Production Technology of S355J2 Hot-rolled H-shaped Steel for Ce-containing Beam-column Components
By using ferrocerium alloy and rare earth composite inclusions in the hot-rolled H-shaped steel production of rectangular billets, the problem of poor utilization of rare earths in the profile is solved, and the production of low-cost and high-performance S355J2 hot-rolled H-shaped steel is achieved, ensuring the product stability and uniformity.
Patent Information
- Application Number
- CN202411162596.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-23
AI Technical Summary
In the existing hot-rolled H-shaped steel production process, the special-formed blank is not suitable for adding a large amount of rare earths during the steel smelting, and it is difficult to achieve continuous casting, resulting in uneven product quality and high cost. The production process of rectangular blanks is simple but not suitable for high efficiency of rare earths. use.
Using rectangular blanks as raw materials, ferrocerium alloy as additives, combined with double slag smelting method and continuous casting process, control smelting and rolling conditions, ensure the stability and refining of components, add rare earths to form rare earth composite inclusions, and improve the cleanliness of steel and mechanical properties.
The production of low-cost and high-performance S355J2 hot-rolled H-shaped steel is realized, ensuring the stability and uniformity of the multi-stage performance of the steel, and improving the metal utilization and mechanical properties through narrow component control.
Smart Images

Figure CN118668140B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the production of hot-rolled H-shaped steel, in particular to a production process of S355J2 hot-rolled H-shaped steel for Ce-containing beam and column components. Background Art
[0002] Steel companies continue to explore the research of adding rare earth elements to steel, and currently still face some technical and application challenges, such as the method of adding rare earths, the amount of addition, the mechanism of action of rare earths in steel, etc. Domestic research shows that rare earths have two main functions in steel: one is to purify molten steel and improve the quality of steel by modifying inclusions with rare earths; the other is to further optimize the performance of steel through rare earth microalloying.
[0003] At present, the production process of hot-rolled H-beam is mainly divided into two categories:
[0004] One type is to use special-shaped blanks to pass through a rough rolling mill and an edge rolling mill for reciprocating continuous rolling, and then continue to reciprocate and continuously roll on a universal finishing mill and an edge rolling mill to obtain the finished product.
[0005] The other type is to use a rectangular billet that is heated and then rolled into an I-shaped profiled billet on a billet opening machine, and then sent to a multi-stand universal rolling mill for continuous hot rolling to obtain the finished product.
[0006] There are significant differences in the manufacturing process between profiled billets and rectangular billets. The profiled billet crystallizer has 12 faces and 12 corners, which makes the billet shell more uneven and the inner cavity thinner. Therefore, factors such as gas in steel, molten steel cleanliness, drawing speed, Mn / S ratio, cooling rate, and protective slag have a more significant impact on the quality of profiled billets. In addition, profiled billets are usually cast with double nozzles. Due to the small diameter of the nozzle, problems such as liquid level fluctuation, flocculation, and flocculation are prone to occur when producing profiled billets containing aluminum or rare earths, which can lead to cracks in the belly of the profiled billet. In contrast, the production of rectangular billets can effectively avoid the above-mentioned surface quality problems, and hot continuous rolling is often used in the rolling process, which reduces the manufacturing cost of the casting billet and the rolling process cost.
[0007] Given the restrictive conditions in the production of profiled billets, this type of billet is not suitable for adding a large amount of rare earths during molten steel smelting and is difficult to achieve continuous pouring. On the contrary, the rectangular billet has a simple manufacturing process, stable performance and low cost. Its larger pouring nozzle diameter and wide rolling process window allow for the addition of a larger amount of rare earths during molten steel smelting and continuous pouring.
[0008] Rare earths can purify and modify inclusions in molten steel, and these properties match the characteristics of rectangular billet production lines. By adding rare earths to existing building materials, the goal is to improve the cleanliness of steel by modifying inclusions, so that the product can meet the performance requirements at both room temperature and low temperature. The goal is to develop a set of universal process parameters and technical procedures with strong operability for mass production of low-cost, high-performance rare earth construction steel.
[0009] Domestic research also shows that rare earths can promote the precipitation of Nb (niobium) in steel, improve the utilization rate of vanadium-niobium alloy elements, and use rare earths to purify molten steel and modify inclusions, thereby improving the mechanical properties of steel and reducing costs. Therefore, this technology focuses on a preparation process for producing hot-rolled H-beams based on rare earth modified rectangular billet inclusions. Summary of the invention
[0010] The present invention aims at the defects of the prior art and provides a production process of S355J2 hot-rolled H-shaped steel for Ce-containing beam and column components.
