A kind of acid copper etching solution and preparation method thereof

By adding specific combinations of chemical substances to the liquid crystal panel etching solution, the combination of copper ions and chloride ions is prevented, and the problem of acidic copper etching solution remaining in complex channel structures is solved, achieving high-precision and low-pollution etching Effect.

CN118653152BActive Publication Date: 2024-11-22HEFEI SINOPISE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411149525.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The acidic copper etching liquid for existing liquid crystal panels is prone to etching residues in complex channel structures, affecting the cleanliness and circuit performance.

Method used

Using the use of copper chloride, hydrochloric acid, lanthanum chloride, sodium chloride, N,N-bis(2-pyridinyl)ethylenediamine, dithiourea modified chitosan, surfactant and azacronic ether Acid copper etching liquid prevents the binding of cuprous ions and chloride ions through chemical and physical action, forming a water-soluble complex and reducing channel residue.

Benefits of technology

It significantly reduces channel residue, ensures a moderate etching rate and appropriate etching angle, reduces the amount of side etching, improves the etching accuracy, and is simple and easy to prepare, easy to obtain raw materials, and has little environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118653152B_ABST
    Figure CN118653152B_ABST
Patent Text Reader

Abstract

The invention discloses an acidic copper etching solution and a preparation method thereof, and belongs to the technical field of metal surface chemical treatment. The acidic copper etching solution comprises the following raw materials in percentage by mass: 3-6% copper chloride, 5-10% hydrochloric acid, 0.5-1% lanthanum chloride, 1-3% sodium chloride, 2-3% ammonium chloride, 0.01-0.5% N,N-bis(2-pyridylmethyl)ethylenediamine, 2-5% dithiourea modified chitosan, 0.1-2% surfactant, 0.5-1.5% azacrown ether, 4-8% N,N-dimethylformamide, and the balance is deionized water. In the preparation process, the raw materials are mixed according to a proportion. When the acidic copper etching solution provided by the invention etches a liquid crystal panel, the side etching amount can be reduced, and the problem of residue after complex channel etching is avoided. In addition, the method for preparing the acidic copper etching solution provided by the invention is simple and easy to implement, the raw materials are easily available, and the environmental pollution is small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal surface chemical treatment, and in particular relates to an acidic copper etching solution and a preparation method thereof. Background Art

[0002] In the manufacturing process of the liquid crystal panel industry, precise etching of the metal layer is a key step to ensure the performance and appearance quality of the circuit. When the metal layer contains a combination of multiple metals such as copper, molybdenum and niobium, choosing a suitable etching system becomes particularly complex and important. First of all, considering that the hydrogen peroxide system has an extremely high etching rate due to its strong oxidizing property, it has an advantage when processing pure copper layers, but when it comes to copper-molybdenum-niobium alloys, too fast an etching rate may lead to non-selective attacks on the molybdenum and niobium layers, and even cause over-etching and interface damage between metal layers. Therefore, the hydrogen peroxide system is not suitable for this metal layer; and the alkaline etching system may destroy the chemical structure of the photoresist, causing pattern deformation or complete failure, making it impossible to accurately control the layout of the circuit.

[0003] The acidic copper chloride system uses copper chloride as an etchant, which can effectively and selectively etch the copper layer under acidic conditions while reducing damage to the molybdenum niobium layer. However, a large amount of copper ions will be generated during the etching process. The copper ions will react with the copper element on the surface to form cuprous ions, which will further combine with the chloride ions in the solution to form cuprous chloride precipitates. The cuprous chloride precipitates tend to adhere to the surface of the metal layer, especially in complex channel structures, forming etching residues that are difficult to remove. These residues will not only affect the cleanliness and appearance of the LCD panel, but may also introduce electrical performance problems such as resistance changes and signal interference, and in severe cases may even cause circuit failure. In addition, the channel residue phenomenon will also affect subsequent copper plating, welding and other process steps, further reducing the overall quality and reliability of the LCD panel.

