Preparation method of reactive hydrophobic white carbon black
The reaction of incomplete hydrolysis of dimethyldichlorosilane and ammonia is formed into a hydrophobic treatment agent, and combined with heating and stirring reaction, it forms a reactive hydrophobic white carbon black, which solves the problems of hydrophilicity limitation and high energy consumption and flash explosion risks of traditional white carbon black. , achieving high grafting rate and safe silicone rubber reinforcement effect.
Patent Information
- Application Number
- CN202411169941.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-26
AI Technical Summary
In the prior art, the surface of gas phase white carbon black and precipitation white carbon black is rich in silicon hydroxyl groups, resulting in its hydrophilicity limiting the wetting and dispersion properties in organic media, and traditional hydrophobic treatment methods have high energy consumption and equipment requirements. Issues of high and flash explosion risk during mixing process.
By incompletely hydrolyzing dimethyldichlorosilane with water, introducing ammonia reaction to form a hydrophobic treatment agent, and heating and stirring with hydrophilic white carbon black to form a reactive hydrophobic white carbon black, with a reactive Si on the surface -N bond, modified white carbon black to improve the reinforcement and structured resistance of silicone rubber.
The preparation of hydrophobic white carbon black with high grafting rate at low temperature is realized, and it is used as a structured control agent for silicon rubber, which improves the safety of the mixing process and the mechanical properties and shelf life of silicon rubber.
Smart Images

Figure CN118667358B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano material preparation, and in particular to a method for preparing reactive hydrophobic white carbon black. Background Art
[0002] Fumed silica is usually produced by hydrolysis and polycondensation of silicon tetrachloride or methyltrichlorosilane in a high-temperature hydrogen-oxygen flame environment. During this preparation process, a large amount of silanol groups remain on the surface of silicon particles and inside their aggregates due to incomplete polycondensation reaction. At the same time, precipitated silica is produced by the reaction of sodium silicate and sulfuric acid, and is processed through a series of steps such as washing, precipitation, and drying. Its surface is also rich in silanol groups. The presence of silanol groups gives silica hydrophilic and oleophobic properties, but this property largely limits its wetting and dispersion properties in organic media, which in turn restricts the application scope of fumed silica in many fields.
[0003] At present, the surface treatment of fumed silica mainly adopts methods such as silicone oil, cyclosiloxane, hexamethyldisilazane or chlorosilane. Silicone oil treatment is mainly achieved by adsorption on the surface of silica, but some polysiloxane is still in a free state; the treatment method with better reactivity is mainly to use chlorosilane, hexamethyldisilazane or cyclosiloxane at high temperature, which has high treatment temperature and high energy consumption.
[0004] Patent CN102220036A discloses a method for preparing silane coupling agent modified white carbon black, by mixing a solvent, water, a catalyst and a coupling agent to prepare a coupling agent sol solution. Then, the white carbon black is evenly dispersed in the sol solution by ultrasonic dispersion or shearing to obtain a turbid liquid with uniform dispersion and ideal particle size. Then, the turbid liquid is placed under uniform stirring to react the coupling agent sol with the white carbon black, and the coupling agent modified white carbon black with high hydrophobicity is prepared by controlling the temperature and reaction time. In this method, a sol solution of the coupling agent is obtained by a sol-gel method, and then the white carbon black can be evenly dispersed in the coupling agent sol solution by the combined action of a variety of kinetic means, thereby ensuring that the white carbon black and the coupling agent can fully react, and then the white carbon black modified by the coupling agent is obtained. Solvents are used in this method, which is not economical and environmentally friendly. The solution using ultrasonic or shear dispersion has high requirements on equipment and is difficult to industrialize.
[0005] Traditionally, hydrophobic silica is used as a reinforcing agent for silicone rubber. Whether it is used to prepare liquid silicone rubber or solid compound rubber, hydrophilic silica is mainly used. In the process of meshing of the rubber, the silica must be modified to enable the silicone rubber to obtain better mechanical properties and shelf life. However, static electricity will be generated during the stirring or meshing process. In the process of meshing mixing, hydroxyl silicone oil or other small molecule silane is added as a structuring control agent to treat silica. Due to the low flash point of hydroxyl silicone oil or small molecule silane, there is a risk of flash explosion.