[0011] To achieve the above object, the present invention adopts the following technical solution: S355J2 hot-rolled H-shaped steel for Ce beam-column components, characterized in that, in terms of mass fraction, the hot-rolled H-shaped steel components are:
[0012] C: 0.18%-0.20%, Si: 0.25%-0.30%, Mn: 1.22%-1.27%, P≤0.025%, S≤0.025%, Nb: 0.008%-0.011%, V: 0.008%-0.012%, N: 0.004%-0.008%, Ce: 0.0015%-0.0055%, Al≤0.015%, the rest are Fe and unavoidable impurities.
[0013] Furthermore, ferrocerium alloy is used as an additive in the preparation process of hot-rolled H-beam (the chemical composition of the ferrocerium alloy is calculated by mass fraction). The index control range of the ferrocerium alloy is: the mass fraction of Ce is 29.9%-30.9%, the mass fraction of O is 0.0045%-0.0080%, the mass fraction of C is 0.013%-0.015%, the mass fraction of Si is 0.012%-0.013%, the mass fraction of Mn is 0.09%-0.012%, the mass fraction of P is less than 0.010%, and the mass fraction of S is less than 0.0050%. The rest is Fe and unavoidable impurities.
[0014] The production process of hot-rolled H-beam includes the following steps:
[0015] S1. Smelting of hot-rolled H-beam;
[0016] S2, continuous casting operation;
[0017] S3. Rolling operation.
[0018] Furthermore, S1 includes:
[0019] 1.1 Loading: Control the loading amount to 115±2 tons, of which the P content in the molten iron is ≤0.120%, and the S content in the molten iron is ≤0.040%; and control the steel output to 110 tons to achieve component stability and refining treatment;
[0020] 1.2 Oxygen supply and slag making: The working oxygen pressure during steelmaking is controlled between 0.8Mpa and 1.4Mpa, the oxygen flow rate is within the range of 16500 to 19000m³ / h, and the terminal pressure gun duration is greater than 40 seconds;
[0021] The double slag smelting method is adopted. The amount of lime added is adjusted according to the silicon content of the molten iron. The initial slag basicity is controlled between 1.5 and 2.0, the slag basicity is between 2.8 and 3.2, and the magnesium oxide content is 8%, so as to control the smelting cycle to 40 to 50 minutes per furnace;
[0022] 1.3 End point composition control: During spot blowing, adjust the flow rate to above 18000m³ / h after 1 minute of spot blowing to ensure that the carbon composition of the steel after one spot blowing meets the steel tapping requirements. The end point composition is controlled at C≥0.06%, P≤0.030%, S≤0.030%, and the steel must be tapped in the same sample to ensure the accuracy of carbon addition;
[0023] 1.4 End point temperature control: control the opening temperature between 1600℃ and 1700℃, and the continuous pouring temperature between 1650℃ and 1680℃;
[0024] 1.5 Deoxidation and alloying: Alloys are added along with the steel flow. The order of adding alloys is: first add deoxidation as the main element, then add alloying elements, i.e. aluminum block - ferrosilicon - manganese silicon - vanadium nitrogen alloy; and start adding when 1 / 3 of the steel is tapped, and add all alloys before 2 / 3 of the steel is tapped. At the same time, use slag cones to ensure that the thickness of the ladle slag layer does not exceed 55mm, so as to stabilize the alloy recovery rate and avoid rephosphorization of molten steel;
[0025] 1.6 Argon blowing and temperature control after argon blowing: Argon is blown throughout the steel-making process to ensure that the slag blocking rate reaches 100%;
[0026] Carry out deoxidation alloying operation: aluminum block - ferrosilicon - manganese silicon - vanadium nitrogen - ferroniobium, start adding alloy when the steel is 1 / 3 tapped, and finish adding before the steel is 3 / 4 tapped;
[0027] Argon blowing control at the argon station: the total argon blowing time is 13 minutes. After adding the ferrocerium rare earth alloy, the steel-loading operation is carried out. After the argon, the strong blowing is controlled for 3 minutes. The soft blowing time is ≥ 7 minutes, and the diameter of the exposed molten steel during soft blowing is not more than 200 mm.
[0028] Furthermore, S2 includes:
[0029] 2.1. The pouring temperature is controlled at 1550℃-1580℃, and the tundish temperature is controlled at 1530℃-1550℃;
[0030] 2.2. When the liquid level in the tundish exceeds 400mm, start pouring and quickly recover to 800mm or above for continuous pouring;
[0031] 2.3. Control the casting speed as follows:
[0032] For the section of 320mm×410mm, the speed of initial pouring is 0.40-0.55m / min, and the speed of continuous pouring is 0.6-0.80m / min;
[0033] For the 230mm×350mm section, the initial pouring speed is 0.8-1.0m / min, and the continuous pouring speed is 1.0-1.50m / min;
[0034] 2.4. The straightening temperature of continuous casting billet is controlled above 880℃;
[0035] 2.5. During the continuous casting process, the liquid level in the tundish should be controlled to be ≤200mm.
