Catalyst and preparation method thereof, sulfur-containing wastewater treatment agent based on advanced oxidation process

In the treatment of sulfur-containing wastewater, a catalyst preparation method combining clay and ammonium carbonate is used to form a porous support, and iron salt, hydrogen peroxide or ozone is used in advanced oxidation methods, the catalyst reuse rate and high corrosion rate are solved. The problem of this achieves the effect of efficiently reducing COD and sulfur content.

CN118681565BActive Publication Date: 2024-11-12SICHUAN XINGAO ENVIRONMENTAL TECH SERVICE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411156616.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

In the prior art, when treating sulfur-containing wastewater, the catalyst has a low reuse rate, resulting in high cost and complex treatment process. The homogeneous catalyst has a high corrosion resistance to the equipment. The active material of the heterogeneous catalyst has a low degree of binding to the support and dissolution. High degree and low reuse rate.

Method used

Using a catalyst preparation method, including the use of clay as a substrate and support, combining ammonium carbonate and other oxidation materials, forming a porous support through the granulation and sintering process, improving the binding of active materials to the support, and using it in advanced oxidation methods Iron salt is used as an active material, combined with hydrogen peroxide or ozone as an oxidizing agent to prepare a catalyst with high catalytic effect and reuse rate.

Benefits of technology

The multiple reuse of the catalyst is realized, the treatment cost is reduced, the catalytic effect is improved, the COD and sulfur content in sulfur-containing wastewater is effectively reduced, the corrosion of the equipment is reduced, and the treatment efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention provides a catalyst and a preparation method thereof, and a sulfur-containing wastewater treatment agent based on an advanced oxidation process, and relates to the technical field of wastewater treatment. The preparation method of the catalyst comprises the following steps: taking a substrate including clay and ammonium carbonate, adding water to stir and mix the substrate, then adding ammonium carbonate and continuing to stir evenly, granulating and forming it, and drying it by ventilation to obtain carrier particles; preparing an aqueous solution of active materials, then placing the carrier particles in the aforementioned solution, soaking for 8 to 15 hours; drying and sintering the soaked carrier particles. When the catalyst is used in combination with hydrogen peroxide and ozone, sulfur-containing wastewater can be treated. The catalyst of the present invention has a shorter preparation time than the catalyst prepared by the conventional impregnation method, which saves more time, and has better catalytic performance. When it is used in combination with an oxidant, sulfur-containing wastewater can be treated well.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wastewater treatment, and specifically relates to a catalyst and a preparation method thereof, and a sulfur-containing wastewater treatment agent based on an advanced oxidation process. Background Art

[0002] For some high-sulfur oil and gas fields, a large amount of sulfur-containing wastewater will be generated during the development process. If it is not effectively treated, it will not only cause serious pollution to the environment, but also cause serious corrosion to the water pipeline, posing serious safety hazards. In sulfur-containing wastewater, sulfur is mainly in the form of H2S and HS - , S 2- There is a small amount of organic sulfur in the wastewater, such as mercaptans, which are highly corrosive and the total amount of sulfur can reach thousands of ppm. At the same time, there is a large amount of organic matter in the sulfur-containing wastewater, and its COD can reach up to 10,000 mg / L. These will increase the difficulty of treating sulfur-containing wastewater in oil and gas fields.

[0003] At present, in oil and gas fields, the treatment of sulfur-containing wastewater mostly first adopts gas stripping desulfurization, and then adopts methods such as coagulation to further treat it. However, gas stripping desulfurization first needs to add acid to make it acidic, and at the same time, gas stripping is more corrosive to the device. In the prior art, there are also advanced oxidation methods for treating it, such as the conventional Fenton oxidation method. The catalyst commonly used in the Fenton oxidation method is a homogeneous catalyst. The problem is that it is necessary to add acid to make the gas field water acidic during use, and it is necessary to add alkali to adjust its pH to neutral after the treatment. Not only is the process complicated and the cost is high, but at the same time, the homogeneous catalyst will produce a large amount of mud phase, resulting in a large loss. Although there are also heterogeneous catalysts currently used, the degree of binding between the active material and the carrier in the existing heterogeneous catalyst is relatively low, resulting in a high dissolution rate of the active material in the heterogeneous catalyst and a low reuse rate. Summary of the invention

[0004] To solve at least one of the above problems, the present invention provides a catalyst and a preparation method thereof, and a sulfur-containing wastewater treatment agent based on an advanced oxidation process. The catalyst can be reused multiple times, thereby reducing costs.

