Low temperature bonding method

The low-temperature bonding method is used to cool and irradiate the sample in a vacuum chamber, which solves the problem of difficulty in bonding materials with low melting points or mismatched thermal expansion coefficients in traditional high-temperature bonding methods, and achieves internal stress control and control of the bonded body. Performance improvements.

CN118658796BActive Publication Date: 2024-10-29SABERS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411132848.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-10-29
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

Traditional high-temperature bonding methods are difficult to effectively bond materials with low melting points or mismatched thermal expansion coefficients, leading to bonded body warping problems, and it is impossible to pre-apply internal stress to improve the electronic band structure and carrier mobility.

Method used

Using the low-temperature bonding method, the samples to be bonded are independently cooled and irradiated in a vacuum chamber to form a low-temperature bonded body, and internal stress is pre-applied during the bonding process to control the bonding temperature below 0°C to ensure The bonded body has controllable internal stress at room temperature or working environment temperature.

Benefits of technology

It effectively alleviates the warping problem of the bonded body caused by the mismatch of thermal expansion coefficient. The pre-imposed internal stress changes the lattice spacing and electronic band structure of the material, improving the carrier mobility and device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118658796B_ABST
    Figure CN118658796B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of wafer bonding technology, and discloses a low-temperature bonding method. The low-temperature bonding method comprises: A: providing a cavity, placing a first sample and a second sample to be bonded in the cavity; B: performing independent cooling treatment on the first sample and the second sample, so that the temperature of the first sample is T1, and the temperature of the second sample is T2; the temperatures T1 and T2 are respectively below 0°C; C: evacuating the cavity, so that the vacuum degree in the cavity reaches a predetermined value; D: performing irradiation treatment on the first sample and the second sample, so that the surfaces of the first sample and the second sample are activated; E: bonding the first sample and the second sample to form a first bonding body; during bonding, the temperature of the first sample is T3, and the temperature of the second sample is T4; T3 and T4 are respectively below 0°C. The low-temperature bonding method provided by the present invention can effectively improve device performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wafer bonding, and in particular to a low-temperature bonding method. Background Art

[0002] Direct bonding technology enables wafers or chips of different materials to form covalent bonds through atomic-level contact and then bond together. Direct bonding technology enables the bonded body to achieve structural properties that are difficult to achieve with single-material wafers or traditional processing methods, and therefore has high application value in the fields of microelectronics, micro-electromechanical or multi-functional chip integration.

[0003] If you want to directly bond materials with low melting points or materials with large thermal expansion coefficient mismatch, the traditional high-temperature bonding method is no longer applicable. The prior art has developed a plasma activated bonding process, that is, before bonding at room temperature in a high vacuum environment, plasma is used to treat the surface of the bonding material to produce a clean surface and create hanging chemical bonds on the surface of the material. However, the bonded body prepared by this bonding method has the problem of warping due to thermal expansion coefficient mismatch.

[0004] Therefore, a low-temperature bonding method is urgently needed to solve the above technical problems. Summary of the invention

[0005] The purpose of the present invention is to provide a low-temperature bonding method, which can achieve low-temperature bonding of samples and effectively alleviate the warping of the bonded body caused by the mismatch of thermal expansion coefficients; and the low-temperature bonding can pre-apply internal stress inside the bonded body. The pre-applied internal stress will change the lattice spacing inside the material, and correspondingly change the electronic energy band structure and density, thereby changing the carrier mobility, so that the performance of the device prepared later is improved.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] Low temperature bonding methods, including:

[0008] A: providing a cavity, placing a first sample and a second sample to be bonded in the cavity;

[0009] B: performing independent cooling treatment on the first sample and the second sample, so that the temperature of the first sample is T1, and the temperature of the second sample is T2; and T1 and T2 are respectively below 0°C;

[0010] C: evacuating the cavity so that the vacuum degree in the cavity reaches a predetermined value;

[0011] D: irradiating the first sample and the second sample to activate the surfaces of the first sample and the second sample;

[0012] E: Bonding the first sample and the second sample to form a first bonded body; during bonding, the temperature of the first sample is T3, and the temperature of the second sample is T4; T3 and T4 are respectively below 0°C.