[0006] Therefore, the preparation of a hydrophobic silica can not only provide a good reinforcement effect for silicone rubber, but also eliminate the danger in the mixing process, and can also make silicone rubber have a longer anti-structural time, which is of great significance to the actual production of silicone rubber. Summary of the invention
[0007] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing reactive hydrophobic silica, which takes hydrophilic silica as the basic raw material, introduces suitable compounds to react with it, so that the silica surface has reactive Si-N bonds, releases reactive silanes during the mixing process, modifies other hydrophilic silica, realizes the functions of silicone rubber reinforcement and anti-structuring, and can ensure safety during the production process.
[0008] The method for preparing the reactive hydrophobic silica of the present invention comprises the following steps:
[0009] (1) adding water to dimethyldichlorosilane to carry out a hydrolysis reaction to obtain an incomplete hydrolyzate;
[0010] The reaction mechanism of step (1) is as follows Figure 1 As shown;
[0011] (2) introducing ammonia gas into the incomplete hydrolyzate for reaction, filtering, and obtaining a hydrophobic treatment agent;
[0012] The reaction mechanism of step (2) is as follows Figure 2 As shown;
[0013] (3) The hydrophilic silica and the hydrophobic treatment agent are mixed evenly, heated and stirred for reaction, and vacuum treated to obtain reactive hydrophobic silica. The reaction mechanism of step (3) is as follows: Figure 3 shown.
[0014] The reaction mechanism of reactive hydrophobic silica in the process of silicone rubber meshing treatment is shown in the figure Figure 4 shown.
[0015] The molar ratio of dimethyldichlorosilane to water in step (1) is 4:3 to 10:9.
[0016] The temperature of the hydrolysis reaction in step (1) is 1-15°C.
[0017] The amount of ammonia used in step (2) is 10-30% of the mass of the incomplete hydrolyzate.
[0018] The reaction temperature of the reaction in step (2) is -10~10°C.
[0019] The hydrophilic silica in step (3) is hydrophilic fumed silica or hydrophilic precipitated silica.
[0020] The surface area of the hydrophilic silica in step (3) is 150-380 m 2 / g.
[0021] The amount of the hydrophobic treatment agent used in step (3) is 10-20% of the mass of the hydrophilic silica.
[0022] The reaction temperature of the reaction in step (3) is 60-130° C., the reaction time is 2-6 hours, and the vacuum degree of the vacuum treatment is -0.04-0.08 MPa.
[0023] In step (3), the hydrophilic silica and the hydrophobic treatment agent are mixed uniformly, and the heating and stirring reaction is carried out under the protection of an inert gas or nitrogen. The inert gas includes argon and helium, and nitrogen protection is preferably used.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The raw materials used in the synthesis of the treatment agent of the present invention are common raw materials, which have been industrialized and are easily available, low in cost, and effective reaction grafting is carried out on the surface of white carbon black.
[0026] 2. The hydrophobic silica obtained by the present invention can be prepared at low temperature, has a high surface grafting rate, and can be used as a structuring control agent for silicone rubber.
[0027] 3. The hydrophobic silica prepared by the present invention has a reactive Si-N bond on its surface, and releases reactive polysiloxane during the mixing process to modify other hydrophilic silica added, thereby achieving the functions of silicone rubber reinforcement and anti-structuring, while ensuring safety during the production process. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is a reaction mechanism diagram of step (1) of the present invention;
[0029] Figure 2 is a reaction mechanism diagram of step (2) of the present invention;
[0030] Figure 3 is a reaction mechanism diagram of step (3) of the present invention;
[0031] Figure 4 This is a diagram of the reaction mechanism of reactive hydrophobic silica during the silicone rubber meshing treatment process. DETAILED DESCRIPTION
[0032] The present invention will be further described below with reference to the embodiments.
[0033] Unless otherwise specified, all raw materials used in the examples are commercially available.
[0034] Example 1
[0035] The method for preparing the reactive hydrophobic silica comprises the following steps:
[0036] (1) adding water to dimethyldichlorosilane, with the molar ratio of dimethyldichlorosilane to water being 4:3, and slowly hydrolyzing the mixture while controlling the reaction temperature to 1°C to obtain an incomplete hydrolyzate;
[0037] (2) introducing ammonia gas at a rate of 30% of the mass of the incomplete hydrolyzate into the incomplete hydrolyzate at a constant speed within 30 minutes, stirring the reaction, and controlling the reaction temperature to -10°C. After the reaction is completed, filtering the reaction to obtain a hydrophobic treatment agent;
[0038] (3) Under nitrogen protection, the specific surface area of 150m 2 / g hydrophilic precipitated silica ① and a hydrophobic treatment agent are evenly mixed, the mass of the hydrophobic treatment agent is 10% of the mass of the hydrophilic silica, heated to 60°C with stirring, reacted for 2h, and the vacuum degree is -0.04MPa to obtain reactive hydrophobic silica 1.
