y:z=2~6:7~10:2
[0013] The composite material for preparing powdered polycarboxylic acid water-reducing agent comprises the following raw materials: modified silica gel, unsaturated small monomers, unsaturated salt monomers, chain transfer agent, and initiator.
[0014] The modified silica gel is silica gel modified by a silane coupling agent containing unsaturated double bonds; the silane coupling agent containing unsaturated double bonds is vinyl trimethoxy silane, vinyl triethoxy silane, vinyl tri (2-methoxyethoxy) silane or γ-methacryloxypropyl trimethoxy silane.
[0015] The initiator is azobisisobutyronitrile, azobisisoheptanenitrile or dimethyl azobisisobutyrate; the chain transfer agent is mercaptoethanol or 3-mercaptopropionic acid.
[0016] The unsaturated small monomer is at least one of acrylic acid, methacrylic acid or acrylamide.
[0017] The unsaturated salt monomer is magnesium acrylate or magnesium methacrylate.
[0018] The present invention also provides a method for preparing the composite material for preparing a powdered polycarboxylate water-reducing agent, the method comprising the following steps:
[0019] Step 1: Activate and acidify the silica gel at high temperature in sequence, and wash it to neutrality to obtain acidified silica gel;
[0020] Step 2: dispersing the acidified silica gel in an organic solvent, adding a silane coupling agent containing an unsaturated double bond, stirring and reacting to obtain a suspension of modified silica gel;
[0021] Step 3: Stir and heat the suspension of modified silica gel to 50-70°C, add an initiator, and drop a mixed solution containing unsaturated small monomers, unsaturated salt monomers, and a chain transfer agent. After the dropwise addition is completed, keep the mixture warm for reaction. After the reaction is completed, filter the mixture, dry and grind the residue to obtain a composite material for preparing a powdered polycarboxylic acid water reducer.
[0022] Furthermore, the mass ratio of the modified silica gel, the unsaturated small monomer, the unsaturated salt monomer, the chain transfer agent and the initiator is 50~150:10~15:5~10:0.1~0.2:0.2.
[0023] In step 1, the specific surface area of the silica gel is 650-800m 2 / g; the high temperature activation condition is heating at 440-460°C for 7-9h; the acidification condition is stirring in a hydrochloric acid solution with a mass concentration of 15-25% for 10-12h.
[0024] In step 2, the organic solvent is toluene; the silane coupling agent containing unsaturated double bonds is vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane or γ-methacryloxypropyltrimethoxysilane.
[0025] In step 2, the mass ratio of the acidified silica gel to the silane coupling agent containing an unsaturated double bond is 1:0.1-0.4; and the stirring reaction time is 10-12 hours.
[0026] In step three, the initiator is azobisisobutyronitrile, azobisisoheptanenitrile or dimethyl azobisisobutyrate; and the chain transfer agent is mercaptoethanol or 3-mercaptopropionic acid.
[0027] In step three, the unsaturated small monomer is at least one of acrylic acid, methacrylic acid or acrylamide; and the unsaturated salt monomer is magnesium acrylate or magnesium methacrylate.
[0028] In step 3, the dropwise addition time is 2 to 4 hours, and the heat preservation reaction time is 1 hour.
[0029] The present invention also provides a powder polycarboxylate water reducer, wherein the powder polycarboxylate water reducer uses the composite material for preparing the powder polycarboxylate water reducer described in the present invention as a raw material.
[0030] The powdered polycarboxylate water reducer is composed of the following raw materials in parts by weight: 80-120 parts of a polycarboxylate water reducer with a solid content of 50-80%, 1-5 parts of a composite material for preparing the powdered polycarboxylate water reducer, and 5-10 parts of an inorganic salt capable of generating a crystalline hydrate.
[0031] The inorganic salt capable of forming a crystalline hydrate is any one or more of anhydrous magnesium sulfate, magnesium sulfate monohydrate, sodium carbonate, and sodium thiosulfate.
[0032] The present invention also provides a preparation method of the powdered polycarboxylate water reducer, which comprises the following steps: heating a polycarboxylate water reducer having a solid content of 50-80% to 65-75° C., adding a composite material for preparing the powdered polycarboxylate water reducer and an inorganic salt capable of generating a crystalline hydrate, stirring evenly, cooling to room temperature, crushing and grinding to obtain the powdered polycarboxylate water reducer.