[0013] Optionally, between step A and step B, there is further included step A1: vacuuming the cavity.

[0014] Optionally, between step A and step B, step A1 is further included: vacuuming the cavity and then backfilling with dry gas.

[0015] Optionally, the T1, the T2, the T3, and the T4 are independently set to -300°C to 0°C.

[0016] Optionally, the absolute value of the temperature difference between T1 and T3 is less than 10°C; the absolute value of the temperature difference between T2 and T4 is less than 10°C.

[0017] Optionally, in step C, the predetermined value of the vacuum degree is less than 0.1 Pa.

[0018] Optionally, in step E, during bonding, the bonding pressure value is 10N to 10000N, and the constant pressure is maintained for 1s to 1000s.

[0019] Optionally, after step E, the first bonding body is further subjected to a heating treatment so that the temperature of the first bonding body reaches room temperature.

[0020] Optionally, the step A further includes: providing a third sample; and after step E, further includes: bonding the first bonding body to the third sample to form a second bonding body.

[0021] Optionally, the low temperature bonding method is performed using a low temperature bonding device, and the low temperature bonding device includes:

[0022] Cavity;

[0023] A support frame is installed in the cavity. There are three support frames, namely a first support frame, a second support frame and a third support frame. The first support frame and the second support frame are arranged opposite to each other. The first support frame is used to clamp and cool the first sample, the second support frame is used to clamp and cool the second sample, and the third support frame is used to carry the bonding body. The temperature of the third support frame is selectively configured at -300°C to 50°C.

[0024] A robot arm is disposed in the cavity and is used for transferring the bonding body between the second support frame and the third support frame.

[0025] Beneficial effects of the present invention: The low-temperature bonding method provided by the present invention can realize low-temperature bonding between samples or between samples and a bonding body. Low-temperature bonding refers to a bonding temperature below 0°C. During bonding, different T1~T4 are set according to different materials of the bonding surfaces, so that when the bonding body is restored to room temperature or working environment temperature, an expected internal stress is generated inside the bonding body. The magnitude of the internal stress is controllable within a certain range and pre-applied to the bonding body. Therefore, the warping of the bonding body caused by stress is controllable and no fragments will be generated. In addition, the pre-applied internal stress will change the lattice spacing inside the sample material, and correspondingly change the electronic energy band structure and density, thereby changing the carrier mobility, thereby improving the performance of the device prepared later. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a flow chart of a low temperature bonding method provided by an embodiment of the present invention;

[0027] Figure 2 is a schematic structural diagram of a low-temperature bonding device provided in an embodiment of the present invention;

[0028] Figure 3 It is a structural schematic diagram of the low-temperature bonding equipment provided in an embodiment of the present invention during sample bonding processing.

[0029] In the figure:

[0030] 100, cavity;

[0031] 210, first support frame; 220, second support frame; 230, first gas circulation channel;

[0032] 300, first sample;

[0033] 400, second sample;

[0034] 510, ion source; 520, shell; 521, second gas circulation channel; 530, ion beam. DETAILED DESCRIPTION

[0035] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.

[0036] In the description of the present invention, unless otherwise clearly specified and limited, the terms "connected", "connected", and "fixed" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0037] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0038] In the description of this embodiment, the terms "upper", "lower", "right", etc., directions or positional relationships are based on the directions or positional relationships shown in the drawings, and are only for the convenience of description and simplification of operation, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used to distinguish in the description and have no special meaning.

[0039] This embodiment provides a low-temperature bonding method, which can achieve low-temperature bonding of samples and can effectively alleviate the warping of the bonded body caused by the mismatch of thermal expansion coefficients; and low-temperature bonding can pre-apply internal stress inside the bonded body. The pre-applied internal stress will change the lattice spacing inside the material, and correspondingly change the electronic energy band structure and density, thereby changing the carrier mobility, thereby improving the performance of the device prepared later.