[0039] Example 2
[0040] The method for preparing the reactive hydrophobic silica comprises the following steps:
[0041] (1) adding water to dimethyldichlorosilane, with the molar ratio of dimethyldichlorosilane to water being 10:9, and slowly hydrolyzing the mixture while controlling the reaction temperature to 15°C to obtain an incomplete hydrolyzate;
[0042] (2) introducing ammonia gas at a rate of 10% of the mass of the hydrolyzate into the incomplete hydrolyzate at a constant speed within 30 minutes, stirring the reaction, and controlling the reaction temperature at 10°C. After the reaction is completed, filtering the reaction to obtain a hydrophobic treatment agent;
[0043] (3) Under argon protection, a 2 / g hydrophilic fumed silica ② and a hydrophobic treatment agent are evenly mixed, the mass of the hydrophobic treatment agent is 15% of the mass of the hydrophilic silica, heated to 100°C with stirring, reacted for 4h, and the vacuum degree is -0.08MPa to obtain reactive hydrophobic silica 2.
[0044] Example 3
[0045] The method for preparing the reactive hydrophobic silica comprises the following steps:
[0046] (1) adding water to dimethyldichlorosilane, with the molar ratio of dimethyldichlorosilane to water being 7:6, and slowly hydrolyzing the mixture while controlling the reaction temperature to 10°C to obtain an incomplete hydrolyzate;
[0047] (2) introducing ammonia gas at a rate of 15% of the mass of the hydrolyzate into the incomplete hydrolyzate at a constant speed within 30 minutes, stirring the reaction, and controlling the reaction temperature to 0°C. After the reaction is completed, filtering the reaction to obtain a hydrophobic treatment agent;
[0048] (3) Under nitrogen protection, the specific surface area of 380m 2 / g hydrophilic fumed silica ③ and a hydrophobic treatment agent are evenly mixed, the mass of the hydrophobic treatment agent is 20% of the mass of the hydrophilic silica, heated to 130°C with stirring, reacted for 6h, and the vacuum degree is -0.06MPa to obtain reactive hydrophobic silica 3.
[0049] The treated and untreated white carbon black in the above examples were used as raw materials to prepare rubber compounds. Information on other raw materials used is shown in Tables 1 and 2 below.
[0050] Table 1 Raw rubber raw material information
[0051]
[0052] Table 2 Hydroxy silicone oil raw material information
[0053]
[0054] Formula process:
[0055] Comparative test of white carbon black ① and white carbon black 1:
[0056] White carbon black①: 110-8s: 750g, 110-7sk: 33g, white carbon black①: 360g, hydroxy silicone oil: 24g, zinc stearate: 1.3g.
[0057] White carbon black 1: 110-8s: 750g, 110-7sk: 33g, white carbon black 1: 120g, white carbon black ①: 240g, hydroxy silicone oil: 11g, zinc stearate: 1.3g.
[0058] Comparative test of white carbon black ② and white carbon black 2:
[0059] White carbon black ②: 110-8s: 750g, 110-7sk: 33g, white carbon black ②: 360g, hydroxy silicone oil: 38g, zinc stearate: 1.3g.
[0060] White carbon black 2: 110-8s: 750g, 110-7sk: 33g, white carbon black 2: 120g, white carbon black ②: 240g, hydroxy silicone oil: 20g, zinc stearate: 1.3g.
[0061] Comparative test of white carbon black ③ and white carbon black 3:
[0062] White carbon black ③: 110-8s: 750g, 110-7sk: 33g, white carbon black ③: 360g, hydroxy silicone oil: 50g, zinc stearate: 1.3g.
[0063] Silica gel 2: 110-8s: 750g, 110-7sk: 33g, Silica gel 3: 120g, Silica gel ③: 240g, Hydroxy silicone oil: 28g, Zinc stearate: 1.3g.
[0064] Rubber mixing process: Add all the raw rubber, 150g of white carbon black (when treating white carbon black, the ratio of the two types of white carbon black added each time is consistent with the total ratio), hydroxy silicone oil and zinc stearate into a kneader and knead into a mass. Then add the remaining white carbon black in 5 times. After all the white carbon black is added, knead evenly and mix at 150℃ for 2h to obtain the mixed rubber.