[0004] At present, the patent application with publication number CN117858361A discloses a method for etching the outer layer of a thick copper plate, comprising the following steps: spraying an etching mixture on the thick copper plate at a spray temperature of 35-60°C and a spray pressure of 0.15-0.50MPa to obtain a thick copper plate to be cleaned, then washing the thick copper plate to be cleaned with running water for 2-3min, and then immersing it in deionized water for 0.5-1.0min and then taking it out to obtain an outer etched thick copper plate; wherein the etching mixture includes a weight ratio of (1050-1100): (4-5) etching solution and corrosion inhibitor, the etching solution is cupric chloride etching solution, the cupric chloride etching solution is cupric chloride dihydrate, hydrochloric acid and ammonium chloride, the corrosion inhibitor is one or more of benzotriazole, 2-mercaptobenzothiazole and hydroxyethylidene diphosphonic acid; the invention can make the etching degree of the middle area and the edge area of ​​the thick copper plate more balanced, but the acidic cupric chloride etching solution of the invention still cannot solve the channel residue problem caused by the existing acidic etching solution. Summary of the invention

[0005] The object of the present invention is to provide an acid copper etching solution and a preparation method thereof, so as to solve the problem that etching residues are easily generated when the etching solution for liquid crystal panels is used in a complex channel structure.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] An acidic copper etching solution comprises the following raw materials in percentage by mass: 3-6% cupric chloride, 5-10% hydrochloric acid, 0.5-1% lanthanum chloride, 1-3% sodium chloride, 2-3% ammonium chloride, 0.01-0.5% N,N-di(2-pyridylmethyl)ethylenediamine, 2-5% dithiourea modified chitosan, 0.1-2% surfactant, 0.5-1.5% azacrown ether, 4-8% N,N-dimethylformamide, and the balance is deionized water.

[0008] The acidic copper etching solution of the present invention comprises copper chloride, hydrochloric acid, lanthanum chloride, sodium chloride, ammonium chloride, N,N-di(2-pyridylmethyl)ethylenediamine, dithiourea-modified chitosan, surfactant, azacrown ether and N,N-dimethylformamide, wherein the copper chloride and hydrochloric acid mainly play an etching role, and the N,N-di(2-pyridylmethyl)ethylenediamine, dithiourea-modified chitosan, surfactant and azacrown ether hinder the interaction between a large number of cuprous ions and chloride ions by chemical and physical effects, and a small amount of cuprous ions still combine with chloride ions to form water-insoluble Cu2Cl2 solid, and the Cu2Cl2 solid will further complex with chloride ions provided by lanthanum chloride, sodium chloride and ammonium chloride to form water-soluble complex, thereby significantly reducing channel residues.

[0009] Preferably, the method for preparing the dithiourea modified chitosan comprises the following steps:

[0010] Chitosan, 1-ethyl-3-methylimidazole acetate and deionized water are uniformly mixed to obtain a chitosan solution; dithiourea is added to the chitosan solution, and stirred at 40-60°C for 0.5-1h, and then cinnamaldehyde is added, and the reaction is continued at a constant temperature with stirring for 4-6h, and the pH value is adjusted to 10-12 to form a precipitate, which is filtered, washed, and dried to obtain dithiourea-modified chitosan.

[0011] Preferably, the mass ratio of chitosan, 1-ethyl-3-methylimidazole acetate, deionized water, dithiourea and cinnamaldehyde is (0.5-2): (6-8): (100-200): (3-5): (2-4).

[0012] During the dissolution process of chitosan, 1-ethyl-3-methylimidazole acetate can destroy the hydrogen bonding within and between chitosan molecules, and has a better dissolution effect on chitosan; then, chitosan and dithiourea are cross-linked with cinnamaldehyde to form dithiourea-modified chitosan; dithiourea-modified chitosan can preferentially complex with cuprous ions, which can effectively reduce the combination of chloride ions and cuprous ions, avoid the formation of insoluble solid particles, and thus reduce channel residues; on the other hand, a protective film is formed on the surface of copper, which inhibits the corrosion of metallic copper in a physical barrier way, regulates the etching rate, and improves the side etching phenomenon.

