A pyrite electrode and preparation method thereof
By designing pyrote electrodes, using meltblown mixed grid substrate and microporous membrane crusher, combined with sodium carbonate sustained release agent, the problem of difficulty in denitrogenation in wastewater is solved, and high efficiency and low cost are achieved Sulfur autotrophic denitrification reduces sludge generation.
Patent Information
- Application Number
- CN202411156639.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-22
AI Technical Summary
Existing sewage treatment technologies are difficult to efficiently denitrozenide in low C/N ratio wastewater, and traditional heterotrophic denitrification processes require additional organic carbon sources, resulting in high sludge generation and operation costs and may cause secondary pollution.
Using pyrote electrodes, combining meltblown mixed grid substrates and pyrote powders, adding microporous membrane pulverizers and sodium carbonate sustained release agents, and designing a tablet-type structure to improve the specific surface area and conductivity of the electrodes and promote sulfur. Autotrophic denitrification reaction.
It significantly improves the efficiency and stability of sulfur autotrophic denitrification, reduces sludge generation, reduces operating costs, and provides high-efficiency denitrification solutions for low-carbon sources.
Smart Images

Figure CN118684331B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of sewage treatment, and more specifically, to a pyrite electrode and a preparation method thereof. Background Art
[0002] The problem of insufficient carbon sources in sewage treatment is becoming increasingly prominent. Controlling nitrogen and reducing carbon, especially low-carbon treatment of nitrates in low C / N sewage, has become a major technical challenge in the industry. Existing sewage treatment often requires the addition of organic carbon sources to improve denitrification efficiency, but in mainstream heterotrophic denitrification treatment, the additional organic carbon source will be converted into a large amount of sludge and carbon dioxide, which runs counter to the concept of low-carbon sewage. Green and low-carbon treatment of sewage has become a hot topic in environmental engineering technology research and an important way to build a sustainable water circulation system.
[0003] Traditional denitrification processes often require additional carbon sources when treating wastewater with high ammonia nitrogen or low C / N ratio. At the same time, deep phosphorus removal requires the addition of chemical agents, which not only increases operating costs but may also cause secondary pollution. Compared with traditional heterotrophic denitrification processes, sulfur autotrophic denitrification processes use low-valent reduced sulfur and sulfide as electron donors, and nitrate and nitrite as electron acceptors for denitrification and nitrogen removal. Due to its advantages such as no need for external carbon sources, high denitrification efficiency, and low sludge production, the sulfur autotrophic denitrification process has received widespread attention and is particularly suitable for the removal of nitrate and nitrite in wastewater with a low carbon-nitrogen ratio.
[0004] For the sulfur autotrophic denitrification process, the application of an external power source can significantly improve its efficiency and stability. Through the external power source, active sulfides, such as polysulfides, can be generated on the electrode surface. These active sulfides can be more effectively utilized by denitrifying bacteria, thereby accelerating the denitrification reaction. However, at present, for the electrochemical sulfur autotrophic denitrification process, there is basically no optimization of the electrode, which makes the electrode more conducive to the sulfur autotrophic denitrification process. Summary of the invention
[0005] In view of the problems existing in the prior art, the present application provides a pyrite electrode and a preparation method thereof.
[0006] A pyrite electrode, comprising a plurality of sheet-shaped pyrite sheets, wherein the pyrite sheets comprise a melt-blown mixed grid substrate and pyrite powder attached to the melt-blown grid substrate;
[0007] The melt-blown mixed grid substrate includes graphene conductive yarns and polypropylene fibers melt-blown between the graphene conductive yarns;
[0008] Strip-shaped carbonate slow-release agents arranged in an interlaced and stacked manner are filled between the flaky pyrite sheets.
[0009] Furthermore, the strip-shaped carbonate sustained-release agent contains 10 to 30% of a binder.
[0010] Furthermore, the binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethylene imine.
[0011] Furthermore, the average diameter of the graphene conductive yarn is greater than the average diameter of the polypropylene fiber.
[0012] Furthermore, the pyrite powder is doped with microporous membrane crushed material.
[0013] Furthermore, the proportion of microporous membrane crushed material in the pyrite powder is 10 to 30 wt %.
