Method for preparing composite substrate

By performing temperature-controlled bonding on the semiconductor substrate and preset internal stress treatment, warping and cracking problems caused by mismatch of the thermal expansion coefficient are solved, and the performance of the composite substrate and the yield of the semiconductor device are improved.

CN118658795BActive Publication Date: 2024-11-12SABERS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411132847.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

In the prior art, bond warping, cracking and crushing problems caused by mismatch of thermal expansion coefficients between semiconductor substrates affect the yield of semiconductor devices.

Method used

By controlling the temperature of the first and second substrates, they are bonded at a preset temperature below 0°C, and the first bond is heated to the working environment temperature to generate a preset internal stress to control the thermal expansion coefficient Warp and cracks caused by mismatch are preset in the substrate surface to control the temperature in different internal stress distributions.

Benefits of technology

It effectively avoids warping and cracks caused by thermal expansion coefficient mismatch of the bond, improves the performance of composite substrates, and improves the performance and yield of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118658795B_ABST
    Figure CN118658795B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of wafer bonding technology, and discloses a method for preparing a composite substrate. The method for preparing the composite substrate comprises: preparing a first substrate and a second substrate; controlling the temperature of the first substrate and the second substrate so that the temperature of the first substrate is T1 and the temperature of the second substrate is T2, wherein both T1 and T2 are less than 0°C; maintaining the temperature of the first substrate at T1 and the temperature of the second substrate at T2 to bond the two to form a first bonding body; heating the first bonding body to a first target temperature T0, and generating a first preset internal stress #imgabs0# at the bonding interface of the first substrate and the second substrate. The method for preparing the composite substrate provided by the present invention can effectively alleviate the warping and cracking of the bonding body caused by the mismatch of the thermal expansion coefficient, avoid the generation of fragments, and improve the performance of semiconductor devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wafer bonding, and in particular to a method for preparing a composite substrate. Background Art

[0002] Direct bonding technology enables wafers or chips of different materials to form covalent bonds through atomic-level contact, and then combine together to form a composite substrate. Direct bonding technology can enable the bonded body to achieve structural properties that are difficult to achieve with single-material wafers or traditional processing methods, and therefore has high application value in the fields of microelectronics, micro-electromechanical or multi-functional chip integration.

[0003] For direct bonding between materials with lower melting points or materials with large mismatch in thermal expansion coefficients, traditional high-temperature bonding methods are no longer applicable. Prior art has also developed a plasma-activated bonding process, which uses plasma to treat the bonding material surface before bonding at room temperature in a high vacuum environment, so that the material has a clean surface and dangling chemical bonds on the surface of the material. However, this bonding method has the problem of warping, cracking, or even breaking of the bonded body due to the mismatch in thermal expansion coefficients between semiconductor substrates, which brings difficulties to the processing of subsequent devices and affects the yield of semiconductor devices.

[0004] Therefore, there is an urgent need for a method for preparing a composite substrate to solve the above technical problems. Summary of the invention

[0005] Based on the above, the object of the present invention is to provide a method for preparing a composite substrate, which can effectively alleviate the warping and cracking of the bonding body caused by the mismatch of thermal expansion coefficients, avoid the generation of fragments, and improve the performance of semiconductor devices.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a composite substrate, comprising:

[0008] preparing a first substrate and a second substrate;

[0009] Controlling the temperature of the first substrate and the second substrate so that the temperature of the first substrate is T1 and the temperature of the second substrate is T2, wherein T1 and T2 are both less than 0° C.;

[0010] Maintaining the temperature of the first substrate at T1 and the temperature of the second substrate at T2 to bond the two to form a first bonding body;

[0011] The first bonding body is heated to a first target temperature T0, and a first preset internal stress is generated at the bonding interface between the first substrate and the second substrate. , wherein the first target temperature T0 is room temperature or the working environment temperature of the first bonding body;

[0012] The first preset internal stress The calculation formula is:

[0013] ;

[0014] Wherein, Y1 and Y2 are Young's modulus of the first substrate and the second substrate at temperature T0, respectively; and are the temperature-dependent linear expansion coefficients of the first substrate and the second substrate, respectively.