[0013] Preferably, the surfactant is polyethylene glycol with a molecular weight of 400-6000, more preferably, the surfactant is polyethylene glycol with a molecular weight of 4000.

[0014] The surfactant can evenly disperse the components of the etching solution and maintain the stability of the etching solution. At the same time, in the early stage of etching, it is adsorbed on the surface of the metal copper to slow down the diffusion rate of ions in the etching solution and reduce the attack intensity of the etching solution on the metal layer. In the later stage of etching, the surfactant layer forms a double-layer membrane structure through adsorption with the complex formed by dithiourea-modified chitosan and cuprous ions. The two synergize to further hinder the combination of chloride ions and cuprous ions. After etching, it is washed with deionized water. Due to the osmotic pressure difference on both sides of the membrane, water molecules enter the inner side of the double-layer membrane. Under the action of water pressure, the double-layer membrane is smoothly separated from the metal surface, which significantly reduces the etching residue on the metal surface.

[0015] Polyethylene glycols with different molecular weights are preferred, which not only facilitates the polyethylene glycol to be better dissolved in the etching solution, but also ensures that the polyethylene glycol forms a stable micelle structure in the etching solution, showing stronger surface activity.

[0016] Preferably, the aza crown ether is 1-aza-15-crown-5 and / or 1,7-diaza-15-crown-5. More preferably, the aza crown ether is composed of 1-aza-15-crown-5 and 1,7-diaza-15-crown-5 in a mass ratio of (2 to 6):3.

[0017] The azacrown ether coordinates with the rare earth lanthanum ion to form a larger conjugated ring that can absorb a large amount of energy. During the etching process, the conjugated ring can isolate the interaction between the cuprous ions and the chloride ions, thereby reducing the etching residue by inhibiting the formation of cuprous chloride precipitation. Further, a mixture of 1-aza-15-crown-5 and 1,7-diaza-15-crown-5 in a specific mass ratio is preferably used as the azacrown ether. The two synergize to enable the conjugated ring to better prevent the combination between the cuprous ions and the chloride ions.

[0018] Preferably, the hydrochloric acid is a 37 wt % hydrochloric acid solution.

[0019] A method for preparing an acidic copper etching solution comprises the following steps:

[0020] Take the raw materials according to the formula, first mix N,N-di(2-pyridylmethyl)ethylenediamine, azacrown ether, N,N-dimethylformamide and deionized water evenly, heat to 35-45°C, stir for 1-2h, then add copper chloride, hydrochloric acid, lanthanum chloride, sodium chloride, ammonium chloride, dithiourea modified chitosan and surfactant, keep stirring at the same temperature for 1-2h to obtain an acidic copper etching solution.

[0021] Beneficial effects of the present invention:

[0022] When the acid copper etching solution provided by the invention etches a liquid crystal panel, the problem of residues after complex channel etching is avoided, and a moderate etching rate and a suitable etching angle are ensured, the amount of side etching is reduced, and the etching precision is improved. In addition, the method for preparing the acid copper etching solution provided by the invention is simple and easy, the raw materials are easily available, and the environmental pollution is small.

[0023] The present invention controls the mass fraction of each component within a certain range, which can not only significantly improve the channel residue phenomenon but also maintain an excellent etching effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention will be further described below in conjunction with the accompanying drawings.

[0025] Figure 1 This is a SEM image of the etching effect of the acid copper etching solution of Example 1 of the present invention;

[0026] Figure 2 This is a SEM image of the etching effect of the acid copper etching solution of Example 2 of the present invention;

[0027] Figure 3 This is a SEM image of the etching effect of the acid copper etching solution of Example 3 of the present invention;

[0028] Figure 4 This is a SEM image of the etching effect of the acid copper etching solution in Comparative Example 1 of the present invention;

[0029] Figure 5 This is a SEM image of the etching effect of the acid copper etching solution of Comparative Example 2 of the present invention;

[0030] Figure 6 This is a SEM image of the etching effect of the acid copper etching solution of Comparative Example 3 of the present invention;