[0014] Furthermore, the microporous membrane crushed material is selected from sulfonic acid modified microporous membrane or sulfonyl modified microporous membrane.
[0015] Furthermore, the pyrite powder is also doped with 1-5% of a polyacrylic acid binder.
[0016] A method for preparing a pyrite electrode comprises the following steps:
[0017] S1: melt-blown polypropylene layer and doped with graphene conductive yarn during the melt-blowing process, and then cooled and solidified to obtain a melt-blown mixed grid substrate;
[0018] S2: preparing pyrite powder, coating and bonding the pyrite powder on a melt-blown mixed grid substrate to obtain a single sheet of pyrite;
[0019] S3: stacking a plurality of flaky pyrite sheets, and applying a staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and pressing them tightly.
[0020] Furthermore, the compacting pressure in the step S3 is 10-100 kPa.
[0021] In summary, the present invention has the following beneficial effects:
[0022] The present invention utilizes a pressed sheet structure design to greatly increase the specific surface area of the electrode, thereby improving the reaction efficiency. Compared with the traditional electrode design, the pyrite electrode of the present invention significantly increases the surface area of the electrode through the pressed sheet structure design. This design is not only conducive to the attachment and growth of sulfur autotrophic denitrifying bacteria, but also can increase the contact area between nitrate and nitrite and pyrite, thereby enhancing the reaction efficiency.
[0023] Secondly, the present invention adopts a melt-blown mixed grid substrate in the electrode substrate design, combining graphene conductive yarn and melt-blown polypropylene fiber. This three-dimensional structure substrate has excellent conductivity and stability, providing a good environment for electrochemical reactions. As a conductive material, graphene has high conductivity and excellent mechanical properties, which can effectively improve the overall conductivity of the electrode. In addition, the melt-blown process of polypropylene fiber makes the substrate structure more stable, ensuring the mechanical stability of the electrode during long-term operation.
[0024] In the design of pyrite powder, the present invention not only uses traditional pyrite, but also specially adds microporous membrane crushed materials. These microporous membrane crushed materials can be unmodified microporous membranes or microporous membranes modified with anions such as sulfonic acid groups. These modified microporous membrane crushed materials have better adsorption performance and chemical stability, which can make pyrite more evenly and firmly attached to the melt-blown mixed grid substrate, thereby enhancing the overall performance of the electrode.
[0025] The addition of microporous membrane crushed materials not only improves the adhesion of pyrite powder, but also enhances its chemical stability. These modified materials have rich pore structures and surface functional groups, which can effectively improve the reactivity and stability of pyrite electrodes. In the denitrification process, these microporous membrane crushed materials can provide more active sites, promote the reduction reaction of nitrate and nitrite, and thus improve the denitrification efficiency.
[0026] In addition, the present invention arranges a strip of sodium carbonate slow-release agent between two flaky pyrite sheets. This design not only improves the bonding strength and stability between the flaky pyrite sheets, but also provides a small amount of carbon source supplement for the sulfur autotrophic denitrification process by slowly releasing sodium carbonate. The slow release of the sodium carbonate slow-release agent can effectively maintain the carbon source concentration in the pyrite electrode, ensuring the continuous reaction and efficient denitrification.
[0027] The present invention not only improves the specific surface area and conductivity of the electrode by optimizing the electrode structure and material composition, but also enhances the stability and efficiency of the reaction, thereby providing an effective solution for the efficient denitrification of wastewater with a low C / N ratio. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a characteristic diagram of the bacterial community structure distribution of the electrochemical sulfur autotrophic reactor after the sludge in Example 10 of the present invention is subjected to high-throughput analysis at the initial and stabilized stages;
[0029] Figure 2 It is a characteristic diagram of the distribution of bacterial community structure of the electrochemical sulfur autotrophic reactor after high-throughput analysis of the sludge in Example 10 of the present invention at the initial and stabilized stages. DETAILED DESCRIPTION
[0030] The present application is further described in detail below in conjunction with embodiments and drawings.
[0031] Example 1
[0032] A method for preparing a pyrite electrode comprises the following steps:
[0033] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0034] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0035] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 60 μm in this embodiment. Then mix the pyrite powder and the adhesive at a mass ratio of 10:1 and apply them on the melt-blown mixed grid substrate to obtain a single piece of pyrite in a sheet shape; the adhesive is xanthan gum.