[0036] Furthermore, S3 includes:
[0037] 3.1. Billet differentiation: When changing the steel type, two refractory bricks are placed on the continuous casting billet or two positions are left empty to differentiate billets of different batches;
[0038] 3.2. Heating furnace temperature control: for billets of different sizes, control the temperature of each section of the heating furnace and the time in the furnace, specifically:
[0039] For the steel billet with a cross section of 230mm×230mm, the temperatures of the heating sections during hot charging are ≤1060℃ for the first section, 1210℃-1250℃ for the second section, 1260℃-1310℃ for the third section, 1250℃-1300℃ for the soaking section, and 150min-180min for the furnace time; the temperatures of the heating sections during cold charging are ≤1100℃ for the first section, 1210℃-1260℃ for the second section, 1260℃-1310℃ for the third section, 1250℃-1315℃ for the soaking section, and 150min-210min for the furnace time;
[0040] For the steel billet with a cross section of 320mm×410mm, the temperatures of the heating sections during hot charging are ≤1060℃ for the first section, 1210℃-1250℃ for the second section, 1260℃-1300℃ for the third section, 1250℃-1300℃ for the soaking section, and 150min-180min for the furnace time; the temperatures of the heating sections during cold charging are ≤1100℃ for the first section, 1210℃-1260℃ for the second section, 1260℃-1310℃ for the third section, 1250℃-1315℃ for the soaking section, and 150min-210min for the furnace time;
[0041] 3.3. Rolling process temperature control: Set the start rolling temperature, finishing rolling temperature and upper cooling bed temperature respectively, specifically:
[0042] The starting rolling temperature of hot-charged steel billet is 1150±30℃, the finishing rolling temperature is 1000-1090℃, and the upper cooling bed temperature is 800-950℃;
[0043] The starting rolling temperature of cold-charged steel billet is 1150±40℃, the finishing rolling temperature is 1000-1090℃, and the upper cooling bed temperature is 800-950℃;
[0044] Descaling operation: During the descaling process, the water pressure is controlled at more than 19Mpa and the billet running speed is 1.0m / s to ensure that the iron oxide scale on the billet surface is removed.
[0045] Compared with the prior art, the present invention has beneficial effects.
[0046] The production process of S355J2 hot-rolled H-shaped steel for Ce-containing beam and column components of the present invention can ensure the performance of the hot-rolled H-shaped steel in multiple grades, low cost, stability, uniformity and consistency, and narrow composition control of each element. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] The present invention is further described below in conjunction with the accompanying drawings and specific implementation methods. The protection scope of the present invention is not limited to the following description.
[0048] Figure 1 This is the morphology of steel slag without rare earth added before argon;
[0049] Figure 2 Morphology of steel slag with rare earth added after argon;
[0050] Figure 3 This is the inclusion morphology of type A sulfide without rare earth addition;
[0051] Figure 4 This is the C-type silicate inclusion morphology without rare earth addition;
[0052] Figure 5 S355J2 (Re) strip structure (pearlite + ferrite) with rare earth added;
[0053] Figure 6 The polygonal ferrite morphology of S355J2 (Re) with rare earth added;
[0054] Figure 7 The morphology of S355J2 (Re) A-type sulfide inclusions;
[0055] Figure 8 It is the S355J2 (Re) C type silicate inclusion morphology;
[0056] Fig. 9 This is the SEM composite rare earth inclusion morphology of S355J2 (Re) 101# sample;
[0057] Fig.10 This is the morphology and energy spectrum analysis area of 101#SEM composite rare earth inclusions;
[0058] Fig.11 Energy spectrum analysis of 101# composite rare earth inclusions;
[0059] Fig.12 This is the SEM composite rare earth inclusion morphology of S355J2 (Re) 102#;
[0060] Fig.13 This is the energy spectrum analysis diagram of 102# composite rare earth inclusions;
[0061] Fig.14 This is the EDS composite rare earth inclusion morphology;
[0062] Fig.15 This is the distribution diagram of each element in the morphology of EDS composite rare earth inclusions;
[0063] Fig.16 Sulfide fracture morphology;
[0064] Fig.17 Aspect ratio of inclusions after rare earth treatment;
[0065] Fig.18 Inclusion size distribution histogram;
[0066] Fig.19 Composition of inclusions of different sizes;
[0067] Fig. 20 Proportions of different inclusion types;
[0068] Fig.21 Impact fracture morphology. DETAILED DESCRIPTION
[0069] In order to better understand the technical solution of the present invention, a specific implementation scheme is provided as follows; and the following scheme is only for illustration.
[0070] Example 1: Production process of S355J2 hot-rolled H-beam for beam and column components
[0071] The production process is as follows: blast furnace molten iron - molten iron pretreatment - converter top and bottom double blowing smelting - billet continuous casting - billet loading - walking beam heating furnace - high-pressure water one-time dephosphorization - billet opening - 11-stand universal continuous rolling - hot saw sampling - walking beam cooling bed cooling - straightening - shape and surface quality inspection - sawing.
