A kind of hybrid aramid nanofiber modified concrete and preparation method thereof

By adding flat glass fiber, graphene and solid glass microbeads in the preparation process of aramid nanofibers, their dispersion properties are improved, and the problems of easy cracking and low mechanical properties of traditional concrete are solved, which significantly improves the toughness and crack resistance of concrete. .

CN118666551BActive Publication Date: 2024-11-19SUZHOU CHUXIN MOYI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411162765.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-19
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Traditional concrete is prone to cracking and has low mechanical properties, making it difficult to effectively improve tensile strength and toughness. Existing fiber-reinforced materials such as glass fibers have problems with strength and toughness degradation when used in concrete, and nanofibers have poor dispersion, which is difficult to promote.

Method used

Aramid nanofibers were prepared by alkali/DMSO immersion method, and flat glass fibers, graphene and solid glass microbeads were added during the preparation process. The dispersion performance of nanofibers was improved by forming continuous structures of dots, lines and surfaces, and the dispersion performance of nanofibers was improved through alkaline. /DMSO solution removes residual organic groups in industrial production and enhances the binding force between fiber and cement.

Benefits of technology

It improves the toughness and permeability of concrete, inhibits the generation of fine cracks, significantly improves the performance of concrete, forms an interactive network structure, reduces pore generation, and enhances crack resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118666551B_ABST
    Figure CN118666551B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of concrete, and particularly relates to a hybrid aramid nanofiber modified concrete and a preparation method thereof. The raw materials of the hybrid aramid nanofiber modified concrete of the present invention include: water, cement, mineral admixture, sand, crushed stone, hybrid aramid nanofiber, water reducer, and expansion agent. In the preparation process of aramid nanofibers by alkali / DMSO soaking method, a certain amount of flat glass fiber, graphene, and solid glass microbead inorganic fillers in different forms are added. Due to the different physical shapes such as appearance, internal structure, surface properties, and particle grading of aramid nanofibers, flat glass fibers, graphene, and solid glass microbeads, morphological effects and micro-aggregate effects can be generated. The above fillers are evenly distributed in cement paste, which reduces the pores of concrete, not only improves the toughness of concrete, but also inhibits the generation of fine cracks. These effects greatly improve the performance of concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete, and in particular relates to a hybrid aramid nanofiber modified concrete and a preparation method thereof. Background Art

[0002] As a brittle material, traditional concrete has the advantages of being easy to shape, low in price, resistant to high temperatures, relatively durable, and having high compressive strength. Since the invention of Portland cement, it has been the main cementing material for concrete for hundreds of years and has been widely used in civil engineering, transportation engineering, etc. around the world.

[0003] The research on concrete materials has developed from ordinary concrete to high-strength concrete, and then from high-strength concrete to high-performance concrete. High-performance concrete focuses on both the mechanical properties and durability of concrete. When preparing high-performance concrete, active mineral fine admixtures and high-efficiency water reducers are added to make the concrete have the characteristics of low water-cement ratio, low cement dosage, low hydration heat and high durability. With the development of the country's economy and technology, more and more new buildings and large structures are being implemented, and the requirements for the performance of concrete materials are gradually increasing; however, the inherent disadvantages of concrete, such as low tensile strength, poor toughness, large shrinkage, easy cracking, etc., are still the main problems in the use of construction materials.

[0004] More than 80% of the cracks in structures in engineering practice are caused by deformation changes. Theoretical and practical studies have shown that most of the cracks caused by deformation changes are caused by shrinkage stress caused by early concrete drying and cooling after hydration. At present, the main technical measures used to reduce cracks caused by deformation changes from the perspective of concrete material composition and proportion include: reducing cement dosage to reduce shrinkage, using expansion agent to compensate for concrete shrinkage, configuring crack-resistant steel bars, and adding fiber reinforcement (such as synthetic fiber, steel fiber, carbon fiber). In essence, it is to improve the volume stability of concrete, or enhance the ability of concrete to resist deformation, or reduce the brittleness of concrete. There are many research reports on polypropylene fiber and steel fiber reinforced concrete and expansive concrete at home and abroad. Fibers such as nylon, polypropylene, and polyethylene are beneficial to improving the impact resistance of mortar. Since then, glass fiber and carbon fiber have appeared, but glass fiber will have problems such as strength and toughness degradation in concrete. It is now mostly used for structural reinforcement, and there is little research on its related physics. Carbon fiber is one of the fibers with the best comprehensive performance known so far, but its high price limits its large-scale application. Summary of the invention

[0005] The purpose of the present invention is to provide a hybrid aramid nanofiber modified concrete and a preparation method thereof, so as to solve the technical problems that ordinary concrete is easy to crack and has low mechanical properties.