[0040] like Figure 1 As shown, the low temperature bonding method comprises the following steps:

[0041] A: providing a cavity 100, placing a first sample 300 and a second sample 400 to be bonded in the cavity 100;

[0042] B: The first sample 300 and the second sample 400 are subjected to independent cooling treatment, so that the temperature of the first sample 300 is T1 and the temperature of the second sample 400 is T2; the temperatures T1 and T2 are respectively below 0°C;

[0043] C: evacuating the cavity 100 so that the vacuum degree in the cavity 100 reaches a predetermined value;

[0044] D: performing irradiation treatment on the first sample 300 and the second sample 400 to activate the surfaces of the first sample 300 and the second sample 400;

[0045] E: The first sample 300 and the second sample 400 are bonded to form a first bonded body; during bonding, the temperature of the first sample 300 is T3, and the temperature of the second sample 400 is T4; T3 and T4 are respectively below 0°C.

[0046] The low-temperature bonding method provided in this embodiment can realize low-temperature bonding between samples or between samples and bonding bodies. Low-temperature bonding refers to a bonding temperature below 0°C. During bonding, different T1~T4 are set according to the different materials of the bonding surfaces, so that when the bonding body is restored to room temperature or working environment temperature, an expected internal stress is generated inside the bonding body. The magnitude of the internal stress is controllable within a certain range and pre-applied to the bonding body. Therefore, the warping of the bonding body caused by stress is controllable and no fragments will be generated. In addition, the pre-applied internal stress will change the lattice spacing inside the sample material, and correspondingly change the electronic band structure and density, thereby changing the carrier mobility, thereby improving the performance of the device prepared later.

[0047] Optionally, step A1 is further included between step A and step B: vacuumizing the cavity 100. After the sample is cooled to below 0°C, if there is gas in the cavity 100, water will condense on the surface of the sample. If condensed water is not desired on the surface of the sample during bonding, the cavity 100 needs to be vacuumized before cooling the sample.

[0048] Alternatively, step A1 is also included between step A and step B: after vacuuming the cavity 100, backfilling with dry gas (such as dry air or high-purity nitrogen, etc.). Before cooling the sample, if you do not want too much condensed water to be generated on the surface of the sample during bonding, you need to first vacuum the cavity 100 before cooling the sample, and then backfill with dry gas. For example, vacuum treatment is performed to a vacuum degree of 100Pa, and then filled with dry air or high-purity nitrogen. The amount of condensed water is controlled by controlling the flow rate of the dry gas to control the humidity of the atmosphere in the cavity 100. It can be understood that if condensed water needs to be generated on the surface of the sample during bonding, and there is no requirement for the amount of condensed water, no additional treatment is required between step A and step B.

[0049] In this embodiment, T1, T2, T3, and T4 are independently set to -300°C to 0°C. This setting can eliminate the internal stress of the first bond body used in a low temperature environment, and those skilled in the art can set the specific temperature as needed. Preferably, the absolute value of the temperature difference between T1 and T3 is less than 10°C; the absolute value of the temperature difference between T2 and T4 is less than 10°C. When the absolute value of the temperature difference exceeds 10°C, the internal stress control does not meet expectations.

[0050] Optionally, in step C, the predetermined value of the vacuum degree is less than 0.1 Pa, so as to facilitate subsequent activation treatment of the surfaces of the first sample 300 and the second sample 400. Optionally, during the irradiation treatment, the ion energy ranges from 0.1keV to 10keV, the ion flow during irradiation is from 0.1mA to 500mA, and the irradiation time is from 10s to 300s.

[0051] In this embodiment, in step E, during bonding, the bonding pressure value is 10N to 10000N, and the constant pressure is maintained for 1s to 1000s. This setting can effectively improve the bonding reliability of the first bonding body.