[0033] The composite material for preparing a powdered polycarboxylic acid water-reducing agent provided by the present invention is obtained by copolymerizing silica gel modified by a silane coupling agent containing unsaturated double bonds, acrylic acid or acrylamide unsaturated small monomers, and acrylate unsaturated monomers. The composite material is an ion cross-linked polymer with high mechanical strength and water absorption. When used in combination with an inorganic salt capable of generating a crystalline hydrate as a raw material for a powdered polycarboxylic acid water-reducing agent, the composite material can quickly absorb the water in the polycarboxylic acid water-reducing agent to rapidly solidify the polycarboxylic acid water-reducing agent, and has good powdering properties, and can significantly improve the problem of sticky blocks generated during the crushing and grinding process of the solid water-reducing agent.
[0034] The powdered polycarboxylate water-reducing agent provided by the present invention can provide an internal curing effect in addition to a water-reducing effect, can effectively promote the full hydration of cement, inhibit the self-shrinkage of concrete, and thus reduce the cracking of concrete. When the humidity of the surrounding cement environment decreases, the water adsorbed by the highly absorbent composite material in the powdered polycarboxylate water-reducing agent will be spontaneously released under the action of osmotic pressure, delaying the reduction of internal humidity, promoting further hydration of cement, and making up for the defects of inadequate traditional curing and low curing efficiency.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) Silica gel is often used for drying and dehumidification due to its strong adsorption capacity, good thermal stability, stable chemical properties, high mechanical strength, recyclability, non-toxicity and pollution-free. However, the water absorption rate of ordinary silica gel is not high. The present invention utilizes the condensation reaction of the silanol group on the surface of silica gel with a silane coupling agent to prepare a modified silica gel containing double bonds, which can be copolymerized with small monomers such as acrylic acid or acrylamide to obtain a highly water-absorbent composite material.
[0037] (2) Polyacrylic acid or polyacrylamide type highly absorbent polymers become gel-like after absorbing water and have low mechanical strength. The present invention introduces magnesium acrylate or magnesium methacrylate monomers during polymerization to form an ion-crosslinked polymer with higher mechanical strength. In addition, the introduction of silica gel components further improves the mechanical strength of the composite material, so that it can still have a certain mechanical strength after absorbing water, thereby achieving the solidification of the polycarboxylate water-reducing agent aqueous solution.
[0038] (3) In the powdered polycarboxylic acid water-reducing agent provided by the present invention, the highly water-absorbent composite material provided by the present invention and the inorganic salt capable of forming crystalline hydrates are used as raw materials. Both of them can absorb water in the aqueous solution of the polycarboxylic acid water-reducing agent to make it solidify rapidly. Among them, the inorganic salt capable of forming crystalline hydrates forms crystalline hydrates after absorbing water. Compared with organic matter, the powdering performance is better, and the problem of sticky blocks generated during the crushing and grinding process of the solid water-reducing agent can be significantly improved.
[0039] (4) The powdered polycarboxylic acid water-reducing agent provided by the present invention can provide internal curing effect on the basis of providing water-reducing performance, which can effectively promote the full hydration of cement, inhibit the self-shrinkage of concrete, and thus reduce the cracking of concrete. When the humidity of the surrounding cement environment decreases, the water adsorbed by the highly absorbent composite material will be spontaneously released under the action of osmotic pressure, delaying the decrease of internal humidity, promoting further hydration of cement, and making up for the defects of traditional curing such as inadequate curing and low curing efficiency.
[0040] (5) The method of the present invention prepares a powdered polycarboxylate water-reducing agent by adsorbing water in the polycarboxylate water-reducing agent aqueous solution, thereby effectively avoiding the high energy consumption caused by the spray drying process, as well as the difficulties in heat dissipation and poor reaction controllability of bulk polymerization. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 is the structural formula of the composite material used to prepare the powdered polycarboxylate water-reducing agent;
[0042] Figure 2 This is a state diagram of the powdered polycarboxylate water-reducing agent obtained after grinding in Example 6;
[0043] Figure 3 This is a state diagram of the powdered polycarboxylate water-reducing agent obtained after grinding in Comparative Example 1;
[0044] Figure 4 This is a state diagram of the powdered polycarboxylate water-reducing agent obtained after grinding in Comparative Example 2;
[0045] Figure 5 This is a state diagram of the powdered polycarboxylic acid water-reducing agent obtained after grinding in Comparative Example 4. DETAILED DESCRIPTION
[0046] The present invention is described in detail below with reference to the embodiments.
[0047] The preparation method of the polycarboxylate water-reducing agent in the embodiment and comparative example is as follows:
[0048] Polycarboxylate water reducer A: Heat 120g of isopentanol polyoxyethylene ether TPEG-2400 to 70°C to melt, add a mixed solution of 1g of sodium hypophosphite and 18g of water, then add 2.6g of acrylic acid, stir evenly, add dropwise a mixed solution of 10g of acrylic acid, 0.8g of ammonium persulfate and 15.6g of water, the dropping time is 3 hours, and after the reaction is completed, keep warm for 1.5h to obtain a polycarboxylate water reducer A with a solid content of 80%.