[0031] Figure 7 is an optical microscope image of the channel residue after etching with the acid copper etching solution in Example 1 of the present invention;

[0032] Figure 8 This is an optical microscope image of the channel residue after etching with the acid copper etching solution in Comparative Example 3 of the present invention;

[0033] Fig. 9 It is an optical microscope picture of a magnified part of the channel residue after etching with an acidic copper etching solution in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Preparation Example 1

[0036] Dithiourea modified chitosan is prepared by the following method:

[0037] 0.5 g of chitosan (CS, deacetylation degree ≥ 95%, viscosity 100-200 mPa·s), 6 g of 1-ethyl-3-methylimidazole acetate and 100 g of deionized water were mixed uniformly to obtain a chitosan solution; 3 g of dithiourea was added to the chitosan solution, stirred at 40°C for 0.5 h, and then 2 g of cinnamaldehyde was added, and the reaction was continued by stirring at a constant temperature for 4 h. The pH value was adjusted to 10 with sodium hydroxide to form a precipitate, which was filtered, washed and dried to obtain dithiourea-modified chitosan.

[0038] Preparation Example 2

[0039] Dithiourea modified chitosan is prepared by the following method:

[0040] 1 g of chitosan (CS, deacetylation degree ≥ 95%, viscosity 100-200 mPa·s), 7 g of 1-ethyl-3-methylimidazole acetate and 150 g of water were mixed uniformly to obtain a chitosan solution; 4 g of dithiourea was added to the chitosan solution, stirred at 50°C for 0.8 h, and then 3 g of cinnamaldehyde was added, and the reaction was continued with stirring at a constant temperature for 5 h. The pH value was adjusted to 11 with sodium hydroxide to form a precipitate, which was filtered, washed and dried to obtain dithiourea-modified chitosan.

[0041] Preparation Example 3

[0042] Dithiourea modified chitosan is prepared by the following method:

[0043] 2 g of chitosan (CS, deacetylation degree ≥ 95%, viscosity 100-200 mPa·s), 8 g of 1-ethyl-3-methylimidazole acetate and 200 g of water were mixed uniformly to obtain a chitosan solution; 5 g of dithiourea was added to the chitosan solution, stirred at 60°C for 1 h, and then 4 g of cinnamaldehyde was added, and the reaction was continued with stirring at a constant temperature for 6 h. The pH value was adjusted to 12 with sodium hydroxide to form a precipitate, which was filtered, washed and dried to obtain dithiourea-modified chitosan.

[0044] Example 1

[0045] An acidic copper etching solution comprises the following raw materials in percentage by weight: 3% cupric chloride, 10% hydrochloric acid (37wt% hydrochloric acid solution), 0.5% lanthanum chloride, 2% sodium chloride, 2% ammonium chloride, 0.02% N,N-di(2-pyridylmethyl)ethylenediamine, 4% dithiourea modified chitosan, 0.1% surfactant, 1% azacrown ether, 6% N,N-dimethylformamide, and the balance is deionized water;

[0046] Wherein, the dithiourea modified chitosan is prepared by Preparation Example 1; the surfactant is polyethylene glycol with a molecular weight of 400; the aza crown ether is 1-aza-15-crown-5;

[0047] The preparation method of the above-mentioned acid copper etching solution comprises the following steps:

[0048] Take the raw materials according to the formula, first mix N,N-di(2-pyridylmethyl)ethylenediamine, azacrown ether, N,N-dimethylformamide and deionized water evenly, heat to 35°C, stir for 1.5 hours, then add copper chloride, hydrochloric acid, lanthanum chloride, sodium chloride, ammonium chloride, dithiourea modified chitosan, and surfactant, maintain the same temperature and continue stirring for 1.5 hours to obtain an acidic copper etching solution.