[0006] In one aspect, the present invention provides a hybrid aramid nanofiber modified concrete, comprising the following components in parts by weight: 120-160 parts of water, 650-700 parts of cement, 100-120 parts of mineral admixture, 570-610 parts of sand, 850-900 parts of crushed stone, 20-30 parts of hybrid aramid nanofiber, 5-10 parts of water reducing agent, and 10-15 parts of expansion agent;

[0007] The hybrid aramid nanofiber preparation process is as follows:

[0008] (1) placing aramid fibers into a reaction kettle containing alkali and dimethyl sulfoxide and stirring the mixture sufficiently to obtain an aramid nanofiber dispersion;

[0009] (2) Flat glass fiber, graphene and solid glass microbeads are added to the aramid nanofiber dispersion, mixed evenly, and then deionized water is added to obtain a mixed aramid nanofiber dispersion. After filtration, washing and drying, mixed aramid nanofibers are obtained; the mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads is 1: (0.5-1): (0.2-0.4): (0.2-0.4).

[0010] The modification effect of fiber on concrete mainly depends on the type of fiber, its distribution in concrete, dosage and other factors. This modification effect is exerted on the optimization of concrete microstructure. In particular, nanofibers, due to their microscopic size effect, have an enhanced and anti-cracking effect that ordinary fibers cannot match.

[0011] In order to achieve a good reinforcing effect, the fiber needs to have good adhesion to cement and good dispersibility. Inorganic fibers have good hydrophilicity and good compatibility with cement matrix. Organic fibers have poor hydrophilicity and poor dispersibility. In particular, organic nanofibers are more difficult to disperse evenly in cement matrix due to the presence of nano effect. In order to improve the dispersibility of aramid nanofibers, CN11812577A adopts the method of grafting halloysite nanotubes and silicon dioxide on the surface of aramid nanofibers to improve their compatibility. However, the process is complicated and the cost is high, and it is difficult to promote and use. The present invention adopts alkali / DMSO soaking method to prepare aramid nanofibers. The aramid nanofibers prepared by this method have good hydrophilicity and improve their dispersibility in aqueous solution to a certain extent. However, due to the inherent agglomeration characteristics of nanofibers, it is difficult to be evenly dispersed in cement matrix when directly added. In order to solve the above problems, the present invention adds a certain amount of flat glass fibers, graphene, and solid glass microbeads inorganic fillers in different forms during the preparation process of aramid nanofibers prepared by alkali / DMSO soaking method. The flat glass fiber has a one-dimensional linear structure, and compared with the ordinary round glass fiber, its cross section is a special-shaped structure, which can increase the contact area with the aramid nanofiber and improve the dispersion performance of the aramid nanofiber; graphene has a two-dimensional lamellar structure, and the solid glass microbead has a zero-dimensional spherical structure. The addition of the above fillers can form a continuous structure of points, lines, and surfaces, and can be mixed with the aramid nanofiber in advance to effectively improve the dispersion performance of the nanofiber. In addition, the present invention adds flat glass fibers, graphene, and solid glass microbeads to the alkali / DMSO solution of aramid nanofibers. The solution can not only effectively remove the organic groups remaining in the industrial production on the surface of flat glass fibers, graphene, and solid glass microbeads, and improve their dispersion performance; but also greatly enhance the bonding force between the inorganic filler and the nanofiber and between the inorganic filler and the cement. Solid glass microbeads have higher mechanical properties than hollow glass microbeads, and the reinforcing effect is obvious. In particular, the amount of lamellar graphene added should be controlled: when the amount is too little, it cannot play a synergistic dispersion role; when the amount is too much, the aramid nanofibers may be over-enriched, which is not conducive to the dispersion of the aramid nanofibers.