[0049] Polycarboxylate water reducer B: Heat 120g of isopentanol polyoxyethylene ether TPEG-2400 to 70°C to melt, add a mixed solution of 1g of sodium hypophosphite and 29.2g of water, then add 2.6g of acrylic acid, stir evenly, add dropwise a mixed solution of 10g of acrylic acid, 0.8g of ammonium persulfate and 15.6g of water, the dropping time is 3 hours, and after the reaction is completed, keep warm for 1.5h to obtain a polycarboxylate water reducer B with a solid content of 75%.
[0050] Polycarboxylate water reducer C: 120g of isobutylene alcohol polyoxyethylene ether TPEG-2400 and 27.4g of water were heated to 70°C to dissolve, then 2.6g of acrylic acid was added and stirred evenly, and a mixed solution of 0.5g of mercaptopropionic acid, 10g of acrylic acid and 15g of water was added dropwise for 3 hours. At the same time, a mixed solution of 0.8g of ammonium persulfate and 15g of water was added dropwise for 3 hours. After the reaction was completed, the mixture was kept warm for 1.5h to obtain a polycarboxylate water reducer C with a solid content of 70%.
[0051] Polycarboxylate water reducer D: 120g of isobutylene alcohol polyoxyethylene ether TPEG-2400 and 42.1g of water were heated to 70°C to dissolve, then 2.6g of acrylic acid was added and stirred evenly, and a mixed solution of 0.5g of mercaptopropionic acid, 10g of acrylic acid and 15g of water was added dropwise for 3 hours. At the same time, a mixed solution of 0.8g of ammonium persulfate and 15g of water was added dropwise for 3 hours. After the reaction was completed, the mixture was kept warm for 1.5h to obtain a polycarboxylate water reducer D with a solid content of 65%.
[0052] Polycarboxylate water reducer E: Add 120g of isopentanol polyoxyethylene ether TPEG-2400 and 70g of water into a 500mL three-necked flask, stir at 35°C until completely dissolved, add 2.5g of acrylic acid and 0.5g of ammonium persulfate, add dropwise a mixed solution of 10g of acrylic acid and 13.5g of water for 3 hours, and at the same time, add dropwise a mixed solution of 0.35g of mercaptoethanol, 0.3g of ascorbic acid and 10g of water for 3.5 hours. After the reaction is completed, keep warm for 1h, add 4.8g of sodium hydroxide, and obtain a polycarboxylate water reducer E with a solid content of 60%.
[0053] Polycarboxylate water reducer F: Add 120g of isopentanol polyoxyethylene ether TPEG-2400 and 80g of water into a 500mL three-necked flask, stir at 35°C until completely dissolved, add 2.5g of acrylic acid and 0.5g of ammonium persulfate, add dropwise a mixed solution of 10g of acrylic acid and 15g of water for 3 hours, and simultaneously add dropwise a mixed solution of 0.35g of mercaptoethanol, 0.3g of ascorbic acid and 25g of water for 3.5 hours. After the reaction is completed, keep warm for 1h, add 16.2g of 30% sodium hydroxide aqueous solution, and supplement 2.8g of water to obtain a polycarboxylate water reducer F with a solid content of 50%.
[0054] The model of the super absorbent resin is Qimai CA-90. Example 1
[0055] A method for preparing a powdered polycarboxylate water reducer: 120 parts of a polycarboxylate water reducer A with a solid content of 80% are taken, heated to 70°C, 2 parts of a composite material for preparing the powdered polycarboxylate water reducer and 5 parts of anhydrous magnesium sulfate are added, stirred evenly, cooled to room temperature, crushed and ground to obtain a powdered polycarboxylate water reducer.