[0036] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them tightly. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate and polyacrylamide hydrogel in a mass ratio of 1:20-30.
[0037] The pyrite electrode prepared by the above method includes 10 flaky pyrite sheets, and strip-shaped carbonate slow-release agents are coated between two flaky pyrite sheets in an interlaced and stacked arrangement. The pyrite sheet includes a melt-blown mixed grid substrate and pyrite powder attached to the melt-blown grid substrate.
[0038] Example 2
[0039] A method for preparing a pyrite electrode comprises the following steps:
[0040] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0041] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0042] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 60 μm in this embodiment. Then mix the pyrite powder and the adhesive at a mass ratio of 10:1 and apply them on the melt-blown mixed grid substrate to obtain a single piece of pyrite in a sheet shape; the adhesive is xanthan gum.
[0043] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0044] Example 3
[0045] A method for preparing a pyrite electrode comprises the following steps:
[0046] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0047] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0048] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 60 μm in this embodiment. Then mix the pyrite powder, adhesive and polyethersulfone microporous membrane crushed material in a mass ratio of 10:1:3 and apply them on the melt-blown mixed grid substrate to obtain a single piece of pyrite in a sheet form; wherein the adhesive is xanthan gum and the average pore size of the polyethersulfone microporous membrane is 10 μm.
[0049] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0050] Example 4
[0051] A method for preparing a pyrite electrode comprises the following steps:
[0052] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0053] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0054] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 60 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 10:1:3 and apply them on the melt-blown mixed grid substrate to obtain a single piece of flaky pyrite; wherein the adhesive is xanthan gum, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0055] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0056] Example 5
[0057] A method for preparing a pyrite electrode comprises the following steps:
[0058] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0059] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0060] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 60 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 10:1:3 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0061] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0062] Example 6
[0063] A method for preparing a pyrite electrode comprises the following steps:
[0064] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 2 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0065] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0066] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 100 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 10:1:3 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0067] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the strip carbonate slow-release agent stacked in an interlaced manner between two flaky pyrite sheets, and press them. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:20:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0068] Example 7
[0069] A method for preparing a pyrite electrode comprises the following steps:
[0070] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0071] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0072] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 60 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 10:1:3 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0073] S3: stack the 15 flaky pyrite sheets obtained in step S2, and apply the strip carbonate slow-release agent stacked in an interlaced manner between two flaky pyrite sheets, and press them tightly. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0074] Example 8
[0075] A method for preparing a pyrite electrode comprises the following steps:
[0076] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0077] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0078] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 60 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 10:1:4 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0079] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them. The pressure is controlled to be 80 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from sodium alginate, xanthan gum, gum arabic, polyacrylic acid, and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0080] Example 9
[0081] A method for preparing a pyrite electrode comprises the following steps:
[0082] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 2 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0083] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0084] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 80 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 12:1:5 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0085] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0086] Example 10
[0087] A method for preparing a pyrite electrode comprises the following steps:
[0088] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0089] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0090] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 50 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 15:2:5 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0091] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them. The pressure is controlled to be 90 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:20:3. The binder is selected from sodium alginate, xanthan gum, gum arabic, polyacrylic acid, and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0092] Embodiment 11
[0093] A method for preparing a pyrite electrode comprises the following steps:
[0094] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0095] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0096] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 20 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 10:1:3 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0097] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0098] Example 12
[0099] A method for preparing a pyrite electrode comprises the following steps:
[0100] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 2 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0101] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0102] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 70 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 11:1:3 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0103] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the strip carbonate slow-release agent stacked in an interlaced manner between two flaky pyrite sheets, and press them tightly. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:21:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0104] Embodiment 13
[0105] A method for preparing a pyrite electrode comprises the following steps:
[0106] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0107] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 500μm.
[0108] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 70 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 10:1:3 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0109] S3: stack the 13 flaky pyrite sheets obtained in step S2, and apply the strip carbonate slow-release agent arranged in an interlaced stack between two flaky pyrite sheets, and press them. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0110] Embodiment 14
[0111] A method for preparing a pyrite electrode comprises the following steps:
[0112] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0113] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 400μm.