[0012] The addition of fillers such as aramid nanofibers, flat glass fibers, graphene, and solid glass microbeads can produce a synergistic reinforcement effect on concrete. Due to the different physical shapes such as appearance, internal structure, surface properties, and particle grading of aramid nanofibers, flat glass fibers, graphene, and solid glass microbeads, a morphological effect can be produced. The sizes of different morphologies are intertwined. Flat glass fibers have a special-shaped structure, which can be bonded to the material and play the role of aggregate; aramid nanofibers are small in size and easily form a dense non-directional network, which plays the role of reinforcing ribs; while graphene and spherical solid glass microbeads can improve the dispersion of flat glass fibers and aramid nanofibers, so that the fibers and cement are tightly bonded together. The above fillers are evenly distributed in the concrete to form an interactive network, which effectively reduces the generation of concrete pores, improves the impermeability, and prevents the generation and development of cracks. At the same time, the addition of the above-mentioned fillers can play a micro-aggregate effect. Aramid nanofibers, flat glass fibers, graphene, and solid glass beads are evenly distributed in the cement slurry, which reduces the pores in the concrete. This not only improves the toughness of the concrete, but also inhibits the generation of fine cracks. These effects greatly improve the performance of the concrete.

[0013] In one embodiment, the cement is silicate cement or sulphoaluminate cement.

[0014] In one embodiment, the mineral admixture is at least one of fly ash, silica powder, and ground slag.

[0015] In one embodiment, the water reducer is a polycarboxylate water reducer.

[0016] In one embodiment, the expansion agent is a UEA expansion agent.

[0017] In one embodiment, the base is sodium hydroxide or potassium hydroxide.

[0018] In one embodiment, the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1 g: (1-2) g: (350-500) ml.

[0019] In one embodiment, the stirring in step (1) is carried out at room temperature for 4-8 days.

[0020] In one embodiment, the mass ratio of the aramid fiber, the flat glass fiber, the graphene, and the solid glass microbeads is 1: (0.6-0.8): 0.3: 0.3. The flat glass fiber is a glass fiber with a cross-sectional major diameter / minor diameter ratio of 2-7, a length of 1-10 mm, and a major diameter and minor diameter length range of 1-60 μm.

[0021] On the other hand, the present invention also provides a method for preparing hybrid aramid nanofiber modified concrete, comprising the following steps:

[0022] (1) Weigh each component according to the proportion;

[0023] (2) Mix water, cement, mineral admixtures and hybrid aramid nanofibers in advance; then, add water reducing agent, expansion agent, sand and gravel in sequence under stirring conditions, and mix them evenly to obtain hybrid aramid nanofiber modified concrete.

[0024] Beneficial effects:

[0025] The present invention adopts alkali / DMSO soaking method to prepare aramid nanofiber, and in the preparation process of preparing aramid nanofiber by alkali / DMSO soaking method, a certain amount of flat glass fiber, graphene, solid glass microbead inorganic filler in different forms is added to give full play to the technical effect of the toughness of organic fiber and the rigidity of flat glass fiber. The addition of fillers such as aramid nanofiber, flat glass fiber, graphene, solid glass microbead can produce synergistic reinforcement effect on concrete. Due to the different physical shapes such as appearance, internal structure, surface property and particle gradation of aramid nanofiber, flat glass fiber, graphene, solid glass microbead, morphological effect and micro-aggregate effect can be produced, aramid nanofiber, flat glass fiber, graphene, solid glass microbead are evenly distributed in cement paste, concrete pores are reduced, not only the toughness of concrete is improved, but also the generation of micro cracks is suppressed, and these effects greatly improve the performance of concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a scanning electron microscope image of the aramid nanofiber prepared in Example 7;

[0027] Figure 2 This is the transmission electron microscopy image of the aramid nanofiber prepared in Example 7. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The aramid fiber used in the embodiments and comparative examples of the present invention is DuPont Kevlar fiber; the flat glass fiber is CSG3PA-820 from Nitto Bo Corporation, 3 mm long, 28 μm in major axis diameter, and 7 μm in minor axis diameter; the circular cross-section glass fiber is 03JAFT692 from Asahi Fiberglass Corporation, 3 mm long and 10 μm in diameter.