[0056] The preparation method of the composite material for preparing the powdered polycarboxylate water reducer is as follows:
[0057] Step 1: Set the specific surface area to 700m 2 / g silica gel is placed in a muffle furnace at 450℃ and dried for 8h, then cooled naturally to room temperature, and the silica gel after high temperature activation is added into a hydrochloric acid solution with a mass concentration of 20%, and the mass volume ratio of silica gel to hydrochloric acid solution is 1g:5mL, and mechanically stirred at room temperature for 12h, and then washed with distilled water to neutrality, and dried in a vacuum oven at 60℃ to constant weight to obtain acidified silica gel, thereby fully exposing the silanol groups on the surface of the silica gel to facilitate subsequent reactions;
[0058] Step 2: Add the acidified silica gel to the toluene solvent, ultrasonicate for 20 minutes to make it uniformly dispersed, then add γ-methacryloxypropyltrimethoxysilane, mechanically stir at 50°C, react for 12 hours to obtain SG-SCA suspension. The mass ratio of acidified silica gel to γ-methacryloxypropyltrimethoxysilane is 1:0.3, and the amount of acidified silica gel and toluene is 1g:5mL;
[0059] Step 3: Stir and heat the SG-SCA suspension to 65°C, add azobisisobutyronitrile, and simultaneously drop a mixed solution containing acrylic acid, magnesium acrylate, and 3-mercaptopropionic acid. The dropping time is 3 hours, followed by insulation for 1 hour, suction filtration, and the filter residue is dried in a vacuum oven at 60°C to constant weight, and then crushed and ground to obtain a composite material for preparing a powdered polycarboxylic acid water reducer; the mass ratio of SG-SCA, acrylic acid, magnesium acrylate, 3-mercaptopropionic acid and azobisisobutyronitrile is 100:14:8:0.15:0.2; the structural formula of the composite material is;
[0060] . Example 2
[0061] A method for preparing a powdered polycarboxylate water reducer: 110 parts of a polycarboxylate water reducer B with a solid content of 75% are taken, heated to 70°C, 2 parts of a composite material for preparing the powdered polycarboxylate water reducer and 8 parts of magnesium sulfate monohydrate are added, stirred evenly, cooled to room temperature, crushed and ground to obtain a powdered polycarboxylate water reducer.
[0062] The method for preparing a composite material of a powdered polycarboxylate water-reducing agent comprises the following steps:
[0063] Step 1: Set the specific surface area to 680m 2 / g silica gel is placed in a muffle furnace at 440℃ and dried for 9 hours, then cooled naturally to room temperature, and the silica gel activated at high temperature is added to a hydrochloric acid solution with a mass concentration of 15%, and the mass volume ratio of silica gel to hydrochloric acid solution is 1g:5mL. It is mechanically stirred at room temperature for 11 hours, and then washed with distilled water until neutral, and dried in a vacuum oven at 60℃ to constant weight to obtain acidified silica gel, thereby fully exposing the silanol groups on the surface of the silica gel to facilitate subsequent reactions;
[0064] Step 2: Add the acidified silica gel to the toluene solvent, ultrasonicate for 20 minutes to make it uniformly dispersed, then add γ-methacryloxypropyltrimethoxysilane, mechanically stir at 50°C, react for 10 hours to obtain SG-SCA suspension. The mass ratio of the acidified silica gel and the silane coupling agent containing unsaturated double bonds is 1:0.4, and the amount of the acidified silica gel and toluene is 1g:5mL;
[0065] Step 3: Stir and heat the SG-SCA suspension to 50°C, add azobisisoheptanonitrile, and simultaneously drop a mixed solution containing acrylic acid, acrylamide, magnesium acrylate, and 3-mercaptopropionic acid. The dropping time is 3 hours, followed by insulation for 1 hour, suction filtration, and the filter residue is dried in a vacuum oven at 60°C to constant weight, and then crushed and ground to obtain a composite material for preparing a powdered polycarboxylic acid water reducer; the mass ratio of SG-SCA, acrylic acid, acrylamide, magnesium acrylate, 3-mercaptopropionic acid and azobisisoheptanonitrile is 120:10:3:8:0.2:0.2; the structural formula of the composite material is:
[0066] . Example 3
[0067] A method for preparing a powdered polycarboxylate water reducer: 100 parts of a polycarboxylate water reducer C with a solid content of 70% are taken, heated to 70°C, 1 part of a composite material for preparing the powdered polycarboxylate water reducer and 10 parts of sodium carbonate are added, stirred evenly, cooled to room temperature, crushed and ground to obtain a powdered polycarboxylate water reducer.