[0114] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 60 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 13:1:4 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0115] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0116] Embodiment 15
[0117] A method for preparing a pyrite electrode comprises the following steps:
[0118] S1: The polypropylene raw material masterbatch is sprayed onto the receiving device by melt-blowing equipment. The melt-blown fiber filaments are melt-softened and connected to each other to form a mesh three-dimensional structure. When the melt-blown polypropylene layer reaches a thickness of 2-3 mm, preferably 3 mm in this embodiment, the graphene conductive yarn is evenly laid on the polypropylene layer, and the thickness of the graphene conductive yarn is controlled to be 2 mm ± 0.5 mm, and then the melt-blown polypropylene layer is melt-blown on the graphene conductive yarn and the above steps are repeated. In this embodiment, three layers of polypropylene layers and two layers of graphene conductive yarn layers are preferably used. After the melt-blowing is completed, the stacked polypropylene layer and the graphene conductive yarn layer are hot-pressed, the hot-pressing temperature is controlled to be 170 ° C, the hot-pressing pressure is 10 kPa, and the hot-pressing time is controlled to be 20 s. After cooling, a melt-blown mixed grid substrate is obtained.
[0119] Among them, the graphene conductive yarn uses 30D graphene conductive yarn produced by Dongguan Keke Textile Materials Co., Ltd.; the average diameter of the polypropylene fiber is 800μm.
[0120] S2: Prepare pyrite powder, grind the pyrite with a ball mill to a particle size of 10-100 μm, preferably 60 μm in this embodiment. Then mix the pyrite powder, adhesive and sulfonic acid modified polyethersulfone microporous membrane crushed material in a mass ratio of 10:1:3 and apply them on the melt-blown mixed grid substrate to obtain a sheet of pyrite; wherein the adhesive is a polyacrylic acid adhesive, and the average pore size of the sulfonic acid modified polyethersulfone microporous membrane is 10 μm.
[0121] S3: stack the 10 flaky pyrite sheets obtained in step S2, and apply the staggered and stacked strip carbonate slow-release agent between two flaky pyrite sheets, and press them. The pressure is controlled to be 100 kPa. The strip carbonate slow-release agent is a mixture of calcium carbonate, polyacrylamide hydrogel and a binder in a mass ratio of 1:25:3. The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethyleneimine. Sodium alginate is selected in this embodiment.
[0122] Comparative Example
[0123] Comparative Example 1 discloses an electrode composed of a pyrite powder filler ground to 60 μm by a ball mill and a sheet electrode.
[0124] Detection Methods
[0125] First, the electrodes of each embodiment and comparative example and the anode composed of carbon particles are used together to form a reactor. Then, the tin-stripped water of the electroplating plant (after treatment and dilution of salt to 50 mS / cm) is used as the inlet water of the electrochemical sulfur autotrophic reactor, and nitrogen stripping is used to keep the inlet DO concentration below 0.2 mg / L. The inlet ammonia nitrogen concentration is 10 mg / L, the inlet nitrite nitrogen is 0 mg / L, the inlet nitrate nitrogen is 100 mg / L, the inlet COD is 20 mg / L, pH=8, and the phosphate concentration is 2 mg / L. The sludge of the municipal sewage plant is added at a sludge concentration of 3000 mg / L MLVSS for domestication. Each reactor operates at the same hydraulic retention time at each stage, and the load is increased by gradually reducing the hydraulic retention time of the reactor. The test device operates continuously and stably for 70 days. The hydraulic retention time of the reactor at different stages is shown in Table 1. The water quality indicators are monitored daily to investigate the operation effect of the reactor.
[0126] Table 1
[0127] stage Time / d Hydraulic retention time / h Phase 1 1-10 24 Phase II 11-20 12 Phase 3 21-30 6 Stage 4 31-40 4 Stage 5 41-60 2.7 Stage 6 61-70 2.2
[0128] The water samples were filtered through a 0.45 μm filter membrane and then the parameters were determined. - -N concentration was measured by ion chromatograph (CIC-D100, Qingdao Shenghan), and TN (total nitrogen) concentration was measured by national standard method (GB11894-89). The average TN removal effect of low hydraulic retention time refers to the average TN removal rate measured at a hydraulic retention time of 2.2h in each stage. The average TN removal effect of medium hydraulic retention time refers to the average TN removal rate measured at a hydraulic retention time of 6h in each stage.