[0029] Example 1

[0030] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 120 parts of water, 650 parts of sulphoaluminate cement, 100 parts of fly ash mineral admixture, 570 parts of sand, 850 parts of crushed stone, 20 parts of hybrid aramid nanofiber, 5 parts of polycarboxylate water reducer, and 10 parts of UEA expansion agent;

[0031] The hybrid aramid nanofiber preparation process is as follows:

[0032] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 4 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1 g:350 ml;

[0033] (2) Flat glass fiber, graphene and solid glass microbeads are added to the aramid nanofiber dispersion, the mixture is evenly mixed, and deionized water is added to obtain a mixed aramid nanofiber dispersion. The mixed aramid nanofibers are obtained after filtration, washing and drying. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads is 1:0.6:0.2:0.2.

[0034] Example 2

[0035] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 160 parts of water, 700 parts of sulphoaluminate cement, 120 parts of silica fume mineral admixture, 610 parts of sand, 900 parts of crushed stone, 30 parts of hybrid aramid nanofiber, 10 parts of polycarboxylate water reducer, and 15 parts of UEA expansion agent;

[0036] The hybrid aramid nanofiber preparation process is as follows:

[0037] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 8 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:2 g:500 ml;

[0038] (2) Flat glass fiber, graphene and solid glass microbeads are added to the aramid nanofiber dispersion, and the mixture is evenly mixed. Deionized water is then added to obtain a mixed aramid nanofiber dispersion. The mixed aramid nanofibers are obtained after filtration, washing and drying. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads is 1:0.8:0.4:0.4.

[0039] Example 3

[0040] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 120 parts of water, 700 parts of sulphoaluminate cement, 100 parts of fly ash mineral admixture, 610 parts of sand, 850 parts of crushed stone, 30 parts of hybrid aramid nanofiber, 5 parts of polycarboxylate water reducer, and 15 parts of UEA expansion agent;

[0041] The hybrid aramid nanofiber preparation process is as follows:

[0042] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 5 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:2 g:350 ml;

[0043] (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion, mixed evenly, and then deionized water was added to obtain a mixed aramid nanofiber dispersion. After filtration, washing and drying, mixed aramid nanofibers were obtained. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1:0.6:0.4:0.2.

[0044] Example 4

[0045] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 160 parts of water, 650 parts of sulphoaluminate cement, 120 parts of silica fume mineral admixture, 570 parts of sand, 900 parts of crushed stone, 20 parts of hybrid aramid nanofiber, 5 parts of polycarboxylate water reducer, and 15 parts of UEA expansion agent;

[0046] The hybrid aramid nanofiber preparation process is as follows:

[0047] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 5 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1 g:500 ml;

[0048] (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion, mixed evenly, and then deionized water was added to obtain a mixed aramid nanofiber dispersion. After filtration, washing and drying, mixed aramid nanofibers were obtained. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1:0.8:0.2:0.4.

[0049] Example 5

[0050] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 130 parts of water, 660 parts of sulphoaluminate cement, 110 parts of fly ash mineral admixture, 580 parts of sand, 870 parts of crushed stone, 22 parts of hybrid aramid nanofiber, 6 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0051] The hybrid aramid nanofiber preparation process is as follows:

[0052] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 6 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.2 g:380 ml;

[0053] (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion and mixed evenly. Deionized water was then added to obtain a mixed aramid nanofiber dispersion. The mixed aramid nanofibers were obtained after filtration, washing and drying. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1:0.7:0.25:0.22.

[0054] Example 6

[0055] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 150 parts of water, 680 parts of sulphoaluminate cement, 112 parts of fly ash mineral admixture, 600 parts of sand, 880 parts of crushed stone, 27 parts of hybrid aramid nanofiber, 8 parts of polycarboxylate water reducer, and 14 parts of UEA expansion agent;

[0056] The hybrid aramid nanofiber preparation process is as follows:

[0057] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 7 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.7 g:400 ml;

[0058] (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion, mixed evenly, and then deionized water was added to obtain a mixed aramid nanofiber dispersion. After filtration, washing and drying, mixed aramid nanofibers were obtained. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1:0.8:0.35:0.38.