[0049] Example 2

[0050] An acidic copper etching solution comprises the following raw materials in percentage by weight: 4.5% cupric chloride, 8% hydrochloric acid (37wt% hydrochloric acid solution), 0.8% lanthanum chloride, 2% sodium chloride, 2.5% ammonium chloride, 0.01% N,N-di(2-pyridylmethyl)ethylenediamine, 2% dithiourea modified chitosan, 1.5% surfactant, 0.5% azacrown ether, 4% N,N-dimethylformamide, and the balance is deionized water;

[0051] Wherein, the dithiourea modified chitosan is prepared by Preparation Example 2; the surfactant is polyethylene glycol with a molecular weight of 2000; the aza crown ether is 1,7-diaza-15-crown-5;

[0052] The preparation method of the above-mentioned acid copper etching solution comprises the following steps:

[0053] Take the raw materials according to the formula, first mix N,N-di(2-pyridylmethyl)ethylenediamine, azacrown ether, N,N-dimethylformamide, and deionized water evenly, heat to 35°C, stir for 1 hour, then add copper chloride, hydrochloric acid, lanthanum chloride, sodium chloride, ammonium chloride, dithiourea modified chitosan, and surfactant, maintain the same temperature and continue stirring for 1 hour to obtain an acidic copper etching solution.

[0054] Example 3

[0055] An acidic copper etching solution comprises the following raw materials in percentage by weight: 6% cupric chloride, 5% hydrochloric acid (37wt% hydrochloric acid solution), 1% lanthanum chloride, 3% sodium chloride, 3% ammonium chloride, 0.5% N,N-di(2-pyridylmethyl)ethylenediamine, 5% dithiourea modified chitosan, 2% surfactant, 1.5% azacrown ether, 8% N,N-dimethylformamide, and the balance is deionized water;

[0056] Wherein, dithiourea modified chitosan is prepared by Preparation Example 3; the surfactant is polyethylene glycol with a molecular weight of 6000; the aza crown ether is obtained by mixing 1-aza-15-crown-5 and 1,7-diaza-15-crown-5 in a mass ratio of 1:1;

[0057] The preparation method of the above-mentioned acid copper etching solution comprises the following steps:

[0058] Take the raw materials according to the formula, first mix N,N-di(2-pyridylmethyl)ethylenediamine, azacrown ether, N,N-dimethylformamide and deionized water evenly, heat to 45°C, stir for 2 hours, then add copper chloride, hydrochloric acid, lanthanum chloride, sodium chloride, ammonium chloride, dithiourea modified chitosan, and surfactant, maintain the same temperature and continue stirring for 2 hours to obtain an acidic copper etching solution.

[0059] Example 4

[0060] An acidic copper etching solution is different from Example 1 only in that the surfactant is polyethylene glycol with a molecular weight of 2000, and the other raw materials, parameters and preparation process are the same as Example 1.

[0061] Example 5

[0062] An acidic copper etching solution is different from Example 1 only in that the surfactant is polyethylene glycol with a molecular weight of 4000, and the other raw materials, parameters and preparation process are the same as Example 1.

[0063] Example 6

[0064] An acidic copper etching solution is different from Example 1 only in that the surfactant is polyethylene glycol with a molecular weight of 5000, and the other raw materials, parameters and preparation process are the same as Example 1.

[0065] Example 7

[0066] An acidic copper etching solution is different from Example 1 only in that the azacrown ether is 1,7-diaza-15-crown-5, and the other raw materials, parameters and preparation process are the same as Example 1.

[0067] Example 8

[0068] An acidic copper etching solution is different from Example 1 only in that the azacrown ether is a mixture of 1-aza-15-crown-5 and 1,7-diaza-15-crown-5 in a mass ratio of 2:3, and the other raw materials, parameters and preparation process are the same as Example 1.

[0069] Example 9

[0070] An acidic copper etching solution is different from Example 1 only in that the azacrown ether is a mixture of 1-aza-15-crown-5 and 1,7-diaza-15-crown-5 in a mass ratio of 5:3, and the other raw materials, parameters and preparation process are the same as Example 1.

[0071] Example 10

[0072] An acidic copper etching solution is different from Example 1 only in that the azacrown ether is a mixture of 1-aza-15-crown-5 and 1,7-diaza-15-crown-5 in a mass ratio of 2:1, and the other raw materials, parameters and preparation process are the same as Example 1.