[0072] Key control parameters: The components and weight percentages of the cerium-containing S355J2 hot-rolled H-beam in this embodiment are:
[0073] (1) The mass fraction of C is 0.19%, the mass fraction of Si is 0.27%, the mass fraction of Mn is 1.23%, the mass fraction of P is 0.021%, the mass fraction of S is 0.022%, the mass fraction of V is 0.012%, the mass fraction of Nb is 0.010%, and the mass fraction of Ce is 0.0032%. The rest is Fe and unavoidable impurities.
[0074] (2) The molten iron loading is 110 tons, the scrap steel loading is 5.2 tons, the total loading is 115.2 tons, and the molten iron temperature is 1354℃.
[0075] (3) Composition of molten iron entering the furnace: 0.63% Si, 0.104% Mn, 0.076% P, 0.024% S.
[0076] (4) Add 3030 kg of lime, 1255 kg of limestone, 850 kg of sintered ore, 3240 kg of raw dolomite and 1840 kg of coarse magnetite.
[0077] (5) The temperature of the converter at the station is 1610℃, the upper steel temperature is 1563℃, 1870kg of silicon manganese, 120kg of carburizer, 10kg of vanadium nitrogen alloy, 15kg of ferroniobium, and 30kg of aluminum ingot are added to the alloy. Strong blowing is for 3 minutes, soft blowing is for 10 minutes, and spot blowing time is for 10 seconds. 80kg of silicon manganese, 10kg of carburizer, and 10kg of vanadium nitrogen alloy are added to the alloy.
[0078] (6) Argon should be blown throughout the steel-making process to avoid slag formation, and the slag blocking rate should be 100%; deoxidation and alloying operation: aluminum block - ferrosilicon - manganese silicon - vanadium nitrogen - ferroniobium, alloy is added when the steel is 1 / 3 of the way through, and all the alloys are added before the steel is 3 / 4 of the way through.
[0079] (7) Control of ferrocerium addition: After blowing argon for 3 minutes at the argon station, add ferrocerium alloy.
[0080] (8) Argon blowing control at the argon station: The total argon blowing time at the argon station is 13 minutes. After blowing argon for 3 minutes, 35 kg of ferrocerium rare earth alloy is added for steel-loading operation.
[0081] (9) Composition of converter slag before argon: 34.46%CaO, 13.87%MnO, 1.39%TiO2, 32.01%SiO2, 6.74%MgO, 1.98%Fe2O3, 10.89%Al2O3, Ce<0.0005%, slag morphology see Figure 1 ; The composition of the converter slag after argon treatment is: 31.34%CaO, 12.15%MnO, 1.41%TiO2, 34.00%SiO2, 6.51%MgO, 2.69%Fe2O3, 11.29%Al2O3, 0.163%Ce, and the morphology of the slag is shown in Figure 2 .
[0082] (10) Composition at the converter end point: C by mass 0.19%, Si by mass 0.27%, Mn by mass 1.23%, P by mass 0.021%, S by mass 0.022%, V by mass 0.012%, Nb by mass 0.010%, Ce by mass 0.0032%.
[0083] (11) 5-strand casting, casting speed 0.5m / min, no casting speed fluctuation phenomenon, the liquid slag layer thickness was measured to be 10mm during the casting process, the internal slag layer structure was normal without any agglomeration or slag flipping phenomenon, the offline submerged nozzle tracking showed no nodule phenomenon inside, and the overall casting process was good.
[0084] (12) The temperature of the soaking section of the heating furnace is 1280°C, the billet opening temperature is 1150°C, the finishing rolling temperature is 1059°C, the finishing rolling exit temperature is 959°C, and the upper cooling bed temperature is 895°C.
[0085] 2. Effect of Ce on slag composition
[0086] In order to fully compare the changes in steel slag before and after the addition of rare earth, the slag sample was taken after the molten steel was blown for 3 minutes at the argon station, and the ferrocerium rare earth alloy was added after blowing argon for 3 minutes. After the total blowing time of argon at the argon station was 13 minutes, the slag sample was taken again and the steel was put into operation.
[0087] Slag morphology Figure 1 and Figure 2 It can be seen that the steel slag is black before rare earth is added. Figure 1 In the process of smelting, black steel slag contains a large amount of iron and other metal oxides. This kind of steel slag shows obvious black color due to the presence of iron, and the surface is relatively rough, showing a block or flaky structure. Black steel slag is rich in iron and other metal elements, and the metal utilization rate is low. After blowing argon for 3 minutes, the steel slag with ferrocerium rare earth alloy added has a green glass-like morphology, a smooth surface, uniform color, and a dense internal structure. Through the comparative analysis of steel slag components, it can be seen that the metal utilization rate is significantly increased after adding rare earth.