[0015] In some possible implementations, the method for preparing the composite substrate further includes:

[0016] Predetermining the first preset internal stress required in the first bonding body The value of

[0017] According to the first preset internal stress The calculation formula is used to find the difference between T1 and T2;

[0018] According to the difference between T1 and T2, the corresponding values ​​of T1 and T2 are selected.

[0019] In some possible implementations, for a single crystal substrate, its Young's modulus Y and linear expansion coefficient are It is estimated by the following formula:

[0020] ;

[0021] ;

[0022] in, is the Young’s modulus of the single crystal substrate along the axial direction; is the Young’s modulus of the single crystal substrate along the radial direction; is the linear expansion coefficient of the single crystal substrate along the axial direction; is the linear expansion coefficient of the single crystal substrate along the radial direction; , , , They are all empirical coefficients, ranging from 0 to 1.

[0023] In some possible implementations, the method for preparing the composite substrate further includes:

[0024] preparing a third substrate;

[0025] Controlling the temperature of the third substrate and the first bonding body so that the temperature of the third substrate is T3 and the temperature of the first bonding body is T4, wherein both T3 and T4 are less than 0° C.;

[0026] Maintaining the temperature of the third substrate at T3 and the temperature of the first bonding body at T4 to bond the two to form a second bonding body;

[0027] The second bonding body is heated to a second target temperature T0', and a second preset internal stress is generated at the bonding interface between the third substrate and the first bonding body. , wherein the second target temperature T0' is room temperature or the working environment temperature of the second bonding body;

[0028] The second preset internal stress The calculation formula is:

[0029] ;

[0030] ;

[0031] ;

[0032] ;

[0033] Wherein, Y3 is the Young's modulus of the third substrate at temperature T0'; is the temperature-dependent linear expansion coefficient of the third substrate.

[0034] In some possible implementations, in the second bonding body, the internal stress at the bonding interface between the first substrate and the second substrate becomes a third preset internal stress , The calculation formula is:

[0035] .

[0036] In some possible embodiments, N regions are preset within the substrate surface of the first substrate and / or the second substrate, and the first substrate and / or the second substrate are temperature-controlled in different zones to form different preset internal stress distributions within the first bonding body; wherein the temperature of each of the regions is less than 0°C, and N≥2.

[0037] In some possible implementations, among the preset internal stresses formed in the N regions, the difference between the maximum preset internal stress and the minimum preset internal stress is less than 10% of the maximum preset internal stress.

[0038] In some possible implementations, when the temperature of the first substrate and the second substrate is controlled, pressure is applied to both sides of the corresponding substrates at the same time, and the applied pressure is smaller than the bonding pressure.

[0039] The beneficial effects of the present invention are:

[0040] The preparation method of the composite substrate provided by the present invention controls the temperature of the first substrate and the second substrate before bonding, so that the first substrate and the second substrate are bonded at a preset temperature below 0°C, and then the first bonding body is heated to the working environment temperature, so that a first preset internal stress can be generated at the bonding interface of the first bonding body. The magnitude of the internal stress is controllable within a certain range, and is pre-applied to the first bonding body, so that the warping and cracking of the first bonding body caused by the mismatch of the thermal expansion coefficients between the substrates are controllable, and no fragments are generated, and the pre-applied internal stress will change the internal lattice spacing of the material near the bonding interface of the composite substrate, and correspondingly change the electronic band structure and density, thereby changing the mobility of the carriers, so that the performance of the device prepared later is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 is a flow chart of a method for preparing a composite substrate provided by an embodiment of the present invention;

[0042] Figure 2 It is a flow chart of another method for preparing a composite substrate provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0043] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only the parts related to the present invention, rather than all structures, are shown in the accompanying drawings.

[0044] In the description of the present invention, unless otherwise clearly specified and limited, the terms "connected", "connected", and "fixed" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0045] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0046] In the description of this embodiment, the terms "upper", "lower", "left", "right", etc., and the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of description and simplification of operation, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used to distinguish in the description and have no special meaning.