[0059] Example 7

[0060] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 140 parts of water, 680 parts of sulphoaluminate cement, 110 parts of fly ash mineral admixture, 580 parts of sand, 870 parts of crushed stone, 25 parts of hybrid aramid nanofiber, 8 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0061] The hybrid aramid nanofiber preparation process is as follows:

[0062] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 6 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.6 g:400 ml;

[0063] (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion, and the mixture was evenly mixed. Deionized water was then added to obtain a mixed aramid nanofiber dispersion. The mixed aramid nanofibers were obtained after filtration, washing and drying. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1:0.7:0.3:0.3.

[0064] Example 8

[0065] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 140 parts of water, 680 parts of sulphoaluminate cement, 110 parts of fly ash mineral admixture, 580 parts of sand, 870 parts of crushed stone, 25 parts of hybrid aramid nanofiber, 8 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0066] The hybrid aramid nanofiber preparation process is as follows:

[0067] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 6 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.6 g:400 ml;

[0068] (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion, mixed evenly, and then deionized water was added to obtain a mixed aramid nanofiber dispersion. After filtration, washing and drying, mixed aramid nanofibers were obtained. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1:0.5:0.3:0.3.

[0069] Example 9

[0070] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 140 parts of water, 680 parts of sulphoaluminate cement, 110 parts of fly ash mineral admixture, 580 parts of sand, 870 parts of crushed stone, 25 parts of hybrid aramid nanofiber, 8 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0071] The hybrid aramid nanofiber preparation process is as follows:

[0072] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 6 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.6 g:400 ml;

[0073] (2) Flat glass fiber, graphene and solid glass microbeads are added to the aramid nanofiber dispersion, mixed evenly, and then deionized water is added to obtain a mixed aramid nanofiber dispersion. After filtration, washing and drying, mixed aramid nanofibers are obtained; the mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads is 1:1:0.3:0.3.

[0074] Comparative Example 1

[0075] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 140 parts of water, 680 parts of sulphoaluminate cement, 110 parts of fly ash mineral admixture, 580 parts of sand, 870 parts of crushed stone, 25 parts of hybrid aramid nanofiber, 8 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0076] The hybrid aramid nanofiber preparation process is as follows:

[0077] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 6 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.6 g:400 ml;

[0078] (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion, mixed evenly, and then deionized water was added to obtain a mixed aramid nanofiber dispersion. After filtration, washing and drying, mixed aramid nanofibers were obtained. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1:0:0.65:0.65.

[0079] Comparative Example 2

[0080] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 140 parts of water, 680 parts of sulphoaluminate cement, 110 parts of fly ash mineral admixture, 580 parts of sand, 870 parts of crushed stone, 25 parts of hybrid aramid nanofiber, 8 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0081] The hybrid aramid nanofiber preparation process is as follows:

[0082] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 6 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.6 g:400 ml;

[0083] (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion and mixed evenly. Deionized water was then added to obtain a mixed aramid nanofiber dispersion. The mixed aramid nanofibers were obtained after filtration, washing and drying. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1:0.91:0:0.39.

[0084] Comparative Example 3

[0085] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 140 parts of water, 680 parts of sulphoaluminate cement, 110 parts of fly ash mineral admixture, 580 parts of sand, 870 parts of crushed stone, 25 parts of hybrid aramid nanofiber, 8 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0086] The hybrid aramid nanofiber preparation process is as follows:

[0087] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 6 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.6 g:400 ml;

[0088] (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion, mixed evenly, and then deionized water was added to obtain a mixed aramid nanofiber dispersion. After filtration, washing and drying, mixed aramid nanofibers were obtained. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1:0.91:0.39:0.

[0089] Comparative Example 4

[0090] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 140 parts of water, 680 parts of sulphoaluminate cement, 110 parts of fly ash mineral admixture, 580 parts of sand, 870 parts of crushed stone, 25 parts of hybrid aramid nanofiber, 8 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0091] The hybrid aramid nanofiber preparation process is as follows:

[0092] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 6 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.6 g:400 ml;

[0093] (2) Adding circular cross-section glass fibers, graphene and solid glass microbeads with the same length into an aramid nanofiber dispersion, mixing the mixture evenly, and then adding deionized water to obtain a mixed aramid nanofiber dispersion. After filtration, washing and drying, mixed aramid nanofibers were obtained. The mass ratio of aramid fibers, circular cross-section glass fibers, graphene and solid glass microbeads was 1:0.7:0.3:0.3.