[0088] See Table 1 for the comparison of slag composition before and after argon without rare earth addition. The total oxygen content of S355J2 before and after argon is basically unchanged, and the total oxygen of S355J2 (Ce) after argon is reduced by 8.64 compared with that before argon. The metal utilization rate of S355J2 after argon is unchanged, and the metal utilization rates of manganese and iron of S355J2 (Ce) after argon are increased by 2.82% and 5.82% respectively.
[0089] Table 1 Comparison of steel slag composition without rare earth before argon and with rare earth after argon Wt%
[0090]
[0091] 3. Effect of Ce on high magnification structure and denatured inclusions
[0092] 3.1 Metallographic structure and rare earth inclusion composition
[0093] The inclusions in steel can be divided into: A-type sulfide inclusions, B-type alumina inclusions, C-type silicate inclusions, D-type spherical oxide inclusions, and Ds-type single-particle spherical oxide inclusions. The inclusions in the hot-rolled S355J2 steel produced by the company are arranged in one or more rows along the rolling line direction. Figure 3 , Figure 4 This long strip-shaped inclusion is embedded in the steel matrix, which has a destructive effect on the continuity of the steel matrix. It is subjected to stress during subsequent processing, welding and service, becomes a stress concentration point, causes damage to the matrix, and thus leads to failure of the beam column during service.
[0094] According to the metal microstructure inspection method GB / T13298-2015 and the metal average grain size determination method GB / T6394-2017, it can be seen from the figure that the structures of S355J2 (Re) steels in the three heats of 101#, 102# and 103# are the same. Using the ZEISS Axiovert40 metallographic microscope, the main structures are polygonal ferrite and pearlite bands along the rolling direction, such as Figure 5 , Figure 6 Table 2 shows the chemical composition of S355J2 (Re) produced by three furnaces.
[0095] Table 2 Chemical composition of S355J2 (Re) Wt%
[0096]
[0097] The rare earth inclusion rating of sample #101 is: A (sulfide) 0.5 level, B (alumina) 0.5 level, C (silicate) 1.0 level; the inclusion rating of sample #102 is: A (sulfide) 2.0 level, B (alumina) 0.5 level, C (silicate) 2.0 level; the inclusion rating of sample #103 is: A (sulfide) 0.5 level, B (alumina) 1.5 level, C (silicate) 1.5 level. In the S355J2 steel produced by the enterprise without adding rare earth, the A-type sulfide is in the form of gray long strips with rounded ends. In the S355J2 (Re) samples with rare earth 101#, 102#, and 103# added, the A-type sulfide is in the form of short rods or ellipsoids, and some A-type sulfides have black cones at the ends. The A-type sulfides in S355J2 (Re) are rare earth composite inclusions ARES (rare earth sulfides), such as Figure 3 , Figure 4 Compared with the S355J2 steel produced by the enterprise without adding rare earth, the C-type silicate is in the form of black or dark gray strips. The C-type silicate in the S355J2 (Re) samples with rare earth 101#, 102#, and 103# added is in the form of strips, but the strips appear in a crystalline glass state, which is a composite inclusion formed by sulfide and silicate. Figure 7 , Figure 8 .
[0098] 3.2 Effect of rare earth on inclusion morphology and size
[0099] The rare earth Ce element has extremely high chemical activity. The absolute value of the standard Gibbs free energy of formation of Ce2O3 in molten steel is equivalent to that of CaO, and its deoxidation and desulfurization capabilities are excellent. When rare earth Ce is added to molten steel, a series of reactions will occur. The priority order of desulfurization and deoxidation reactions of 1 mol Ce at 1873K is CeO2→Ce2O3→Ce2O2S→Ce2S3→Ce3S4→CeS. From thermodynamics, it can be seen that the chemical properties of rare earth Ce are active. After adding Ce to molten steel, it will react with elements such as O and S before Al and Mn to form rare earth inclusions, and will also react with oxide and silicate inclusions to form composite inclusions. After rare earth Ce is added to steel, the inclusions are obviously deteriorated and spherical, or rare earth Ce can turn long strip inclusions into short rod-shaped, ellipsoidal or spherical composite inclusions, thereby reducing stress concentration and improving mechanical properties.
[0100] Fig. 9 , Fig.10 This is a scanning electron microscope image of the morphology of 101# with composite rare earth inclusions. Fig.11Energy spectrum analysis of composite rare earth inclusions. The formed rare earth composite inclusions are small in size and elliptical in shape with smooth edges. The rare earth elements show a trend of surrounding manganese sulfide inclusions. Through energy spectrum analysis, it can be seen that the inclusions contain C, O, Si, Al, Ca, Fe, Mn, S, and Ce elements. The statistical analysis results are shown in Table 3.