[0047] This embodiment provides a method for preparing a composite substrate, which is used to achieve low-temperature bonding between two substrates to solve the problem in the prior art that the bonded body is warped, cracked, or even broken due to mismatch in thermal expansion coefficients between different substrates.

[0048] like Figure 1 As shown, the method for preparing the composite substrate provided in this embodiment includes the following steps:

[0049] S1, preparing a first substrate and a second substrate;

[0050] The materials of the first substrate and the second substrate of this embodiment can be silicon, silicon carbide, lithium niobate, lithium tantalate, etc. Among them, lithium tantalate has excellent piezoelectric, ferroelectric, acousto-optic and electro-optic effects, and can be used for electronic communication devices such as resonators, filters, transducers, and high-frequency surface acoustic wave devices; lithium niobate has good nonlinear optical properties and can be used as an optical waveguide material, or used to make medium and low frequency surface acoustic wave filters, high-power high-temperature resistant ultrasonic transducers, etc. In addition, the first substrate and the second substrate of this embodiment can be single crystal substrates or polycrystalline substrates.

[0051] In an optional embodiment, the material of the first substrate is polycrystalline silicon carbide, and the material of the second substrate is single-crystalline silicon carbide, thereby realizing the bonding between the polycrystalline substrate and the single-crystalline substrate. In another optional embodiment, the material of the first substrate is silicon carbide, and the material of the second substrate is lithium niobate, thereby realizing the bonding between two substrates of different materials.

[0052] S2, controlling the temperature of the first substrate and the second substrate, so that the temperature of the first substrate is T1, and the temperature of the second substrate is T2, wherein T1 and T2 are both less than 0° C.;

[0053] In this embodiment, T1 and T2 can be independently set to -300°C to 0°C. Specifically, those skilled in the art can set the values ​​of T1 and T2 according to the different bonding surface materials. Exemplarily, a first support frame and a second support frame arranged relatively to each other can be provided, and the first support frame clamps and cools the first substrate, and the second support frame clamps and cools the second substrate. Furthermore, a first temperature measuring element can be set between the first support frame and the first substrate, and a second temperature measuring element can be set between the second substrate and the second support frame, so as to realize real-time monitoring of the temperature of the first substrate and the second substrate.

[0054] S3, maintaining the temperature of the first substrate at T1 and the temperature of the second substrate at T2 to bond the two substrates to form a first bonding body;

[0055] In this embodiment, the temperatures of the first substrate and the second substrate are set below 0°C before bonding, and the temperatures of the first substrate and the second substrate are kept unchanged during the bonding process, thereby achieving low-temperature bonding between the first substrate and the second substrate and improving the performance of the first bonding body. Exemplarily, the bonding pressure value during bonding can be set to 10N to 10000N, and the constant pressure is maintained for 1s to 1000s, thereby improving the bonding reliability of the first bonding body.

[0056] S4, heating the first bonding body to a first target temperature T0, generating a first preset internal stress at the bonding interface between the first substrate and the second substrate .

[0057] In this embodiment, the first target temperature T0 refers to the room temperature or the working environment temperature of the first bonding body. Specifically, a third support frame can be provided, and the first bonding body can be placed on the third support frame so as to heat the first bonding body. Exemplarily, the temperature of the third support frame can be configured to be -300°C to 50°C.

[0058] In this embodiment, the temperature of the first substrate and the second substrate is controlled before bonding, so that the first substrate and the second substrate are bonded at a preset temperature below 0°C, and then the first bonding body is heated to the working environment temperature, so that a first preset internal stress can be generated at the bonding interface of the first bonding body. The magnitude of the internal stress is controllable within a certain range, and is pre-applied to the first bonding body. Therefore, the warping and cracking of the first bonding body caused by the mismatch of the thermal expansion coefficients between the substrates are controllable, and no fragments will be generated. In addition, the pre-applied internal stress will change the internal lattice spacing of the material near the bonding interface of the composite substrate, and accordingly change the electronic band structure and density, thereby changing the carrier mobility, so that the performance of the device prepared later is improved.