[0094] Comparative Example 5

[0095] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 140 parts of water, 680 parts of sulphoaluminate cement, 110 parts of fly ash mineral admixture, 580 parts of sand, 870 parts of crushed stone, 25 parts of hybrid aramid nanofiber, 8 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0096] The hybrid aramid nanofiber preparation process is as follows:

[0097] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 6 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.6 g:400 ml;

[0098] (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion and mixed evenly. Deionized water was then added to obtain a mixed aramid nanofiber dispersion. The mixed aramid nanofibers were obtained after filtration, washing and drying. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1:0.7:0.7:0.3.

[0099] Comparative Example 6

[0100] A hybrid aramid nanofiber modified concrete comprises the following components in parts by weight: 140 parts of water, 680 parts of sulphoaluminate cement, 110 parts of fly ash mineral admixture, 580 parts of sand, 870 parts of crushed stone, 25 parts of hybrid aramid nanofiber, 8 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0101] The hybrid aramid nanofiber preparation process is as follows:

[0102] (1) placing aramid fiber in a reaction kettle containing potassium hydroxide and dimethyl sulfoxide, and stirring at room temperature for 6 days to obtain an aramid nanofiber dispersion; the ratio of the aramid fiber, potassium hydroxide and dimethyl sulfoxide is 1 g:1.6 g:400 ml;

[0103] (2) Deionized water is added to an aramid nanofiber dispersion to obtain a mixed aramid nanofiber dispersion, and aramid nanofibers are obtained after filtration, washing, and drying; aramid nanofibers, flat glass fibers, graphene, and solid glass microbeads are uniformly mixed in an aqueous solution, and mixed aramid nanofibers are obtained after filtration, washing, and drying; the mass ratio of aramid fibers, flat glass fibers, graphene, and solid glass microbeads is 1:0.7:0.3:0.3.

[0104] The preparation process of the hybrid aramid nanofiber modified concrete in the above embodiment is the same as that in the comparative example, and includes the following steps:

[0105] (1) Weigh each component according to the proportion;

[0106] (2) Mix water, cement, mineral admixtures and hybrid aramid nanofibers in advance; then, add water reducing agent, expansion agent, sand and gravel in sequence under stirring conditions, and mix them evenly to obtain hybrid aramid nanofiber modified concrete.

[0107] The mechanical properties of concrete were tested according to GB / T 50081-2019; the cracking area of ​​concrete was tested according to GB / T 50082-2009. The main performance indicators of the above embodiments and comparative examples are shown in Tables 1 and 2:

[0108]

[0109]

[0110] It can be seen from Tables 1 and 2 that due to the different physical shapes such as appearance, internal structure, surface properties and particle grading of aramid nanofibers, flat glass fibers, graphene and solid glass beads, morphological effects and micro-aggregate effects can be produced. Aramid nanofibers, flat glass fibers, graphene and solid glass beads are evenly distributed in the cement paste, which reduces the porosity of concrete, improves the toughness of concrete, and inhibits the generation of fine cracks. These effects greatly improve the performance of concrete.

[0111] Figure 1 and Figure 2 This is an electron microscope image of the aramid nanofiber prepared in Example 7. It can be seen from the image that the surface of the aramid nanofiber is relatively rough and the diameter is between 30nm and 100nm. It can be seen from Examples 7-9 that when the mass ratio of aramid fiber, flat glass fiber, graphene, and solid glass microbead is 1: (0.6-0.8): 0.3: 0.3, the performance indicators of concrete reach the best.