[0101] Fig.12 This is a scanning electron microscope image of the morphology of 102# with composite rare earth inclusions. Fig.13 This is the energy spectrum analysis of composite rare earth inclusions. The formed rare earth composite inclusions are small in size and elliptical in shape with smooth edges. The rare earth elements show a trend of wrapping manganese sulfide inclusions from both ends to the middle. Through energy spectrum analysis, it can be seen that the inclusions contain C, O, Si, Al, Ca, Fe, Mn, S, and Ce elements. The statistical analysis results are shown in Table 4. Spectra 28, Spectra 29, Spectra 30, and Spectra 31 correspond to Fig. 9 , Fig.10 The point scanning positions in the graphs 59, 60, and 61 correspond to Fig.12 The point scan position in .
[0102] Table 3 Quantitative element content Wt% in different regions of 101# composite rare earth inclusions
[0103]
[0104] Table 4 Quantitative element content Wt% in different regions of 102# composite rare earth inclusions
[0105]
[0106] from Fig.14 , Fig.15 The element distribution and element enrichment areas in the inclusions can be seen in the scanned images. The rare earth element Ce in the inclusions is enriched in the black head area protruding around the inclusions and at the ends. This area is also rich in Si and Al elements. Mn and S elements are enriched in the middle area. From the growth trend of the inclusions, it can be seen that the rare earth Ce, Si, and Al elements coated on the periphery have a tendency to wrap the middle MnS inclusion around and form an ellipsoidal rare earth composite inclusion.
[0107] Rare earth elements are generally added after the molten steel is deoxidized and desulfurized. At this time, rare earth elements can modify the oxide and sulfide inclusions in the molten steel to generate small, nearly spherical rare earth compounds. The thermal expansion coefficients of MnS and Al2O3 are 18.1×10 -6 / ℃ and 8.0×10 -6 / ℃, and the thermal expansion coefficient of the iron matrix is 12.5×10 -6 / ℃ is very different. During the hot processing of steel, not only will stress fields be formed to cause crack sources, which will harm the mechanical properties of steel, but also the inclusions will be disconnected from the surrounding matrix and cause corrosion. The thermal expansion coefficient of rare earth inclusions is 11.5×10 -6 / ℃, which is very close to the iron matrix, so the fine rare earth inclusions will eliminate the adverse effects of conventional inclusions on steel.
[0108] The method of obtaining fine rare earth inclusions is to make the oxygen and sulfur content in the molten steel as low as possible. In addition, there is an appropriate range for rare earth content. Once the steel is impure or too much rare earth is added, the generated composite compounds will aggregate into larger particles, forming string inclusions after rolling, and RE-Fe brittle intermetallic compounds will be produced, deteriorating the performance of the steel. It is generally believed that fine rare earth inclusions can be obtained when RE / (O+S)>0.8.
[0109] 3.3 Analysis of size and quantity of rare earth inclusions
[0110] The rare earth inclusion rating of sample 101#: A (sulfide) 0.5, B (alumina) 0.5, C (silicate) 1.0; the inclusion rating of sample 102#: A (sulfide) 2.0, B (alumina) 0.5, C (silicate) 2.0; the inclusion rating of sample 103#: A (sulfide) 0.5, B (alumina) 1.5, C (silicate) 1.5. From the inclusion rating of the three samples, it can be seen that the inclusion types are mainly sulfide and silicate types. When the A-type inclusion is long and the length range is 37um-436um, the inclusion will first be truncated. When the inclusion becomes small, it can further form rare earth composite inclusions. Fig.16 This is a photo of sulfide fracture magnified 10,000 times.
[0111] After rare earth was added to the three batches of test steel, the inclusions in the samples tended to be elliptical in size and increased in size, with the aspect ratio concentrated in the range of 2:1 to 6:1. In addition, rare earth Ce was found in the composite inclusions, proving that Ce added to the steel modified the inclusions, making the single flat MnS inclusion tend to generate small-sized elliptical MnS, and composited with the rare earth Al and Si inclusions. The aspect ratio of the rare earth composite inclusions is shown in Figure 1. Fig.17 The size of composite rare earth inclusions is mostly below 37um.
[0112] The number of composite rare earth inclusions in industrial production samples 101#, 102#, and 103# was counted. The field emission electron scanning electron microscope was used to perform regional scanning at a magnification of 601 times. The scanning time was 58.2 minutes, the field of view area was 3276075μm², the total number of fields of view was 121, and the total scanning time was four hours. The OTS software was used for data analysis and statistics. As shown in Table 5, it can be seen that the inclusion size is concentrated in 2-30um. Fig.18 is the inclusion size histogram, Fig.19 It is composed of different size inclusion types. Fig. 20 The proportion of different inclusion types, the proportion of composite rare earth inclusion modification is 0.03-0.12%.