[0052] In this embodiment, step E further includes heating the first bonding body to bring the temperature of the first bonding body to room temperature. The heating treatment can effectively improve the efficiency of the first bonding body returning from low temperature to room temperature or working temperature.

[0053] Preferably, step A further includes: providing a third sample; and after step E, further includes: bonding the first bonding body to the third sample to form a second bonding body. The two bonding processes can be completed in the same cavity 100, which effectively improves the bonding efficiency and avoids the negative impact on the bonding surface caused by changing the cavity or changing the atmosphere.

[0054] The low temperature bonding method is completed using low temperature bonding equipment, such as Figure 2 and Figure 3 As shown, the low-temperature bonding equipment includes a cavity 100, a support frame and a manipulator. The support frame is installed in the cavity 100. There are three support frames, namely a first support frame 210, a second support frame 220 and a third support frame. The first support frame 210 and the second support frame 220 are arranged opposite to each other. The first support frame 210 is used to clamp and cool the first sample 300, the second support frame 220 is used to clamp and cool the second sample 400, and the third support frame is used to carry the bonding body; the manipulator is arranged in the cavity 100, and is used to transfer the bonding body between the second support frame 220 and the third support frame.

[0055] Specifically, the first support frame 210 and the second support frame 220 are both provided with a first gas circulation channel 230, and the first gas circulation channel 230 is used to circulate low-temperature gas. Figure 2 and Figure 3The flow direction of the cryogenic gas is indicated in the figure. The first gas circulation channel 230 is provided in both the first support frame 210 and the second support frame 220. The first gas circulation channel 230 is used to circulate the cryogenic gas. When the first sample 300 and the second sample 400 are bonded, the circulating cryogenic gas is fed into the first support frame 210 and the second support frame 220. The first support frame 210 and the first sample 300 are in thermal contact with each other, so that the temperature of the first sample 300 is reduced to the same level as that of the first support frame 210. The second support frame 220 and the second sample 400 are in thermal contact with each other, so that the temperature of the second sample 400 is reduced to the same level as that of the second support frame 220. The first sample 300 and the second sample 400 are in a low temperature state, thereby achieving low temperature bonding.

[0056] Optionally, the low-temperature bonding device further includes an ion source assembly, the ion source assembly includes an ion source 510 and a housing 520, the housing 520 is provided with a housing cavity for mounting the ion source 510, and the direction of the cavity opening of the housing cavity is set at an angle with the surface of the first sample 300 or the second sample 400. During irradiation, the high-speed ion beam 530 generated by the ion source 510 is neutralized and irradiated to the surface of the first sample 300 or the second sample 400 through the cavity opening of the housing cavity, so as to clean the surface of the first sample 300 or the second sample 400 and generate suspended chemical bonds on the surface of the first sample 300 or the second sample 400; the direction of the cavity opening of the housing cavity is set at an angle with the surface of the first sample 300 or the second sample 400 to avoid interfering with the bonding process of the first sample 300 and the second sample 400. In this embodiment, two ion source assemblies are provided, one of which is used to irradiate the first sample 300, and the other is used to irradiate the second sample 400. In other embodiments, the ion source assembly can also be set to one or more. For example, the ion source assembly is provided with one ion source, and two ion sources 510 are provided in the ion source assembly, wherein one ion source 510 is used to irradiate the first sample 300, and the other ion source 510 is used to irradiate the second sample 400. Those skilled in the art may set it according to the needs.

[0057] Furthermore, a second gas circulation channel 521 is provided in the housing 520, and the second gas circulation channel 521 is arranged around the ion source 510 to circulate low-temperature gas. By circulating low-temperature gas in the second gas circulation channel 521, the low-temperature gas can cool the housing 520, which can effectively prevent heat radiation from the ion source 510.