[0059] Furthermore, in this embodiment, the first preset internal stress The calculation formula is:

[0060] ;

[0061] Wherein, Y1 and Y2 are Young's modulus of the first substrate and the second substrate at temperature T0, respectively; and are the temperature-dependent linear expansion coefficients of the first substrate and the second substrate, respectively.

[0062] It should be noted that the above Y1, Y2, and All of them can be obtained by measuring the material.

[0063] The technicians in this field can flexibly preset the required internal stress at the bonding interface of the first substrate and the second substrate through the above calculation formula, just by adjusting the corresponding values ​​of T1 and T2. The specific operation process is as follows: First, set the first preset internal stress required in the first bonding body in advance. Then, according to the first preset internal stress The calculation formula is used to infer the difference between T1 and T2; then, the corresponding values ​​of T1 and T2 are selected according to the difference between T1 and T2 and the specific working conditions of the first substrate and the second substrate.

[0064] In this embodiment, the first substrate and the second substrate may be single crystal substrates or polycrystalline substrates. For single crystal substrates, Young's modulus and linear expansion coefficients in different crystal directions within the bonding plane are significantly different, so it is necessary to use the correlation coefficient for estimation. In this embodiment, the Young's modulus Y and linear expansion coefficient of the single crystal substrate are It can be estimated by the following formula:

[0065] ;

[0066] ;

[0067] in, is the Young’s modulus of the single crystal substrate along the axial direction; is the Young’s modulus of the single crystal substrate along the radial direction; is the linear expansion coefficient of the single crystal substrate along the axial direction; is the linear expansion coefficient of the single crystal substrate along the radial direction; , , , They are all empirical coefficients, ranging from 0 to 1.

[0068] It should be noted that the above , , , All of them can be obtained by measuring the material.

[0069] Furthermore, to achieve the bonding between the first bonding body and the third substrate, as Figure 2 As shown, the method for preparing the composite substrate in this embodiment also includes the following steps:

[0070] S5, preparing a third substrate;

[0071] The material of the third substrate may be silicon, silicon carbide, lithium niobate, lithium tantalate, etc., and the third substrate may be a single crystal substrate or a polycrystalline substrate. In an optional embodiment, when the material of the first substrate is polycrystalline silicon carbide and the material of the second substrate is single crystal silicon carbide, the material of the third substrate may be single crystal silicon.

[0072] S6, controlling the temperature of the third substrate and the first bonding body, so that the temperature of the third substrate is T3, and the temperature of the first bonding body is T4, wherein T3 and T4 are both less than 0° C.;

[0073] In this embodiment, T3 and T4 can be independently set to -300°C to 0°C. Specifically, those skilled in the art can set the values ​​of T3 and T4 according to different bonding surface materials.

[0074] S7, maintaining the temperature of the third substrate at T3 and the temperature of the first bonding body at T4 to bond the two to form a second bonding body;

[0075] By setting the temperatures of the third substrate and the first bonding body to below 0°C before bonding, and keeping the temperatures of the third substrate and the first bonding body unchanged during the bonding process, low-temperature bonding between the third substrate and the first bonding body is achieved, thereby improving the performance of the first bonding body.

[0076] S8, heating the second bonding body to a second target temperature T0', generating a second preset internal stress at the bonding interface between the third substrate and the first bonding body .

[0077] In this embodiment, the second target temperature T0' refers to the room temperature or the working environment temperature of the second bonding body. In this embodiment, by controlling the temperatures of T3 and T4 below 0°C, low-temperature bonding of the third substrate and the first bonding body is achieved, and a second preset internal stress can be generated at the bonding interface between the first bonding body and the third substrate. , reducing defects such as warping and cracks of the second bonding body caused by the mismatch of thermal expansion coefficients between substrates, and effectively improving the performance of the second bonding body.

[0078] Furthermore, the second preset internal stress of this embodiment is The calculation formula is:

[0079] ;

[0080] ;

[0081] ;

[0082] ;

[0083] Wherein, Y3 is the Young's modulus of the third substrate at temperature T0'; is the temperature-dependent linear expansion coefficient of the third substrate.

[0084] It should be noted that the above Y3, All of them can be obtained by measuring the material.

