A kind of solid waste base sand and its preparation method and application in imitation stone paint
By combining the modified foamed ceramics of solid aldehyde compounds and modified foamed ceramics of solid phenolic compounds with partially hydrolyzed polyacrylamide modified foamed ceramics, the alkali corrosion resistance of solid waste-based sand in imitation stone paint is solved. and the problem of poor water resistance, the imitation stone paint effect of high adhesion, sealing and low-temperature construction has been achieved.
Patent Information
- Application Number
- CN202411169920.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing solid waste-based sand made of foamed ceramics has poor alkali corrosion resistance and water resistance in imitation stone paint.
Combined with solid aldehyde-based compounds modified foam ceramics and solid phenolic compounds modified foam ceramics and partially hydrolyzed polyacrylamide modified foam ceramics, the resistance of solid waste-based sand is improved by adjusting their mass ratio and preparation method. Alkaline corrosion and water resistance.
It significantly improves the alkali corrosion resistance and water resistance of imitation stone paint, simplifies the construction process, enhances the adhesion and sealing of the paint film, and realizes low-temperature construction and high-color hiding.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic materials, and in particular to solid waste base sand, a preparation method thereof and application thereof in stone-like paint. Background Art
[0002] Foamed ceramics are polymer materials with ceramic as the matrix. They are made from powdered solid waste as raw materials through high-temperature sintering. They have a porous structure and have good thermal insulation properties, corrosion resistance and easy processing. They can be used in construction, automobiles, aerospace and other fields.
[0003] After being crushed and ground, foamed ceramics can be used as solid waste base sand, which is applied to imitation stone paint to increase the roughness and adhesion of the paint surface. However, the existing solid waste base sand made of foamed ceramics used in imitation stone paint generally has the problems of poor alkali corrosion resistance and poor water resistance. Summary of the invention
[0004] The present invention provides a solid waste base sand and a preparation method thereof and application in stone-like paint, which solves the problem of poor alkali corrosion resistance and poor water resistance of solid waste base sand made of foamed ceramics in the related art when applied to stone-like paint.
[0005] The technical solution of the present invention is as follows:
[0006] A solid waste base sand comprises component A and component B, wherein component A comprises foamed ceramics modified by solid aldehyde compounds and foamed ceramics modified by solid phenol compounds, and component B comprises foamed ceramics modified by partially hydrolyzed polyacrylamide.
[0007] As a further technical solution, the mass ratio of the component A to the component B is 0.5~1:1.
[0008] The present invention limits the mass ratio of component A to component B to 0.5-1:1, thereby further improving the alkali corrosion resistance and water resistance of the stone-like paint prepared from solid waste-based sand.
[0009] As a further technical solution, the mass of the foamed ceramic modified by the solid aldehyde compound is greater than or equal to the mass of the foamed ceramic modified by the solid phenol compound.
[0010] The present invention limits the mass of the foamed ceramic modified by the solid aldehyde compound to be greater than or equal to the mass of the foamed ceramic modified by the solid phenol compound, thereby further improving the alkali corrosion resistance and water resistance of the stone-like paint prepared from the solid waste-based sand.
[0011] As a further technical solution, the mass of the foamed ceramic modified by the solid aldehyde compound is ≥ 2 times the mass of the foamed ceramic modified by the solid phenol compound.
[0012] The present invention limits the mass of the foamed ceramic modified by the solid aldehyde compound to ≥2 times the mass of the foamed ceramic modified by the solid phenol compound, thereby further improving the alkali corrosion resistance and water resistance of the stone-like paint prepared from solid waste-based sand.
[0013] As a further technical solution, the mass ratio of the solid aldehyde compound modified foamed ceramic to the solid phenol compound modified foamed ceramic is 12:3-13:2.
[0014] The present invention limits the mass ratio of the solid aldehyde compound modified foamed ceramic to the solid phenol compound modified foamed ceramic to 12:3-13:2, thereby further improving the alkali corrosion resistance and water resistance of the stone-like paint prepared from solid waste base sand.
[0015] As a further technical solution, the raw materials of the solid aldehyde compound modified foamed ceramic include a solid aldehyde compound and a foamed ceramic in a mass ratio of 1 to 2:30;
[0016] The raw materials of the solid phenol compound modified foamed ceramic include solid phenol compound and foamed ceramic in a mass ratio of 1 to 2:30;
[0017] The raw materials of the partially hydrolyzed polyacrylamide modified foamed ceramic include partially hydrolyzed polyacrylamide and foamed ceramic in a mass ratio of 2 to 4:30.
[0018] As a further technical solution, the number of aldehyde groups in the solid aldehyde compound is ≥2; the number of phenol groups in the solid phenol compound is ≥2.
[0019] As a further technical solution, the solid aldehyde compound can be any compound containing two or more aldehyde groups, preferably one or two of isophthalic acid dicarboxylic acid and trimesic acid; the solid phenol compound can be any compound containing two or more aldehyde groups, preferably one or more of pyrogallol, pyrogallol, and 1,2,4-pyrogallol.
[0020] As a further technical solution, the preparation method of the solid aldehyde compound modified foamed ceramic comprises the following steps: uniformly mixing the solid aldehyde compound, foamed ceramic and solvent, filtering, and drying to obtain the solid aldehyde compound modified foamed ceramic;
[0021] The preparation method of the solid phenol compound modified foamed ceramic comprises the following steps: uniformly mixing the solid phenol compound, foamed ceramic and solvent, filtering and drying to obtain the solid phenol compound modified foamed ceramic.
[0022] The preparation method of partially hydrolyzed polyacrylamide modified foamed ceramics comprises the following steps: uniformly mixing partially hydrolyzed polyacrylamide, foamed ceramics and solvent, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramics.