[0005] The technical solution of the present invention is as follows: A method for preparing a catalyst comprises the following steps:

[0006] S1. Take a substrate including clay and ammonium carbonate, add water to stir and mix the substrate, then add ammonium carbonate and continue to stir evenly, granulate it, and dry it under ventilation at 20-45° C. for 1-3 days to obtain carrier particles; the mass ratio of the ammonium carbonate to the substrate is 10:1-3;

[0007] S2, preparing an aqueous solution of active material with a concentration of 0.1-0.3 mol / L, then placing the carrier particles in the aforementioned solution, and soaking them at 50-80° C. for 8-15 hours;

[0008] S3. Keep the soaked carrier particles at 80-100°C for 1-3 hours, then heat to 500-800°C and sinter for 2-5 hours.

[0009] In the present invention, the reason why ammonium carbonate is added after the substrate is added with water and mixed evenly is that ammonium carbonate will slowly decompose into gas under certain temperature conditions. Normally, ammonium carbonate begins to decompose at 50°C, and its decomposition products are ammonia, carbon dioxide and water. When ammonium carbonate is in the form of an aqueous solution, it begins to decompose at about 70°C. The gas generated during the decomposition of ammonium carbonate will not only turn the carrier into a porous material, but also expand the volume of the gas released during the decomposition of ammonium carbonate. During the process of the porous material discharging the gas, the pressure in the pores is reduced. Under the action of the pressure difference, the external liquid phase material will be adsorbed into the pores, which can not only reduce the immersion time, but also the active material adsorbed into the pores is more tightly combined with the carrier. In the subsequent use process, its solubility is low and can be used multiple times.

[0010] Theoretically, other materials that can generate gas, such as ammonium bicarbonate, can also be applied to the present invention. However, in actual practice, the decomposition temperature of ammonium bicarbonate is low, and it is easy to decompose at room temperature, and the production process is not easy to control. At the same time, after the decomposition of ammonium carbonate, the gas generated is carbon dioxide and ammonia, and the liquid phase is water, which will not remain in the carrier particles, so it will not have a significant impact on the carrier particles, which is difficult to achieve with other materials.

[0011] As for the substrate, it includes clay. Clay is both the raw material of the carrier and the adhesive of the carrier. Clay has certain bonding properties. After high-temperature sintering, the bonding is enhanced. If clay is used alone as the substrate, although the carrier can also be prepared and the catalyst can achieve a good catalytic effect, the water resistance of the carrier is poor, resulting in a relatively low reuse rate; therefore, in the present invention, the carrier usually also includes other raw materials, such as at least one of the common aluminum oxide, titanium oxide, bauxite, and shale. In this case, the addition ratio of clay to the other raw materials in the substrate is 10:6~12, which can not only increase the water resistance and reuse rate of the catalyst, but also enhance the performance of the catalyst to a certain extent.

[0012] When the carrier particles are granulated, since the carrier particles of the present invention need to be immersed in an aqueous solution for a period of time before sintering, in order to avoid the carrier particles from disintegrating in the aqueous solution, the granulation pressure is usually above 0.5MPa. Generally speaking, in order to make the sintered catalyst have good catalytic performance, the particle size of the catalyst particles needs to be controlled: when the particle size is greater than 10mm, the effect is poor; when the particle size is less than 5mm, it has a better effect. Therefore, in the present invention, the particle size is limited to no more than 10mm.

[0013] In S2, the amount of carrier particles added and the ratio of active material aqueous solution added are usually equal volumes, i.e. 1 cm 3 The carrier particles can be added to 1 ml of the active material aqueous solution; or the excessive impregnation method can be used, that is, the amount of active material aqueous solution added to submerge the carrier particles. In the present invention, since the impregnation needs to be performed under a higher temperature condition, the excessive impregnation method is selected.