[0058] Preferably, two support racks form a support rack group, and at least two support rack groups can be arranged in the cavity 100. By setting at least two support rack groups, the at least two support rack groups can be subjected to cooling treatment respectively, so as to facilitate multiple bonding treatments. For example, two support rack groups are arranged in the cavity 100, and the temperature of the two support racks of one support rack group is reduced to -100°C, and the temperature of the two support racks of the other support rack group is reduced to -200°C. The first sample 300 and the second sample 400 are first bonded on the support rack group at a temperature of -100°C to form a first bonding body, and then the first bonding body and the third sample are bonded on the support rack group at a temperature of -200°C to form a second bonding body.

[0059] In this embodiment, the low temperature bonding equipment further includes an atmosphere preparation component, and the atmosphere preparation component is used to perform a vacuum process on the cavity 100. Optionally, the atmosphere preparation component is configured as a vacuum pump.

[0060] Preferably, the low temperature bonding device further comprises a temperature measuring element, the temperature measuring element comprises a first temperature measuring element and a second temperature measuring element, the first temperature measuring element is arranged between the first support frame 210 and the first sample 300, and the second temperature measuring element is arranged between the second support frame 220 and the second sample 400. By arranging the first temperature measuring element between the first support frame 210 and the first sample 300, and arranging the second temperature measuring element between the second support frame 220 and the second sample 400, the first sample 300 and the second sample 400 can be individually controlled in temperature according to the characterization of the temperature by the first temperature measuring element and the second temperature measuring element.

[0061] The third support frame is provided with a bonding body placement area, which is used to place the bonding body, and the temperature of the third support frame is selectively configured at -300°C to 50°C. During operation, a manipulator can be used to transport the bonding body (such as the first bonding body or the second bonding body) to the bonding body placement area. Exemplarily, when the bonding body placement area is 0°C to 50°C, it is used to return the temperature of the bonding body at a negative temperature to the ambient temperature. When the bonding body placement area is -300°C to 0°C, it is used to reduce the bonding body to the target temperature before bonding with other samples. By setting the bonding body placement area, the bonding body is prevented from directly rising / cooling down on the support frame, thereby reducing the frequency of heating and cooling the support frame and improving the bonding rate.

[0062] Optionally, the first support frame 210 clamps the first sample 300 through an electrostatic chuck; the second support frame 220 clamps the second sample 400 through an electrostatic chuck. The electrostatic chuck has strong adaptability and can accurately fix the sample on the table of the support frame. Optionally, the cryogenic gas is helium or nitrogen.

[0063] Taking the first sample 300 as silicon carbide and the second sample 400 as a silicon wafer as an example, the low temperature bonding method includes the following steps:

[0064] S1. Separate bonding temperature control is performed on silicon carbide and silicon wafer. The bonding temperature of silicon carbide is -200°C and the bonding temperature of silicon wafer is -50°C.

[0065] S2. Vacuum the cavity 100 to a vacuum degree of 1×10 -3 Pa;

[0066] S3, activation treatment, using neutralized argon ions to irradiate silicon carbide and silicon wafers, the ion energy is 1.5keV, the ion beam 530 flow is 50mA, and the irradiation time is 60s;

[0067] S4, bonding treatment, preparing a bonded body of silicon carbide and silicon wafer, wherein the bonding pressure value during bonding is 5000N, and the constant pressure is maintained for 60s;

[0068] S5. The temperature of the bonded body obtained in S4 is raised to 20°C. The bond strength of the bonded body is measured to be 1.9 J / m 2 , the interface internal stress is 1.2×10 6 N / m 2 , the stress uniformity on the wafer surface is good.

[0069] Taking the first sample 300 as silicon carbide and the second sample 400 as silicon oxide as an example, the low temperature bonding method includes the following steps:

[0070] S1. Separate bonding temperature control is performed on silicon carbide and silicon oxide. The bonding temperature of silicon carbide is -150°C and the bonding temperature of silicon oxide is -150°C.