[0085] In the above-mentioned second bonding body, the internal stress at the bonding interface between the first substrate and the second substrate becomes a third preset internal stress , The calculation formula is:

[0086] .

[0087] A person skilled in the art can set the third preset internal stress at the bonding interface between the first substrate and the second substrate in advance by using the above calculation formula: , and a second preset internal stress at the bonding interface between the third substrate and the first bonding body ; Then calculate the relationship between T1, T2, T3, and T4; and then select the corresponding values ​​of T1, T2, T3, and T4 according to the specific working conditions.

[0088] Since the preset internal stress required in different areas of the same bonding body is different, in order to further improve the performance of the composite substrate and improve its warping, in some embodiments, N (N≥2) areas can be preset in the substrate surface of the first substrate and / or the second substrate, and the first substrate and / or the second substrate can be zoned and temperature controlled, so as to form different preset internal stress distributions in the first bonding body. Among them, the temperature of each area is less than 0°C. The present invention avoids cutting multiple areas of the substrate for separate temperature control by zoned temperature control on the same substrate, simplifies the operation and improves the work efficiency. Exemplarily, the first substrate can be divided into three areas, and the second substrate is also divided into three corresponding areas, so that the preset internal stresses corresponding to the three target interfaces can be preset in advance, and then the corresponding T1 and T2 values ​​in the three areas can be calculated respectively. Of course, for the bonding of the first bonding body and the third substrate, the above-mentioned zoned temperature control method can also be used for low-temperature bonding.

[0089] Furthermore, among the preset internal stresses formed in the above-mentioned N regions, the difference between the maximum preset internal stress and the minimum preset internal stress should be less than 10% of the maximum preset internal stress. Such a setting can avoid the situation where the substrate warps and deforms due to the large difference between different preset internal stresses in the same bonding interface.

[0090] In addition, in this embodiment, when the temperature of the first substrate, the second substrate, the third substrate and the first bonding body is controlled, pressure can be applied to both sides of the corresponding substrate or bonding body at the same time, so that the warping of the substrate can be further suppressed. It should be noted that the pressure applied to the substrate or bonding body during the above temperature control process should be less than the bonding pressure during bonding.

[0091] The method of the present invention is described below by a specific embodiment:

[0092] First, a first substrate and a second substrate are provided, wherein the first substrate is silicon carbide and the second substrate is silicon;

[0093] The silicon carbide and the silicon wafer are temperature-controlled independently, wherein the silicon carbide temperature T1 = -200°C and the silicon temperature T2 = -50°C; the silicon carbide and the silicon are bonded while maintaining the above temperatures to form a first bonding body;

[0094] The first bonding body is heated to a first target temperature T0, wherein the first target temperature T0=20°C; a first preset internal stress generated at the bonding interface of silicon carbide and silicon Calculate using the following formula:

[0095] ;

[0096] in:

[0097] Thermal Expansion Coefficient of Silicon Carbide 4.4×10 -6 / K, basically independent of temperature; the Young's modulus Y1 of silicon carbide at 20°C is 480 GPa; the thermal expansion coefficient of silicon 2.6×10 -6 / K, basically independent of temperature; the Young's modulus Y2 of silicon at 20°C is 130 GPa;

[0098] The calculation shows that the first preset internal stress 8.04×10 7 N / m 2 .

[0099] Further, a third substrate is provided, wherein the third substrate is silicon oxide;

[0100] The silicon oxide and the first bonding body are temperature-controlled independently, so that the temperature of the silicon oxide is T3 = -20°C and the temperature of the first bonding body is T4 = -100°C; the silicon oxide and the first bonding body are bonded while maintaining the above temperatures to form a second bonding body;

[0101] The second bonding body is heated to a second target temperature T0', where the second target temperature T0'=20°C; a second preset internal stress is generated at the bonding interface between the silicon oxide and the first bonding body. Calculate using the following formula:

[0102] ;

[0103] in:

[0104] Thermal expansion coefficient of silicon oxide 0.54×10 -6 / K, which is basically independent of temperature; the Young's modulus Y3 of silicon oxide at 20°C is 70 GPa; K1=9.68×10 -4 ; K2=1.82×10 -4 ; K3=3.40×10 -4 ;

[0105] The calculation shows that the second preset internal stress 2.89×10 7 N / m 2 .