[0014] In S3, the carrier particles are first dried at 80-100°C to remove moisture inside the carrier particles; then, the temperature is raised to a sintering temperature to sinter and activate the carrier particles, thereby obtaining a catalyst.

[0015] One embodiment of the present invention is that the active material is an iron salt. In the advanced oxidation process, when the active material is an iron salt, its oxidant is usually hydrogen peroxide or ozone, and under the catalysis of the iron salt, hydrogen peroxide and ozone can efficiently produce hydroxyl radicals, so that organic matter and sulfide can be quickly oxidized. Of course, the oxidant at this time can also be persulfate, but when the simple iron salt catalyzes persulfate, its effect is relatively poor. At the same time, in actual use, persulfate is used less to treat wastewater, which is mainly due to the fact that although persulfate can treat wastewater, the persulfate after treatment can generate sulfate, which is a new water pollutant. In the prior art, there are also other transition metals or rare metals doped in iron salts, such as manganese ions, copper ions, etc., which can be applied to the present invention.

[0016] Another object of the present invention is to provide a catalyst prepared by any of the above methods, which has good catalytic effect and high reusability.

[0017] Another object of the present invention is to provide a sulfur-containing wastewater treatment agent based on an advanced oxidation process, the treatment machine comprising the above-mentioned catalyst and an oxidant, wherein the catalyst is used to catalyze the oxidant.

[0018] Another embodiment of the present invention is that the active material in the catalyst is an iron salt, and the oxidant is hydrogen peroxide or ozone. Under this condition, the mass ratio of the catalyst to the oxidant is 2 to 4:1.

[0019] The beneficial effects of the present invention are:

[0020] The catalyst of the present invention has ammonium carbonate that is easy to decompose and generate gas arranged in the carrier, and at the same time, the ammonium carbonate is not degraded before the carrier particles are sintered, and at the same time, when the impregnation operation is performed, the impregnation temperature is limited to the decomposition temperature of the ammonium carbonate. Therefore, during the impregnation process, the decomposition of the ammonium carbonate will generate bubbles, which will not only make the carrier a porous material, but also, when the bubbles are removed from the internal voids of the carrier, due to the pressure difference between the inside and outside of the voids, the external active material will enter the inside of the carrier, so that the present invention can complete the impregnation faster, thereby saving time. At the same time, the catalyst prepared by the present invention, when used in conjunction with an oxidant, has a good effect of reducing COD and sulfur content, and can be used for the treatment of produced water from sulfur-containing oil and gas fields; and the catalyst of the present invention can be reused many times, saving production costs. DETAILED DESCRIPTION

[0021] In order to make the technical solutions and technical advantages of the present invention more clear, the technical solutions in the implementation process of the present invention will be clearly and completely described below in conjunction with embodiments.

[0022] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0023] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0024] In the following examples, unless otherwise specified, the parts described are parts by mass.

[0025] Example 1: S1. Take 5 parts of aluminum oxide powder, 5 parts of bauxite, 1 part of titanium dioxide, 10 parts of clay and add 5 parts of water to mix evenly, then add 3 parts of ammonium carbonate and mix evenly, then use a granulator to granulate at a pressure of 0.5 MPa, and then ventilate and dry it at room temperature for 2 days. In this example, the particle size of the carrier particles is 1~4 mm.

[0026] S2, preparing an aqueous solution of ferrous sulfate with a concentration of 0.15 mol / L, then adding carrier particles into a container, and immersing the carrier particles with the aforementioned solution, heating to 75° C., and soaking for 8 hours under reflux conditions;

[0027] S3. Take the carrier particles after soaking in S2, filter out excess water, and keep the carrier particles at 90°C for 2 hours under a nitrogen atmosphere. Then raise the temperature to 650°C and sinter for 4 hours. Cool to room temperature to obtain catalyst AST-1.