[0065] The mixed rubber is vulcanized to prepare silicone rubber, and the vulcanization process is as follows:
[0066] Take 70g of the mixed rubber, add 1wt.% of D25 premixed rubber and mix evenly on a double-roll mill, then thinly pass it 6 times to sheet; the D25 premixed rubber is a mixture of 2,5-bis(tert-butyl)-2,5-dimethylhexane and polydimethylsiloxane raw rubber with a molecular weight of 600,000-700,000 in a mass ratio of 1:1; vulcanize on a flat vulcanizer at 170℃×6.5min to obtain silicone rubber. The obtained silicone rubber was subjected to mechanical property tests, including: structural condition: 7d plasticity value growth rate was tested by GBT 12828-2006, determination of plasticity value and recovery value of raw rubber and unvulcanized mixed rubber, parallel plate method, tensile strength was tested by GB / T 528-2009 determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber, elongation at break was tested by GB / T 528-2009 determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber, tear strength was tested by GB / T 529-2008 determination of tear strength of vulcanized rubber or thermoplastic rubber, and hardness was tested by GB / T 6031-2017 determination of hardness of vulcanized rubber or thermoplastic rubber. The results are shown in Table 3 below:
[0067] Table 3 Silicone rubber mechanical properties test
[0068]
[0069] From the above comparison, it can be seen that the reactive hydrophobic silica prepared by the present invention as a part of the reinforcing agent shows advantages in mechanical properties, which is generally better than the silicone rubber prepared by the traditional process.
[0070] Structured Situation Assessment:
[0071] The mixed rubber was stored at room temperature, and samples were taken at the initial stage, 1d, 3d, and 7d after production to test the plasticity value. The results are shown in Table 4:
[0072] Table 4 Plasticity value test results
[0073]
[0074] Through the above comparison, the plasticity value of the rubber compound prepared by using the reactive hydrophobic silica prepared by the present invention increases slowly, thereby it can be determined that the rubber compound has better anti-structural performance and shelf life.
[0075] The carbon content of treated and untreated white carbon black in the above embodiment was tested using the GB / T20020-2013 fumed silica test method. The results are shown in Table 5 below:
[0076] Table 5 Carbon content test results
[0077]
[0078] It can be seen from the above table that the surface grafting rate of the hydrophobic silica prepared in the embodiment of the present invention is high.
Claims
1. A method for preparing a reactive hydrophobic silica, characterized in that: The following steps are involved: (1) adding water to dimethyldichlorosilane to carry out a hydrolysis reaction to obtain an incomplete hydrolyzate; (2) introducing ammonia gas into the incomplete hydrolyzate for reaction, filtering, and obtaining a hydrophobic treatment agent; (3) mixing the hydrophilic silica and the hydrophobic treatment agent uniformly, heating and stirring to react, and vacuum treating to obtain reactive hydrophobic silica; The molar ratio of dimethyldichlorosilane to water in step (1) is 4:3 to 10:9; The temperature of the hydrolysis reaction in step (1) is 1-15°C; The amount of ammonia used in step (2) is 10-30% of the amount of the incomplete hydrolyzate; The reaction temperature of the reaction in step (2) is -10~10°C; The reaction temperature of the reaction in step (3) is 60-130° C., the reaction time is 2-6 hours, and the vacuum degree of the vacuum treatment is -0.04-0.08 MPa.
2. The method for preparing reactive hydrophobic silica according to claim 1, characterized in that: The hydrophilic silica in step (3) is hydrophilic fumed silica or hydrophilic precipitated silica.
3. The method for preparing reactive hydrophobic silica according to claim 2, characterized in that: The surface area of the hydrophilic silica in step (3) is 150-380 m 2 / g.
4. The method for preparing reactive hydrophobic silica according to claim 1, characterized in that: The amount of the hydrophobic treatment agent used in step (3) is 10-20% of the mass of the hydrophilic silica.
5. The method for preparing reactive hydrophobic silica according to claim 1, characterized in that: In step (3), the hydrophilic silica and the hydrophobic treatment agent are mixed evenly, and the heating and stirring reaction is carried out under the protection of an inert gas.
Citation Information
Patent Citations
Method for preparing white carbon black modified by silane coupling agent
CN102220036A
Surface treated metallic oxide fine powder and preparation and use thereof
CN101200601A
Bladder for tire production
CN101392098A
Non-cohesive high temperature resistant organic silicon sealant and preparation method thereof