[0106] The internal stress of the bonding interface of silicon carbide and silicon becomes the third preset internal stress , Calculate using the following formula:

[0107] ;

[0108] The calculation shows that the third preset internal stress 1.03×10 8 N / m 2 .

[0109] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.

Claims

1. A method for preparing a composite substrate, characterized in that: include: preparing a first substrate and a second substrate; Controlling the temperature of the first substrate and the second substrate so that the temperature of the first substrate is T1 and the temperature of the second substrate is T2, wherein T1 and T2 are both less than 0° C.; Maintaining the temperature of the first substrate at T1 and the temperature of the second substrate at T2 to bond the two to form a first bonding body; The first bonding body is heated to a first target temperature T0, and a first preset internal stress is generated at the bonding interface between the first substrate and the second substrate. , wherein the first target temperature T0 is room temperature or the working environment temperature of the first bonding body; The first preset internal stress The calculation formula is: ; Wherein, Y1 and Y2 are Young's modulus of the first substrate and the second substrate at temperature T0, respectively; and are the temperature-dependent linear expansion coefficients of the first substrate and the second substrate, respectively.

2. The method for preparing a composite substrate according to claim 1, characterized in that: The method for preparing the composite substrate further includes: Predetermining the first preset internal stress required in the first bonding body The value of According to the first preset internal stress The calculation formula is used to find the difference between T1 and T2; According to the difference between T1 and T2, the corresponding values ​​of T1 and T2 are selected.

3. The method for preparing a composite substrate according to claim 2, characterized in that: For a single crystal substrate, its Young's modulus Y and linear expansion coefficient It is estimated by the following formula: ; ; in, is the Young’s modulus of the single crystal substrate along the axial direction; is the Young’s modulus of the single crystal substrate along the radial direction; is the linear expansion coefficient of the single crystal substrate along the axial direction; is the linear expansion coefficient of the single crystal substrate along the radial direction; , , , They are all empirical coefficients, ranging from 0 to 1.

4. The method for preparing a composite substrate according to any one of claims 1 to 3, characterized in that: The method for preparing the composite substrate further includes: preparing a third substrate; Controlling the temperature of the third substrate and the first bonding body so that the temperature of the third substrate is T3 and the temperature of the first bonding body is T4, wherein both T3 and T4 are less than 0° C.; Maintaining the temperature of the third substrate at T3 and the temperature of the first bonding body at T4 to bond the two to form a second bonding body; The second bonding body is heated to a second target temperature T0', and a second preset internal stress is generated at the bonding interface between the third substrate and the first bonding body. , wherein the second target temperature T0' is room temperature or the working environment temperature of the second bonding body; The second preset internal stress The calculation formula is: ; ; ; ; Wherein, Y3 is the Young's modulus of the third substrate at temperature T0'; is the temperature-dependent linear expansion coefficient of the third substrate.

5. The method for preparing a composite substrate according to claim 4, characterized in that: In the second bonding body, the internal stress of the bonding interface between the first substrate and the second substrate becomes a third preset internal stress , The calculation formula is: 。 6. The method for preparing a composite substrate according to claim 1, characterized in that: N regions are preset within the substrate surface of the first substrate and / or the second substrate, and the temperature of the first substrate and / or the second substrate is controlled in different zones to form different preset internal stress distributions within the first bonding body; wherein the temperature of each of the regions is less than 0°C, and N≥2.

7. The method for preparing a composite substrate according to claim 6, characterized in that: Among the preset internal stresses formed in the N regions, the difference between the maximum preset internal stress and the minimum preset internal stress is less than 10% of the maximum preset internal stress.

8. The method for preparing a composite substrate according to claim 1, characterized in that: When the temperature of the first substrate and the second substrate is controlled, pressure is applied to both sides of the corresponding substrates at the same time, and the applied pressure is smaller than the bonding pressure.