[0028] Example 2: S1. Take 6 parts of alumina powder, 2 parts of shale, 10 parts of clay and add 4 parts of water to mix evenly, then add 3 parts of ammonium carbonate and mix evenly, then use a granulator to granulate at a pressure of 0.5 MPa, and then ventilate and dry it at room temperature for 3 days. In this example, the particle size of the carrier particles is 1~4 mm.

[0029] S2, prepare a 0.15 mol / L ferrous sulfate aqueous solution, then add carrier particles into a container, immerse the carrier particles in the above solution, heat to 70° C., and soak for 8 hours under reflux;

[0030] S3. Take the carrier particles after soaking in S2, filter out excess water, and keep the carrier particles at 80°C for 3 hours under a nitrogen atmosphere. Then raise the temperature to 600°C and sinter for 4 hours. Cool to room temperature to obtain catalyst AST-2.

[0031] Example 3: S1. Take 4 parts of bauxite, 3 parts of zinc oxide powder, 10 parts of clay and add 3 parts of water to mix evenly, then add 4 parts of ammonium carbonate and mix evenly, then use a granulator to granulate at a pressure of 0.5 MPa, and then ventilate and dry it at room temperature for 3 days. In this example, the particle size of the carrier particles is 4~8 mm.

[0032] S2, preparing an active material aqueous solution with a total concentration of 0.2 mol / L, wherein the active material is composed of ferrous sulfate and copper sulfate in a molar ratio of 1:0.5, then adding carrier particles into a container, and immersing the carrier particles with the above solution, heating to 70° C., and soaking for 10 hours under reflux conditions;

[0033] S3. Take the carrier particles after soaking in S2, filter out excess water, and keep the carrier particles at 80°C for 3 hours under a nitrogen atmosphere. Then raise the temperature to 600°C and sinter for 4 hours. Cool to room temperature to obtain catalyst AST-3.

[0034] Example 4: This example is different from Example 1 in that the pressure during the granulation process is 0.4 MPa, and the rest are the same, and finally the catalyst AST-4 is obtained.

[0035] Example 5: This example is different from Example 1 in that "5 parts of aluminum oxide powder, 5 parts of bauxite, 1 part of titanium dioxide, and 10 parts of clay" are replaced with 21 parts of clay, and the rest are the same, and finally the catalyst AST-5 is obtained.

[0036] Comparative Example 1

[0037] The difference between this comparative example and Example 1 is that porous ceramsite is used as the carrier particles, and the particle size thereof is 1-4 mm, and the rest are the same, and finally the catalyst AST-6 is obtained.

[0038] Example 6: In this example, the sulfur-containing wastewater treatment agent based on the advanced oxidation process includes a catalyst and an oxidant, wherein the oxidant is hydrogen peroxide with a mass fraction of 50%, the mass ratio of the sum of the mass of CODcr and sulfur to hydrogen peroxide (100% purity) is 1:1, and the mass ratio of the catalyst to hydrogen peroxide is 3:1.

[0039] Example 7: In this example, the sulfur-containing wastewater treatment agent based on the advanced oxidation method includes a catalyst and an oxidant, wherein the oxidant is ozone, wherein for every 10g of CODcr and sulfur in the wastewater, 5.5g of ozone is added, and the mass ratio of the catalyst to ozone is 2.5:1.

[0040] In order to further illustrate the effect of the sulfur-containing wastewater treatment agent based on the advanced oxidation method prepared in the above embodiment, the sulfur-containing wastewater treatment agent based on the advanced oxidation method prepared above is tested below.

[0041] In the following test process, the sulfur-containing wastewater used is the produced water of Puguang gas field, and its COD content is 4359 mg / L, which is mainly straight-chain alkanes and also contains some aromatic hydrocarbons. The sulfur content is 472 ppm, among which the sulfur is mainly hydrogen sulfide and its water-soluble substances, containing a small amount of mercaptan.

[0042] Performance Testing

[0043] The produced water was placed in the kettle, and the catalysts prepared in Examples 1 to 5 and Comparative Example 1 were added at 30° C. according to the methods of Example 6 and Example 7, and the corresponding oxidant was added at the same time. The water quality of the produced water in the kettle was tested at regular intervals. The results are shown in Table 1.