[0113] Table 5 Analysis results of inclusion particle size
[0114]
[0115] 4. Impact of Ce on Performance
[0116] Adding a small amount of rare earth to steel can significantly improve the strength and plasticity of steel. There is a suitable amount of rare earth elements to affect the mechanical properties of S355J2. The presence of low-melting-point metal elements will reduce the impact toughness of the material, so adding various rare earth elements can improve the impact toughness of the material. The reason why rare earth elements affect impact performance is the influence of rare earth elements on grain boundaries and inclusions. Rare earth elements improve the strength of grain boundaries through grain boundary purification and inclusion modification, and reduce the possibility of cracks extending through defects, so that the material can absorb more crack extension energy when subjected to impact loads. However, when rare earth elements are added in excess, brittle and hard rare earth non-metallic inclusions and intermetallic compounds are formed, the grain boundary strength is weakened, and the impact performance of the material is deteriorated.
[0117] Table 6 shows the properties of the rare earth added test steel. Under the same process, the effects of adding rare earth and not adding rare earth on impact toughness are compared. The results show that rare earth elements change the properties and shapes of inclusions, and transform the strip-shaped plastic MnS inclusions into spherical rare earth sulfide oxides that are difficult to deform. Therefore, during rolling, the inclusions will not elongate along the rolling direction, and the spherical inclusions greatly reduce the stress concentration caused by the strip-shaped inclusions, and are not prone to transverse fracture, thereby significantly improving the impact energy value and improving the comprehensive performance of the steel plate.
[0118] Fig.21 As for the impact fracture morphology, from the mechanical test data of industrial rare earth steel products, the strength of S355J2 (Re) meets the technical requirements, KV2 (20℃)>110J, KV2 (0℃)>78J, KV2 (-20℃)>46.8J, the fracture surface reduction rate>70%, and the toughness value meets the 0℃ impact toughness, -20℃ impact toughness, and transverse 20℃ impact toughness at the same time. The alloy cost remains unchanged. From the average impact toughness value, it can be seen that the series impact values of S355J2 (Re) are all higher than S355J2.
[0119] Table 6 Comparison of mechanical properties of S355J2 (Re) and S355J2
[0120]
[0121] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, it should be understood by those skilled in the art that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features therein may be replaced by equivalents. Therefore, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope defined by the claims of the present invention.
Claims
1. S355J2 hot-rolled H-shaped steel for Ce-containing beam and column components, characterized in that: in terms of mass fraction, the hot-rolled H-shaped steel components are: C: 0.18%-0.20%, Si: 0.25%-0.30%, Mn: 1.22%-1.27%, P≤0.025%, S≤0.025%, Nb: 0.008%-0.011%, V: 0.008%-0.012%, N: 0.004%-0.008%, Ce: 0.0015%-0.0055%, Al≤0.015%, the rest are Fe and unavoidable impurities; Ferrocerium alloy is used as an additive in the preparation process of hot-rolled H-shaped steel, and the index control range of the ferrocerium alloy is: the mass fraction of Ce is 29.9%-30.9%, the mass fraction of O is 0.0045%-0.0080%, the mass fraction of C is 0.013%-0.015%, the mass fraction of Si is 0.012%-0.013%, the mass fraction of Mn is 0.09%-0.012%, the mass fraction of P is less than 0.010%, and the mass fraction of S is less than 0.0050%; the rest is Fe and unavoidable impurities; The production process of S355J2 hot-rolled H-shaped steel for Ce-containing beam and column components comprises the following steps: S1. Smelting of hot-rolled H-beam; S2, continuous casting operation; S3, rolling operation; S1 includes: 1.1 Loading: Control the loading amount to 115±2 tons, of which the P content in the molten iron is ≤0.120%, and the S content in the molten iron is ≤0.040%; and control the steel output to 110 tons to achieve component stability and refining treatment; 1.2 Oxygen supply and slag making: The working oxygen pressure during steelmaking is controlled between 0.8Mpa and 1.4Mpa, the oxygen flow rate is within the range of 16500 to 19000m³ / h, and the terminal pressure gun duration is greater than 40 seconds; The double slag smelting method is adopted. The amount of lime added is adjusted according to the silicon content of the molten iron. The initial slag basicity is controlled between 1.5 and 2.0, the slag basicity is between 2.8 and 3.2, and the magnesium oxide content is 8%, so as to control the smelting cycle to 40 to 50 minutes per furnace; 1.3 End point composition control: During spot blowing, adjust the flow rate to above 18000m³ / h after 1 minute of spot blowing to ensure that the carbon composition of the steel after one spot blowing meets the steel tapping requirements. The end point composition is controlled at C≥0.06%, P≤0.030%, S≤0.030%, and the steel must be tapped in the same sample to ensure the accuracy of carbon addition; 1.4 End point temperature control: control the opening temperature between 1600℃ and 1700℃, and the continuous pouring temperature between 1650℃ and 1680℃; 1.5 Deoxidation and alloying: Alloys are added along with the steel flow. The order of adding alloys is: first add deoxidation as the main element, then add alloying elements, i.e. aluminum block - ferrosilicon - manganese silicon - vanadium nitrogen alloy; and start adding when 1 / 3 of the steel is tapped, and add all alloys before 2 / 3 of the steel is tapped. At the same time, use slag cones to ensure that the thickness of the ladle slag layer does not exceed 55mm, so as to stabilize the alloy recovery rate and avoid rephosphorization of molten steel; 1.6 Argon blowing and temperature control after argon blowing: Argon is blown throughout the steel-making process to ensure that the slag blocking rate reaches 100%; Carry out deoxidation alloying operation: aluminum block - ferrosilicon - manganese silicon - vanadium nitrogen - ferroniobium, start adding alloy when the steel is 1 / 3 tapped, and finish adding before the steel is 3 / 4 tapped; Argon blowing control of argon station: total argon blowing time is 13 minutes, steel loading operation is carried out after adding ferrocerium rare earth alloy, strong blowing is controlled for 3 minutes after argon, soft blowing time is ≥ 7 minutes, and the diameter of exposed molten steel during soft blowing is not more than 200mm; S2 includes: 2.