[0129] Table 2
[0130] Example Average TN removal effect (%) Average TN removal effect at low hydraulic retention time (%) Average TN removal effect at medium hydraulic retention time (%) Example 1 96.13 67.45 92.25 Example 2 96.26 71.74 92.34 Example 3 97.24 74.14 93.33 Example 4 97.37 77.34 94.23 Example 5 98.42 80.45 95.46 Example 6 99.54 83.21 96.48 Example 7 99.56 83.35 96.34 Example 8 99.63 82.64 96.76 Example 9 99.51 82.31 97.78 Example 10 99.62 83.28 96.96 Embodiment 11 99.67 83.76 97.34 Example 12 99.68 82.73 96.74 Embodiment 13 99.93 83.21 97.25 Embodiment 14 99.99 83.23 96.56 Embodiment 15 99.92 82.14 97.21 Comparative Example 1 86.12 61.67 81.34
[0131] The electrodes of each embodiment and comparative example and the anode composed of carbon particles are used together to form a reactor. In subsequent experiments, the nitrified tail water of the etching water washing water of the circuit board factory is used as the inlet of the electrochemical sulfur autotrophic reactor, and nitrogen stripping is used to keep the inlet DO concentration below 0.2 mg / L. The inlet ammonia nitrogen concentration is 10 mg / L, the inlet nitrite nitrogen is 0 mg / L, the inlet nitrate nitrogen is 100 mg / L, the inlet COD is 20 mg / L, pH=8, and the phosphate concentration is 2 mg / L. The sludge of the municipal sewage plant is added for domestication at a sludge concentration of 3000 mg / L MLVSS. Each reactor operates at the same hydraulic retention time at each stage, and the load is increased by gradually reducing the hydraulic retention time of the reactor. The test device operates continuously and stably for 70 days. The hydraulic retention time of the reactor at different stages is shown in Table 1. The water quality indicators are monitored daily to investigate the operation effect of the reactor.
[0132] Table 3
[0133] stage Time / d Hydraulic retention time / h Phase 1 1-10 24 Phase II 11-20 12 Phase 3 21-30 6 Stage 4 31-40 4 Stage 5 41-60 2.7 Stage 6 61-70 2.2
[0134] The water samples were filtered through a 0.45 μm filter membrane and then the parameters were determined. - -N concentration was measured by ion chromatograph (CIC-D100, Qingdao Shenghan), and TN (total nitrogen) concentration was measured by national standard method (GB11894-89). The average TN removal effect of low hydraulic retention time refers to the average TN removal rate measured at a hydraulic retention time of 2.2h in each stage. The average TN removal effect of medium hydraulic retention time refers to the average TN removal rate measured at a hydraulic retention time of 6h in each stage.
[0135] It can be seen from the data in the above table that the pyrite electrode prepared by the present invention adopts a melt-blown mixed grid substrate and pyrite powder, and a strip-shaped sodium carbonate sustained-release agent is arranged between two flaky pyrite sheets, so that the pyrite electrode has a better sewage treatment effect, and when microporous membrane crushed material and modified microporous membrane crushed material are added to the pyrite powder, the pyrite electrode has a better treatment effect and treatment efficiency.
[0136] Table 4
[0137] Example Average TN removal effect (%) Average TN removal effect at low hydraulic retention time (%) Average TN removal effect at medium hydraulic retention time (%) Example 1 92.50 73.33 94.85 Example 2 95.45 77.49 96.05 Example 3 97.20 80.15 96.58 Example 4 94.02 79.73 99.35 Example 5 97.63 86.65 99.31 Example 6 96.90 86.43 98.15 Example 7 98.58 87.99 99.79 Example 8 96.43 84.60 99.08 Example 9 98.34 87.49 99.84 Example 10 99.08 90.57 98.16 Embodiment 11 98.23 88.06 99.05 Example 12 98.52 88.86 98.80 Embodiment 13 97.80 88.19 98.10 Embodiment 14 96.43 87.62 96.06 Embodiment 15 95.88 85.61 97.02 Comparative Example 1 81.97 64.92 84.12
[0138] The sludge of Example 10 was subjected to high throughput analysis to determine the sludge community distribution characteristics after initial and stable operation.