[0071] S2, evacuating the cavity 100 and backfilling with dry gas;

[0072] S3, activation treatment, using neutralized argon ions to irradiate silicon carbide and silicon oxide, the ion energy is 1.5keV, the ion beam 530 flow is 50mA, and the irradiation time is 60s;

[0073] S4, bonding treatment, preparing a bonded body of silicon carbide and silicon oxide, wherein the bonding pressure value during bonding is 5000N, and the constant pressure is maintained for 60s;

[0074] S5. The temperature of the bonded body obtained in S4 was raised to 50°C. The interfacial stress of the bonded body was measured to be 8.1×10 6 N / m 2 .

[0075] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, various obvious changes, readjustments and substitutions can be made without departing from the protection scope of the present invention. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. Low temperature bonding method, It is characterized in that include: A: providing a cavity (100), and placing a first sample (300) and a second sample (400) to be bonded in the cavity (100); B: performing independent cooling treatment on the first sample (300) and the second sample (400), so that the temperature of the first sample (300) is T1 and the temperature of the second sample (400) is T2; and T1 and T2 are respectively below 0°C; C: evacuating the cavity (100) so that the vacuum degree in the cavity (100) reaches a predetermined value; D: performing irradiation treatment on the first sample (300) and the second sample (400), so that the surfaces of the first sample (300) and the second sample (400) are activated; E: The first sample (300) and the second sample (400) are bonded to form a first bonded body; during bonding, the temperature of the first sample (300) is T3, and the temperature of the second sample (400) is T4; T3 and T4 are both below 0°C.

2. The low temperature bonding method according to claim 1, It is characterized in that Also included between step A and step B is step A1: vacuuming the cavity (100).

3. The low temperature bonding method according to claim 1, It is characterized in that Also included between step A and step B is step A1: evacuating the cavity (100) and then backfilling with dry gas.

4. The low temperature bonding method according to any one of claims 1 to 3, It is characterized in that The T1, the T2, the T3, and the T4 are independently set to -300°C to 0°C.

5. The low temperature bonding method according to any one of claims 1 to 3, It is characterized in that The absolute value of the temperature difference between T1 and T3 is less than 10°C; the absolute value of the temperature difference between T2 and T4 is less than 10°C.

6. The low temperature bonding method according to any one of claims 1 to 3, It is characterized in that In the step C, the predetermined value of the vacuum degree is less than 0.1 Pa.

7. The low temperature bonding method according to any one of claims 1 to 3, It is characterized in that In the step E, during bonding, the bonding pressure value is 10N to 10000N, and the constant pressure is maintained for 1s to 1000s.

8. The low temperature bonding method according to any one of claims 1 to 3, It is characterized in that After step E, the first bonding body is subjected to a heating treatment so that the temperature of the first bonding body reaches room temperature.

9. The low temperature bonding method according to any one of claims 1 to 3, It is characterized in that The step A further includes: providing a third sample; and after the step E, the step further includes: bonding the first bonding body to the third sample to form a second bonding body.

10. The low temperature bonding method according to claim 1, It is characterized in that The low temperature bonding method is completed by using a low temperature bonding device, and the low temperature bonding device comprises: Cavity (100); A support frame installed in the cavity (100), wherein three support frames are provided, namely a first support frame (210), a second support frame (220) and a third support frame, wherein the first support frame (210) and the second support frame (220) are arranged opposite to each other, the first support frame (210) is used to clamp and cool the first sample (300), the second support frame (220) is used to clamp and cool the second sample (400), and the third support frame is used to carry a bonding body, and the temperature of the third support frame is selectively configured to be between -300°C and 50°C; A robot arm is arranged in the cavity (100) and is used to transfer the bonding body between the second support frame (220) and the third support frame.

Citation Information

Patent Citations

  • Method for directly bonding glass substrate and polystyrene substrate at room temperature and glass substrate recycling method

    CN107583697A

  • Preparation method of heterogeneous bonding structure

    CN111383915A