[0112] Comparative Examples 1-3 Compared with Example 7, when it lacks any component of flat glass fiber, graphene, and solid glass microspheres, the mechanical properties and crack resistance of concrete are greatly reduced. The addition of fillers such as aramid nanofibers, flat glass fibers, graphene, and solid glass microspheres can produce a synergistic enhancement effect on concrete. Due to the different physical shapes such as the appearance, internal structure, surface properties, and particle grading of aramid nanofibers, flat glass fibers, graphene, and solid glass microspheres, a morphological effect can be produced. The above fillers are evenly distributed in the concrete to form an interactive network, which effectively reduces the generation of concrete pores, improves impermeability, and prevents the generation and development of cracks. At the same time, the addition of the above fillers can play a micro-aggregate effect. Aramid nanofibers, flat glass fibers, graphene, and solid glass microspheres are evenly distributed in cement paste, which reduces the pores of concrete, not only improves the toughness of concrete, but also suppresses the generation of fine cracks. These effects greatly improve the performance of concrete. Comparative Example 4 shows that when round glass fibers are used instead of flat glass fibers, its mechanical properties are greatly reduced. Comparative Example 5 shows that when the amount of lamellar graphene added is too much, aramid nanofibers may be over-enriched, which is not conducive to the dispersion of aramid nanofibers. Comparative Example 6 shows that directly blending aramid nanofibers with fillers such as flat glass fibers, graphene, and solid glass microbeads in an aqueous solution cannot solve the technical problem that aramid nanofibers are easy to agglomerate. In the preparation process of aramid nanofibers prepared by the alkali / DMSO soaking method, a certain amount of flat glass fibers, graphene, and solid glass microbeads inorganic fillers in different forms are added. Flat glass fibers have a linear structure, graphene has a lamellar structure, and solid glass microbeads have a spherical structure. The addition of the above fillers can form a continuous structure of points, lines, and surfaces, and can be mixed with aramid nanofibers in advance to effectively improve the dispersion performance of nanofibers.

[0113] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A hybrid aramid nanofiber modified concrete, characterized in that: The invention comprises the following components in parts by weight: 120-160 parts of water, 650-700 parts of cement, 100-120 parts of mineral admixture, 570-610 parts of sand, 850-900 parts of crushed stone, 20-30 parts of mixed aramid nanofiber, 5-10 parts of water reducing agent, and 10-15 parts of expansion agent; The hybrid aramid nanofiber preparation process is as follows: (1) placing aramid fibers into a reactor containing alkali and dimethyl sulfoxide and stirring thoroughly to obtain an aramid nanofiber dispersion; (2) Flat glass fiber, graphene and solid glass microbeads were added to the aramid nanofiber dispersion and mixed evenly. Deionized water was then added to obtain a mixed aramid nanofiber dispersion. After filtration, washing and drying, mixed aramid nanofibers were obtained. The mass ratio of aramid fiber, flat glass fiber, graphene and solid glass microbeads was 1: (0.5-1): (0.2-0.4): (0.2-0.4).

2. The hybrid aramid nanofiber modified concrete according to claim 1, characterized in that: The cement is silicate cement or sulphoaluminate cement.

3. The hybrid aramid nanofiber modified concrete according to claim 1, wherein: The mineral admixture is at least one of fly ash, silica fume and ground slag.

4. The hybrid aramid nanofiber modified concrete according to claim 1, wherein: The water reducer is a polycarboxylate water reducer.

5. The hybrid aramid nanofiber modified concrete according to claim 1, wherein: The expansion agent is UEA expansion agent.

6. The hybrid aramid nanofiber modified concrete according to claim 1, wherein: The alkali is sodium hydroxide or potassium hydroxide.

7. The hybrid aramid nanofiber modified concrete according to claim 1, wherein: The ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1g: (1-2)g: (350-500)ml.

8. The hybrid aramid nanofiber modified concrete according to claim 1, wherein: The stirring in step (1) is carried out at room temperature for 4-8 days.

9. The hybrid aramid nanofiber modified concrete according to claim 1, wherein: The mass ratio of the aramid fiber, the flat glass fiber, the graphene, and the solid glass microbeads is 1:(0.6-0.8):0.3:0.

3.

10. The method for preparing hybrid aramid nanofiber modified concrete according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Weigh each component according to the proportion; (2) Mix water, cement, mineral admixtures and hybrid aramid nanofibers in advance; then, add water reducer, expansion agent, sand and gravel in sequence under stirring conditions, and mix them evenly to obtain hybrid aramid nanofiber modified concrete.