[0139] As attached Figure 1 As shown, phylum 1 is Planctomycetes, phylum 2 is Patescibacteria (unnamed phylum), phylum 3 is Chloroflexi, phylum 4 is Thermodesulfurobacteria, phylum 5 is Verrucomicrobia, phylum 6 is Deinococcus, phylum 7 is Campylobacter, phylum 8 is Firmicutes, phylum 9 is Bacteroidetes, and phylum 10 is Proteobacteria.
[0140] The initial sludge was mainly composed of Proteobacteria, Bacteroidota, Firmicutes and Deinococcota. After acclimation, a large number of Campylobacterota were enriched in the electrochemical sulfur autotrophic reactor, and its relative abundance in the reactor reached 55.48%. According to literature reports, Campylobacterota is related to sulfur autotrophic denitrifying bacteria, indicating that sulfur autotrophic denitrifying bacteria show advantages under the acclimation of the electrochemical sulfur autotrophic process, and the reactor has excellent sulfur autotrophic microbial affinity. At the same time, the relative abundance of Firmicutes decreased, which may be due to the low C / N ratio and the microbial selectivity on the surface of the electrochemical sulfur autotrophic bioreactor.
[0141] As attached Figure 2 It shows that genus 1 is sediment marine phagocytic bacteria, genus 2 is mesophilic cold microbacteria, genus 3 is Lachnospira, genus 4 is Theilonia, genus 5 is Truppella, genus 6 is Sarcina, genus 7 is another marine source bacteria, genus 8 is granular bacteria, genus 9 is lake sediment Bacillus, and genus 10 is Thiomonas.
[0142] The main microbial genera in the reactor were Sulfurimonas, Limnobacter, Lentimicrobium, Sporosarcina, Truepera and Tissierella. Sulfurimonas was the dominant genus, and its relative abundance increased from undetected to 60.16% on the 70th day, and continued to increase. The significant dominance of Sulfurimonas indicated that the filler used in the reactor had the ability to quickly start efficient sulfur autotrophic denitrification in situ.
[0143] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A pyrite electrode, characterized in that: It comprises a plurality of sheet-like pyrite sheets, wherein the pyrite sheets comprise a melt-blown mixed grid substrate and pyrite powder attached to the melt-blown mixed grid substrate; A polypropylene fiber layer is formed by melt-blowing and graphene conductive yarn is doped in the melt-blowing process, and a melt-blown mixed grid substrate is obtained after cooling and solidification; the average diameter of the graphene conductive yarn is greater than the average diameter of the polypropylene fiber; The pyrite powder is doped with microporous membrane crushed material; Strip-shaped carbonate slow-release agents arranged in an interlaced and stacked manner are filled between the flaky pyrite sheets.
2. A pyrite electrode according to claim 1, characterized in that: The strip carbonate slow-release agent contains 10-30% of a binder.
3. A pyrite electrode according to claim 2, characterized in that: The binder is selected from one of sodium alginate, xanthan gum, gum arabic, polyacrylic acid and polyethylene imine.
4. A pyrite electrode according to claim 1, characterized in that: The proportion of the microporous membrane crushed material in the pyrite powder is 10 to 30 wt %.
5. A pyrite electrode according to claim 1, characterized in that: The microporous membrane crushed material is selected from sulfonic acid group modified microporous membrane or sulfonyl group modified microporous membrane.
6. A method for preparing a pyrite electrode according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: forming a polypropylene fiber layer by melt-blowing and doping graphene conductive yarn during the melt-blowing process, and obtaining a melt-blown mixed grid substrate after cooling and solidification; S2: preparing pyrite powder, coating and bonding the pyrite powder on a melt-blown mixed grid substrate to obtain a single sheet of pyrite; S3: stack multiple flaky pyrite sheets, apply staggered strips of carbonate slow-release agent between two flaky pyrite sheets, and press them tightly, with the pressure controlled at 100 kPa.