[0073] Comparative Example 1

[0074] An acidic copper etching solution is different from Example 1 only in that an equal mass of dithiourea is used to replace dithiourea-modified chitosan, and the remaining raw materials, parameters and preparation process are the same as Example 1.

[0075] Comparative Example 2

[0076] An acidic copper etching solution is different from Example 1 only in that an equal mass of chitosan (CS, deacetylation degree ≥ 95%, viscosity 100-200 mPa·s) is used to replace the dithiourea modified chitosan, and the other raw materials, parameters and preparation process are the same as Example 1.

[0077] Comparative Example 3

[0078] An acidic copper etching solution is different from Example 1 only in that an equal amount of polyethylene glycol with a molecular weight of 400 is used to replace dithiourea modified chitosan, and the other raw materials, parameters and preparation process are the same as Example 1.

[0079] Comparative Example 4

[0080] An acidic copper etching solution is different from Example 1 only in that an equal mass of dithiourea-modified chitosan (prepared in Preparation Example 1) is used to replace polyethylene glycol with a molecular weight of 400, and the remaining raw materials, parameters and preparation process are the same as Example 1.

[0081] Comparative Example 5

[0082] An acidic copper etching solution is different from Example 1 only in that an equal mass of azacrown ether is used to replace lanthanum chloride, and the remaining raw materials, parameters and preparation process are the same as Example 1.

[0083] Comparative Example 6

[0084] An acidic copper etching solution is different from Example 1 only in that an equal mass of lanthanum chloride is used to replace the azacrown ether, and the other raw materials, parameters and preparation process are the same as Example 1.

[0085] The acid copper etching solutions obtained in Examples 1-10 and Comparative Examples 1-6 were subjected to performance tests, and the test process was as follows:

[0086] Etching effect: At 33°C, a thick copper substrate with a copper layer thickness of 6μm was etched using an etcher, and the Taper angle, CD Basis, and channel residue were observed by SEM. The specific test results are shown in Table 1 below;

[0087] Among them, each group of etching solutions etches fifty samples (3cm×3cm), and the number of samples with no channel residue accounts for 90-100%, that is, the channel residue situation is recorded as A; the number of samples with no channel residue accounts for 60-90%, that is, the channel residue situation is recorded as B; the number of samples with no channel residue accounts for 30-60%, that is, the channel residue situation is recorded as C; the number of samples with no channel residue accounts for 0-30%, that is, the channel residue situation is recorded as D;

[0088] In addition, the etching effect SEM images of Examples 1-3 and Comparative Examples 1-3 are shown as follows: Figure 1-6 As shown, the optical microscope images of Example 1 and Comparative Example 3 are as follows Figure 7 , 8 As shown, Fig. 9 It is a partial enlarged view of the channel residue of Comparative Example 3;

[0089] Table 1

[0090]

[0091] Combined with the data recorded in Table 1, it can be seen that the acid copper etching solution prepared in Examples 1-10 has better overall performance, and the specific analysis is as follows:

[0092] It can be seen from the test results of Example 1, Example 7, Example 8, and Example 9 that compared with using 1-aza-15-crown-5 or 1,7-diaza-15-crown-5 alone as an aza crown ether, the acidic copper etching solution prepared by using a mixture of 1-aza-15-crown-5 and 1,7-diaza-15-crown-5 as an aza crown ether has better performance;

[0093] It can be seen from the test results of Example 1, Example 4, Example 5, and Example 6 that the acidic copper etching solution prepared by using polyethylene glycol with a molecular weight of 4000 as a surfactant has better performance;

[0094] It can be seen from the test results of Example 1, Comparative Example 1 and Comparative Example 2 that, compared with the acidic copper etching solution prepared with dithiourea or chitosan as raw materials, the acidic copper etching solution prepared with dithiourea-modified chitosan has better performance, indicating that the dithiourea-modified chitosan in this case has an effect that dithiourea or chitosan cannot match;