1. The pouring temperature is controlled at 1550℃-1580℃, and the tundish temperature is controlled at 1530℃-1550℃; 2.
2. When the liquid level in the tundish exceeds 400mm, start pouring and quickly recover to 800mm or above for continuous pouring; 2.
3. Control the casting speed as follows: For the section of 320mm×410mm, the speed of initial pouring is 0.40-0.55m / min, and the speed of continuous pouring is 0.6-0.80m / min; For the 230mm×350mm section, the initial pouring speed is 0.8-1.0m / min, and the continuous pouring speed is 1.0-1.50m / min; 2.
4. The straightening temperature of continuous casting billet is controlled above 880℃; S3 includes: 3.
1. Billet differentiation: When changing the steel type, two refractory bricks are placed on the continuous casting billet or two positions are left empty to differentiate billets of different batches; 3.
2. Heating furnace temperature control: for billets of different sizes, control the temperature of each section of the heating furnace and the time in the furnace; 3.
3. Rolling process temperature control: set the start rolling temperature, finishing rolling temperature and upper cooling bed temperature respectively; The control of the temperature of each section of the heating furnace and the time in the furnace for steel billets of different sizes specifically includes: For the steel billet with a cross section of 230mm×230mm, the temperatures of the heating sections during hot charging are ≤1060℃ for the first section, 1210℃-1250℃ for the second section, 1260℃-1310℃ for the third section, 1250℃-1300℃ for the soaking section, and 150min-180min for the furnace time; the temperatures of the heating sections during cold charging are ≤1100℃ for the first section, 1210℃-1260℃ for the second section, 1260℃-1310℃ for the third section, 1250℃-1315℃ for the soaking section, and 150min-210min for the furnace time; For the steel billet with a cross section of 320mm×410mm, the temperatures of the heating sections during hot charging are ≤1060℃ for the first section, 1210℃-1250℃ for the second section, 1260℃-1300℃ for the third section, 1250℃-1300℃ for the soaking section, and 150min-180min for the furnace time; the temperatures of the heating sections during cold charging are ≤1100℃ for the first section, 1210℃-1260℃ for the second section, 1260℃-1310℃ for the third section, 1250℃-1315℃ for the soaking section, and 150min-210min for the furnace time; The said setting of the start rolling temperature, the finishing rolling temperature and the upper cooling bed temperature respectively specifically includes: The starting rolling temperature of hot-charged steel billet is 1150℃±30℃, the finishing rolling temperature is 1000℃-1090℃, and the upper cooling bed temperature is 800℃-950℃; The starting rolling temperature of the cold-charged steel billet is 1150℃±40℃, the finishing rolling temperature is 1000℃-1090℃, and the upper cooling bed temperature is 800℃-950℃; Descaling operation: During the descaling process, the water pressure is controlled at more than 19Mpa and the billet running speed is 1.0m / s to ensure that the iron oxide scale on the billet surface is removed.
Citation Information
Patent Citations
Process method for producing Nb-containing low-cost small and medium-specification hot-rolled H-shaped steel
CN112522601A
Tough microalloyed non-quenched and tempered steel and production process thereof
CN115141976A
High-toughness hot-rolled H-shaped steel for building and preparation method thereof
CN115418559A
Smelting and continuous casting method for rare earth microalloyed 355MPa-grade low-cost hot-rolled H-shaped steel
CN115491576A
Low-temperature-resistant hot-rolled H-shaped steel and preparation method thereof
CN118127412A