[0068] The method for preparing a composite material of a powdered polycarboxylate water-reducing agent comprises the following steps:
[0069] Step 1: Set the specific surface area to 650m 2 / g silica gel is placed in a muffle furnace at 450℃ and dried for 8h, then cooled naturally to room temperature, and the silica gel after high temperature activation is added into a hydrochloric acid solution with a mass concentration of 25%, and the mass volume ratio of silica gel to hydrochloric acid solution is 1g:5mL, and mechanically stirred at room temperature for 10h, and then washed with distilled water to neutrality, and dried in a vacuum oven at 60℃ to constant weight to obtain acidified silica gel, thereby fully exposing the silanol groups on the surface of silica gel to facilitate subsequent reactions, and the amount of acidified silica gel and toluene is 1g:5mL;
[0070] Step 2: Add the acidified silica gel to the toluene solvent, ultrasonicate for 20 minutes to make it uniformly dispersed, then add vinyl trimethoxysilane, mechanically stir at 50°C, react for 11 hours to obtain SG-SCA suspension. The mass ratio of the acidified silica gel to the silane coupling agent containing unsaturated double bonds is 1:0.1;
[0071] Step 3: Stir and heat the SG-SCA suspension to 70°C, add dimethyl azobisisobutyrate, and simultaneously drop a mixed solution containing methacrylic acid, magnesium methacrylate, and mercaptoethanol. The dropping time is 2 hours, followed by insulation for 1 hour, suction filtration, and the filter residue is dried in a vacuum oven at 60°C to constant weight, and then crushed and ground to obtain a composite material for preparing a powdered polycarboxylate water reducer; the mass ratio of SG-SCA, methacrylic acid, magnesium methacrylate, mercaptoethanol, and dimethyl azobisisobutyrate is 150:13:6:0.1:0.2; the structural formula of the composite material is:
[0072] . Example 4
[0073] A method for preparing a powdered polycarboxylate water reducer: 90 parts of a polycarboxylate water reducer D with a solid content of 65% are taken, heated to 70°C, 3 parts of a composite material for preparing the powdered polycarboxylate water reducer and 6 parts of sodium thiosulfate are added, stirred evenly, cooled to room temperature, crushed and ground to obtain a powdered polycarboxylate water reducer.
[0074] The method for preparing a composite material of a powdered polycarboxylate water-reducing agent comprises the following steps:
[0075] Step 1: Set the specific surface area to 720m 2 / g silica gel is placed in a muffle furnace at 460℃ and dried for 7h, then cooled naturally to room temperature, and the silica gel after high temperature activation is added to a hydrochloric acid solution with a mass concentration of 20%, and the mass volume ratio of silica gel to hydrochloric acid solution is 1g:5mL. It is mechanically stirred at room temperature for 12h, then washed with distilled water until neutral, and dried in a vacuum oven at 60℃ to constant weight to obtain acidified silica gel, thereby fully exposing the silanol groups on the surface of the silica gel to facilitate subsequent reactions;
[0076] Step 2: Add the acidified silica gel to the toluene solvent, ultrasonicate for 20 minutes to make it uniformly dispersed, then add vinyl triethoxysilane, mechanically stir at 50°C, react for 12 hours to obtain SG-SCA suspension. The mass ratio of the acidified silica gel and the silane coupling agent containing unsaturated double bonds is 1:0.2, and the amount of the acidified silica gel and toluene is 1g:5mL;
[0077] Step 3: Stir and heat the SG-SCA suspension to 65°C, add dimethyl azobisisobutyrate, and simultaneously drop a mixed solution containing methacrylic acid, magnesium acrylate, and mercaptoethanol. The dropping time is 2.5 hours, followed by insulation for 1 hour, suction filtration, and the filter residue is dried in a vacuum oven at 60°C to constant weight, and then crushed and ground to obtain a composite material for preparing a powdered polycarboxylate water reducer; the mass ratio of SG-SCA, methacrylic acid, magnesium acrylate, mercaptoethanol, and dimethyl azobisisobutyrate is 75:10:5:0.2:0.2; the structural formula of the composite material is:
[0078] . Example 5
[0079] A method for preparing a powdered polycarboxylate water reducer: 80 parts of a polycarboxylate water reducer E with a solid content of 60% are taken, heated to 70°C, 4 parts of a composite material for preparing the powdered polycarboxylate water reducer and 7 parts of magnesium sulfate monohydrate are added, stirred evenly, cooled to room temperature, crushed and ground to obtain a powdered polycarboxylate water reducer.
[0080] The method for preparing a composite material of a powdered polycarboxylate water-reducing agent comprises the following steps:
[0081] Step 1: Set the specific surface area to 800m 2 / g silica gel is placed in a muffle furnace at 450℃ and dried for 8h, then cooled naturally to room temperature, and the silica gel after high temperature activation is added into a hydrochloric acid solution with a mass concentration of 20%, and the mass volume ratio of silica gel to hydrochloric acid solution is 1g:5mL, and mechanically stirred at room temperature for 12h, and then washed with distilled water to neutrality, and dried in a vacuum oven at 60℃ to constant weight to obtain acidified silica gel, thereby fully exposing the silanol groups on the surface of the silica gel to facilitate subsequent reactions;
[0082] Step 2: Add the acidified silica gel to the toluene solvent, ultrasonicate for 20 minutes to make it uniformly dispersed, then add vinyl tri(2-methoxyethoxy)silane, mechanically stir at 50°C, and react for 12 hours to obtain SG-SCA suspension. The mass ratio of the acidified silica gel and the silane coupling agent containing unsaturated double bonds is 1:0.3, and the amount of the acidified silica gel and toluene is 1g:5mL;
[0083] Step 3: Stir and heat the SG-SCA suspension to 60°C, add azobisisobutyronitrile, and simultaneously drop a mixed solution containing acrylic acid, methacrylic acid, magnesium acrylate, and 3-mercaptopropionic acid. The dropping time is 3 hours, followed by insulation for 1 hour, suction filtration, and the filter residue is dried in a vacuum oven at 60°C to constant weight, and then crushed and ground to obtain a composite material for preparing a powdered polycarboxylic acid water reducer; the mass ratio of SG-SCA, acrylic acid, methacrylic acid, magnesium acrylate, 3-mercaptopropionic acid and azobisisobutyronitrile is 50:8:2:6:0.15:0.2; the structural formula of the composite material is:
[0084] . Example 6
[0085] A preparation method of a powdered polycarboxylate water reducer: 80 parts of a polycarboxylate water reducer F with a solid content of 50% are taken, heated to 70°C, 5 parts of a composite material for preparing the powdered polycarboxylate water reducer and 10 parts of anhydrous magnesium sulfate are added, stirred evenly, cooled to room temperature, crushed and ground to obtain a powdered polycarboxylate water reducer.