[0095] From the test results of Example 1, Comparative Example 3 and Comparative Example 4, it can be seen that the performance of the acidic copper etching solution obtained by mixing dithiourea-modified chitosan and a surfactant is significantly better than that of the acidic copper etching solution using dithiourea-modified chitosan or a surfactant alone;

[0096] It can be seen from the test results of Example 1, Comparative Example 5 and Comparative Example 6 that the interaction between azacrown ether and lanthanum chloride is beneficial to improving the channel residual phenomenon;

[0097] Combination Figure 1-9 ,Depend on Figure 1-3 It is known that the acidic etching solution prepared in Examples 1-3 etches the thick copper substrate, and the etching surface is smooth, there is no residue in the channel, the side etching amount is small, and the etching angle is moderate; Figure 4-6 It is known that the acidic etching solution prepared in Comparative Examples 1-3 etches the thick copper substrate, leaving a large amount of residual foreign matter on the etching surface, and the amount of side etching is too large; Figure 7 , 8 9. It is known that after the acidic copper etching solution prepared in Example 1 etches the thick copper substrate, there is no residue in the channel, while after the acidic copper etching solution prepared in Comparative Example 3 etches the thick copper substrate, there is obvious residue in the channel;

[0098] In summary, the acidic copper etching solutions prepared in Examples 1-10 are more effective in improving the channel residue phenomenon than those in Comparative Examples 1-6, and have excellent etching effects and high etching precision.

[0099] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0100] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An acidic copper etching solution, characterized in that, The invention comprises the following raw materials in percentage by mass: 3-6% copper chloride, 5-10% hydrochloric acid, 0.5-1% lanthanum chloride, 1-3% sodium chloride, 2-3% ammonium chloride, 0.01-0.5% N,N-di(2-pyridylmethyl)ethylenediamine, 2-5% dithiourea modified chitosan, 0.1-2% surfactant, 0.5-1.5% azacrown ether, 4-8% N,N-dimethylformamide, and the balance is deionized water.

2. An acidic copper etching solution according to claim 1, characterized in that, The preparation method of the dithiourea modified chitosan comprises the following steps: Chitosan, 1-ethyl-3-methylimidazole acetate and deionized water are uniformly mixed to obtain a chitosan solution; dithiourea is added to the chitosan solution, and stirred at 40-60°C for 0.5-1h, and then cinnamaldehyde is added, and the reaction is continued at a constant temperature with stirring for 4-6h, and the pH value is adjusted to 10-12 to form a precipitate, which is filtered, washed, and dried to obtain dithiourea-modified chitosan.

3. An acidic copper etching solution according to claim 2, characterized in that, The mass ratio of chitosan, 1-ethyl-3-methylimidazole acetate, deionized water, dithiourea and cinnamaldehyde is (0.5-2): (6-8): (100-200): (3-5): (2-4).

4. An acidic copper etching solution according to claim 1, characterized in that, The surfactant is polyethylene glycol with a molecular weight of 400-6000.

5. An acidic copper etching solution according to claim 1, characterized in that, The surfactant is polyethylene glycol with a molecular weight of 4000.

6. An acidic copper etching solution according to claim 1, characterized in that, The aza crown ether is 1-aza-15-crown-5 and / or 1,7-diaza-15-crown-5.

7. An acidic copper etching solution according to claim 1, characterized in that, The azacrown ether is composed of 1-aza-15-crown-5 and 1,7-diaza-15-crown-5 in a mass ratio of (2-6):

3.

8. A method for preparing an acidic copper etching solution, characterized in that: Used to prepare the acid copper etching solution as described in any one of claims 1 to 7, comprising the following steps: Take the raw materials according to the formula, first mix N,N-di(2-pyridylmethyl)ethylenediamine, azacrown ether, N,N-dimethylformamide and deionized water evenly, heat to 35-45°C, stir for 1-2h, then add copper chloride, hydrochloric acid, lanthanum chloride, sodium chloride, ammonium chloride, dithiourea modified chitosan and surfactant, keep stirring at the same temperature for 1-2h to obtain an acidic copper etching solution.