[0044] Table 1 Water quality testing

[0045]

[0046] It can be seen from Table 1 that the catalyst and sulfur-containing wastewater treatment agent prepared in the embodiment of the present invention can effectively treat sulfur-containing wastewater and can effectively reduce the COD content and sulfur content of pulmonary edema.

[0047] At the same time, the inventors found through experiments that the effect was not very obvious because the COD content and sulfur content in the wastewater were both high. After experiments, the inventors found that if the catalyst prepared in Example 1 is used to treat wastewater with a COD content of less than 500 mg / L and a sulfur content of less than 100 ppm, the COD content can be reduced to below 20 mg / L and the sulfur content can be reduced to below 2 ppm within 10 minutes, so that the wastewater treated in this way can meet the direct discharge conditions.

[0048] The inventors analyzed that the reason why the efficiency of catalyst AST-6 is so low may be that for the conventional impregnation method, the impregnation time is usually about 20 hours, while the impregnation time in the embodiment of the present invention is only 8 hours, and there is only a small amount of active material on the carrier, resulting in its low catalytic performance.

[0049] 2. Repeated use rate test

[0050] Catalysts AST-1, AST-4, and AST-5 were used to treat wastewater several times in succession according to the method of Example 5, and the COD reduction rate and sulfur content reduction rate after 30 minutes were recorded. At the same time, after each use, the catalyst particles were filtered, washed, and dried for the next use. The number of times when the COD removal rate was lower than 70% and the number of times when the desulfurization rate was lower than 90% were recorded, and the final results are shown in Table 2.

[0051] Table 2 Reusability test results.

[0052]

[0053] As can be seen from Table 2, the catalyst prepared in the embodiment of the present invention can be reused for many times; at the same time, it is found that the weight of AST-4 and AST-5 will gradually decrease during the repeated use. At the same time, the inventor analyzed that the reason why the desulfurization situation is better than that of COD is that hydrogen peroxide itself can remove hydrogen sulfide well: hydrogen peroxide has strong oxidizing properties, and can still oxidize negative divalent sulfur even without a catalyst, and has a high efficiency; although hydrogen peroxide can also have a certain treatment effect on COD, the efficiency is low, and the removal rate is usually only about 20% to 30% without a catalyst.

[0054] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a catalyst, It is characterized in that The following steps are involved: S1. Take a substrate including clay and ammonium carbonate, add water to stir and mix the substrate, then add ammonium carbonate and continue to stir evenly, granulate it, and dry it under ventilation at 20-45° C. for 1-3 days to obtain carrier particles; the mass ratio of the ammonium carbonate to the substrate is 10:1-3, and the particle size of the carrier particles is not more than 10 mm; S2, preparing an aqueous solution of active material with a concentration of 0.1-0.2 mol / L, then placing the carrier particles in the aforementioned solution, and soaking them at 50-80° C. for 8-15 hours; S3, keeping the soaked carrier particles at 80-100°C for 1-3 hours, then heating to 500-800°C and sintering for 2-5 hours; The active material is an iron salt.

2. The method according to claim 1, It is characterized in that The substrate also includes at least one of aluminum oxide, titanium oxide, zinc oxide, bauxite, and shale.

3. The method according to claim 1 or 2, It is characterized in that The addition ratio of the clay to the other raw materials in the base material is 10:6-12.

4. The method according to claim 1, It is characterized in that In S1, the granulation pressure is not less than 0.5 MPa.

5. A catalyst prepared by the method according to any one of claims 1 to 4.

6. A sulfur-containing wastewater treatment agent based on advanced oxidation process, It is characterized in that The invention comprises the catalyst according to claim 5, and an oxidant, wherein the catalyst is used for catalyzing the oxidant.

7. The sulfur-containing wastewater treatment agent based on advanced oxidation process according to claim 6, It is characterized in that The active material in the catalyst is iron salt, the oxidant is hydrogen peroxide or ozone, and the mass ratio of the catalyst to the oxidant is 2-4:1.