[0086] The method for preparing a composite material of a powdered polycarboxylate water-reducing agent comprises the following steps:
[0087] Step 1: Set the specific surface area to 760m 2 / g silica gel is placed in a muffle furnace at 450℃ and dried for 8h, then cooled naturally to room temperature, and the silica gel after high temperature activation is added into a hydrochloric acid solution with a mass concentration of 20%, and the mass volume ratio of silica gel to hydrochloric acid solution is 1g:5mL, and mechanically stirred at room temperature for 12h, and then washed with distilled water to neutrality, and dried in a vacuum oven at 60℃ to constant weight to obtain acidified silica gel, thereby fully exposing the silanol groups on the surface of the silica gel to facilitate subsequent reactions;
[0088] Step 2: Add the acidified silica gel to the toluene solvent, ultrasonicate for 20 minutes to make it uniformly dispersed, then add γ-methacryloxypropyltrimethoxysilane, mechanically stir at 50°C, react for 12 hours to obtain SG-SCA suspension. The mass ratio of the acidified silica gel and the silane coupling agent containing unsaturated double bonds is 1:0.4, and the amount of the acidified silica gel and toluene is 1g:5mL;
[0089] Step 3: Stir and heat the SG-SCA suspension to 55°C, add azobisisoheptanonitrile, and simultaneously drop a mixed solution containing acrylic acid, magnesium methacrylate, and mercaptoethanol. The dropping time is 4 hours, followed by insulation for 1 hour, suction filtration, and the filter residue is dried in a vacuum oven at 60°C to constant weight, and then crushed and ground to obtain a composite material for preparing a powdered polycarboxylate water reducer; the mass ratio of SG-SCA, acrylic acid, magnesium methacrylate, mercaptoethanol, and azobisisoheptanonitrile is 110:15:10:0.2:0.2; the structural formula of the composite material is:
[0090] . Comparative Example 1
[0091] A method for preparing a powdered polycarboxylate water reducer comprises the following steps: taking 80 parts of a polycarboxylate water reducer F having a solid content of 50%, heating the mixture to 70°C, adding 6 parts of a composite material for preparing the powdered polycarboxylate water reducer, stirring the mixture evenly, cooling the mixture to room temperature, crushing the mixture, and grinding the mixture to obtain the powdered polycarboxylate water reducer.
[0092] Wherein, the preparation method of the composite material for preparing the powdered polycarboxylic acid water-reducing agent is the same as that in Example 6. Comparative Example 2
[0093] A preparation method of a powdered polycarboxylate water reducer: 80 parts of a polycarboxylate water reducer F with a solid content of 50% are taken, heated to 70°C, 30 parts of anhydrous magnesium sulfate are added, stirred evenly, cooled to room temperature, crushed and ground to obtain a powdered polycarboxylate water reducer. Comparative Example 3
[0094] A preparation method of a polycarboxylate water reducer: 80 parts of a polycarboxylate water reducer F with a solid content of 50% are taken, heated to 70°C, 5 parts of a commercially available super absorbent resin are added, stirred evenly, and after cooling to room temperature, a viscous paste state is formed. Comparative Example 4
[0095] A preparation method of a powdered polycarboxylate water reducer: 80 parts of a polycarboxylate water reducer F with a solid content of 50% are taken, heated to 70°C, 5 parts of a composite material for preparing the powdered polycarboxylate water reducer and 10 parts of anhydrous magnesium sulfate are added, stirred evenly, cooled to room temperature, crushed and ground to obtain a powdered polycarboxylate water reducer.
[0096] The method for preparing a composite material of a powdered polycarboxylate water-reducing agent comprises the following steps:
[0097] Step 1: Set the specific surface area to 760m 2 / g silica gel is placed in a muffle furnace at 450℃ and dried for 8h, then cooled naturally to room temperature, and the silica gel after high temperature activation is added into a hydrochloric acid solution with a mass concentration of 20%, and the mass volume ratio of silica gel to hydrochloric acid solution is 1g:5mL, and mechanically stirred at room temperature for 12h, and then washed with distilled water to neutrality, and dried in a vacuum oven at 60℃ to constant weight to obtain acidified silica gel, thereby fully exposing the silanol groups on the surface of the silica gel to facilitate subsequent reactions;
[0098] Step 2: Add the acidified silica gel to the toluene solvent, ultrasonicate for 20 minutes to make it uniformly dispersed, then add γ-methacryloxypropyltrimethoxysilane, mechanically stir at 50°C, react for 12 hours to obtain SG-SCA suspension. The mass ratio of acidified silica gel to γ-methacryloxypropyltrimethoxysilane is 1:0.4, and the amount of acidified silica gel and toluene is 1g:5mL;
[0099] Step 3: Stir and heat the SG-SCA suspension to 55°C, add azobisisoheptanonitrile, and simultaneously drop a mixed solution containing acrylic acid and mercaptoethanol. The dropping time is 4 hours, followed by insulation for 1 hour, suction filtration, and the filter residue is dried in a vacuum oven at 60°C to constant weight, and then crushed and ground to obtain a composite material for preparing a powdered polycarboxylic acid water reducer; the mass ratio of SG-SCA, acrylic acid, mercaptoethanol and azobisisoheptanonitrile is 110:19:0.2:0.2; the structural formula of the composite material is:
[0100] .
[0101] With reference to GB / T 8077-2023 "Test Method for Homogeneity of Concrete Admixtures", the polycarboxylate water-reducing agent solution before curing, the powdered polycarboxylate water-reducing agent samples obtained in Examples 1 to 6, and Comparative Examples 1 to 4 were tested for the fluidity of the slurry. The water-cement ratio was 0.29, and the water-reducing agent dosage was the solid dosage of the cementitious material. As can be seen from the table below, compared with the polycarboxylate water-reducing agent solution before curing, the dispersion and dispersion retention performance of Examples 1 to 6 prepared by this method are basically the same as before curing, indicating that the curing operation will not affect the water reduction and retention performance of the water-reducing agent.
[0102] .
[0103] Concrete performance test: Referring to GB8076-2008 "Concrete Admixtures", the polycarboxylate water-reducing agent solution before curing, the powdered polycarboxylate water-reducing agent samples obtained in Examples 1 to 6, and Comparative Examples 1 to 4 were tested for slump and time-dependent change, and compressive strength. The water-reducing agent dosage is the solid dosage of the cementitious material. As can be seen from Table 2 below, compared with the polycarboxylate water-reducing agent solution before curing, the dispersion, dispersion retention performance and compressive strength of Examples 1 to 6 prepared by this method in concrete are basically the same as before curing, indicating that the curing operation will not affect the water reduction and retention performance of the water-reducing agent and the concrete strength.
[0104] .
[0105] Shrinkage test: Referring to the contact method in GB / T 50082-2009 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete", shrinkage tests (contact method) were carried out on the polycarboxylate water-reducing agent solution before curing, the powder polycarboxylate water-reducing agent samples obtained in Examples 1 to 6, and Comparative Examples 1 to 4. The dosage and preparation of concrete specimens were the same as those for the concrete performance test. As can be seen from the table below, compared with the polycarboxylate water-reducing agent solution before curing, Examples 1 to 6 prepared by this method can significantly reduce the drying shrinkage of concrete.
[0106] .
[0107] Note: The unit of the values in the above table is 1×10 -6 .
[0108] Crushing and grinding test: Grinding test was carried out on polycarboxylate water reducer F with 50% solid content and Example 6 and Comparative Examples 1 to 4 using the water reducer solution for solidification. The results are shown in Table 4. Among them, comparative example 3 adds commercially available super absorbent resin for curing, and the sample obtained after cooling is in a paste state, and it is impossible to crush and grind to obtain a powder polycarboxylate water reducer; comparative example 1 only adds a composite material for preparing a powder polycarboxylate water reducer, and can be cured after cooling to room temperature, but the grinding performance is slightly lacking, and there is a phenomenon of sticky blocks; comparative example 2 only adds an inorganic salt that can generate a crystalline hydrate, although it can be cured and has good grinding performance, but due to the insufficient water absorption performance of the inorganic salt, the amount of addition is high, the content of the water reducer component in the sample is low, and it can be seen from the results of Table 3 that comparative example 2 cannot reduce the drying shrinkage of concrete; the composite material prepared in comparative example 4 cannot form an ion cross-linked polymer because magnesium acrylate or magnesium methacrylate monomers are not added, and the mechanical strength of the material after absorbing water is slightly poor. It is used in combination with an inorganic salt that can generate a crystalline hydrate, and can be cured after cooling to room temperature, but the grinding performance is slightly lacking, and there is a slight phenomenon of sticky blocks. While embodiment 6 can not only be cured, but also has high hardness and good grinding performance, and can also significantly reduce the drying shrinkage of concrete.
[0109] .
[0110] The detailed description of a composite material for preparing a powdered polycarboxylic acid water-reducing agent, a powdered polycarboxylic acid water-reducing agent and a preparation method with reference to the above-mentioned embodiments is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A method for preparing a composite material for preparing a powdered polycarboxylate water-reducing agent, characterized in that: The preparation method comprises the following steps: Step 1: Activate and acidify the silica gel at high temperature in sequence, and wash it to neutrality to obtain acidified silica gel; Step 2: dispersing the acidified silica gel in an organic solvent, adding a silane coupling agent containing an unsaturated double bond, stirring and reacting to obtain a suspension of modified silica gel; Step 3: Stirring and heating the suspension of modified silica gel to 50-70° C., adding an initiator, and dripping a mixed solution containing an unsaturated small monomer, an unsaturated salt monomer, and a chain transfer agent. After the dripping is completed, the mixture is kept warm for reaction. After the reaction is completed, the mixture is filtered, and the obtained residue is dried and ground to obtain a composite material for preparing a powdered polycarboxylic acid water reducer. The unsaturated small monomer is at least one of acrylic acid, methacrylic acid or acrylamide; the unsaturated salt monomer is magnesium acrylate or magnesium methacrylate; The structural formula of the composite material is: Wherein, R1 represents H or CH3; a=0 or 1, R2 represents COOCH2CH2CH2; R3 represents COOH or CONH2; Represents silica gel; x:y:z=2~6:7~10:
2.
2. The preparation method according to claim 1, characterized in that: The mass ratio of modified silica gel, unsaturated small monomer, unsaturated salt monomer, chain transfer agent and initiator is 50-150:10-15:5-10:0.1-0.2:0.
2.
3. The preparation method according to claim 1, characterized in that: In step 1, the specific surface area of the silica gel is 650 to 800 m 2 / g; the high temperature activation condition is heating at 440-460°C for 7-9h; the acidification condition is stirring in a hydrochloric acid solution with a mass concentration of 15-25% for 10-12h.
4. The preparation method according to claim 1, characterized in that: In step 2, the organic solvent is toluene; the silane coupling agent containing unsaturated double bonds is vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tri (2-methoxyethoxy) silane or γ-methacryloxypropyl trimethoxysilane; the mass ratio of the acidified silica gel to the silane coupling agent containing unsaturated double bonds is 1:0.1-0.4; The stirring reaction time is 10 to 12 hours.
5. The preparation method according to claim 1, characterized in that: In step three, the initiator is azobisisobutyronitrile, azobisisoheptanenitrile or dimethyl azobisisobutyrate; and the chain transfer agent is mercaptoethanol or 3-mercaptopropionic acid.
6. A composite material for preparing a powdered polycarboxylate water-reducing agent prepared by the preparation method according to any one of claims 1 to 5.
7. A powder polycarboxylate water reducer, characterized in that: The powdered polycarboxylate water reducer uses the composite material for preparing the powdered polycarboxylate water reducer according to claim 6 as a raw material.
8. The powdered polycarboxylate water-reducing agent according to claim 7, characterized in that: The powdered polycarboxylate water reducer is composed of the following raw materials in parts by weight: 80 to 120 parts of a polycarboxylate water reducer with a solid content of 50 to 80%, 1 to 5 parts of a composite material for preparing the powdered polycarboxylate water reducer, and 5 to 10 parts of an inorganic salt capable of generating a crystalline hydrate.
9. The powdered polycarboxylate water-reducing agent according to claim 8, characterized in that: The inorganic salt capable of forming a crystalline hydrate is any one or more of anhydrous magnesium sulfate, magnesium sulfate monohydrate, sodium carbonate, and sodium thiosulfate.
10. The method for preparing a powdered polycarboxylate water-reducing agent according to any one of claims 7 to 9, characterized in that: The preparation method comprises the following steps: heating a polycarboxylate water reducer with a solid content of 50 to 80% to 65 to 75° C., adding a composite material for preparing a powdered polycarboxylate water reducer and an inorganic salt capable of generating a crystalline hydrate, stirring evenly, cooling to room temperature, crushing and grinding to obtain a powdered polycarboxylate water reducer.