[0023] The present invention also proposes a method for preparing solid waste base sand, wherein solid aldehyde compound modified foamed ceramics and solid phenol compound modified foamed ceramics are uniformly mixed to obtain component A; and partially hydrolyzed polyacrylamide modified foamed ceramics are used as component B.
[0024] The present invention also proposes the use of the solid waste base sand or the solid waste base sand prepared by the preparation method in stone-like paint.
[0025] As a further technical solution, the imitation stone paint includes a primer and a topcoat. The raw materials of the primer include the following components in parts by mass: 100 parts of emulsion A, 1 to 3 parts of a film-forming aid, 0.15 to 0.35 parts of a defoamer, 30 to 50 parts of a silica sol, 0.3 to 0.9 parts of a bactericide, 1 to 3 parts of a thickener, 1.5 to 3.5 parts of propylene glycol, 135 to 150 parts of water, and 10 to 30 parts of component A. The raw materials of the topcoat include the following components in parts by mass: 3 to 5 parts of emulsion B, 40 to 50 parts of nano lithium silicate, 20 to 30 parts of component B, 0.2 to 0.4 parts of a wetting agent, and 22 to 27 parts of water.
[0026] As a further technical solution, the emulsion A includes one or both of aqueous chlorinated polypropylene emulsion and polysiloxane emulsion; and the emulsion B is fluorosilicone emulsion.
[0027] The working principle and beneficial effects of the present invention are:
[0028] 1. The present invention provides a solid waste base sand, comprising component A and component B, wherein component A comprises solid aldehyde compound modified foamed ceramics and solid phenol compound modified foamed ceramics, and component B comprises partially hydrolyzed polyacrylamide modified foamed ceramics. During the application of the solid waste base sand, component A and component B interact with each other to improve the crosslinking degree of the system, thereby improving the alkali corrosion resistance and water resistance of the imitation stone paint.
[0029] 2. The imitation stone paint provided by the present invention includes a primer and a topcoat. After the primer is applied to the substrate, the topcoat can be directly applied. The traditional process is to apply the primer first, then the intermediate layer, and finally the topcoat on the substrate. Compared with the traditional process, the present invention is simple to construct and saves a lot of manpower and material resources. In addition, the imitation stone paint provided by the present invention not only has strong penetration and high adhesion to the substrate, but also has good adhesion to the primer and the topcoat, and at the same time has good sealing, can be applied at low temperature, has good gloss, and color hiding power>94. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The raw materials in the following examples and comparative examples are as follows:
[0032] The foamed ceramic is prepared by the following method: 50 parts of molybdenum tailings, 20 parts of shale, 10 parts of perlite, 3 parts of zinc oxide, 3 parts of talc, 14.5 parts of calcium carbonate, 0.5 parts of silicon carbide, and 0.5 parts of sodium silicate pentahydrate are mixed and put into a closed ball mill to ball-mill the mixture until the fineness of the mixture is 250 mesh sieve residue ≤1.2%, and then transferred to a granulator to form 50 mesh granules, and then transferred to a mold for heat treatment, crushing and grinding to obtain foamed ceramics. The heat treatment is: heating to 900°C at a rate of 12°C / min, keeping warm for 25 minutes, heating to 1100°C at a rate of 5°C / min, keeping warm for 35 minutes, and cooling to room temperature at a rate of 15°C / min;
[0033] The weight average molecular weight of partially hydrolyzed polyacrylamide is 25 million, and the degree of hydrolysis is 28.5%;
[0034] The aqueous chlorinated polypropylene emulsion is aqueous chlorinated polypropylene emulsion X-696;
[0035] The polysiloxane emulsion is polysiloxane emulsion TS-702, with an active matter content of 80%;
[0036] Fluorosilicone emulsion SD5681;
[0037] The film-forming aid is dodecyl alcohol ester;
[0038] The defoamer is BYK-024;
[0039] The silica sol is a neutral silica sol with a silicon dioxide content of 29.9 wt%, a sodium oxide content of 0.06 wt%, and a viscosity (25 °C) of 3.39 MPa·s, purchased from Guangzhou Zhonggao Chemical Co., Ltd.
[0040] The thickener is thickener AR-2;
[0041] The effective substance content in nano lithium silicate is 22.7wt%;
[0042] The wetting agent is BYK-346.
[0043] Example 1
[0044] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0045] S2, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0046] S3, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0047] S4, 2 parts of the foamed ceramic modified by the solid aldehyde compound and 8 parts of the foamed ceramic modified by the solid phenol compound are mixed evenly to obtain component A; 25 parts of the foamed ceramic modified by the partial hydrolysis of polyacrylamide are obtained to obtain component B;
[0048] S5, 80 parts of water-based chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 10 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed uniformly to obtain a primer;
[0049] S6. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0050] Example 2
[0051] S1. Dissolve 1 g of isophthalaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 20 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0052] S2, dissolving 1 g of pyrogallol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 35 min, filtering, and drying to obtain a solid phenol compound modified foamed ceramics;
[0053] S3, dissolving 2 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0054] S4, mixing 2 parts of solid aldehyde compound modified foamed ceramics and 8 parts of solid phenol compound modified foamed ceramics to obtain component A; partially hydrolyzing 20 parts of polyacrylamide modified foamed ceramics to obtain component B;
[0055] S5, 100 parts of water-based chlorinated polypropylene emulsion, 1 part of film-forming aid, 0.15 parts of defoamer, 30 parts of silica sol, 0.3 parts of bactericide, 1 part of thickener, 10 parts of component A, 1.5 parts of propylene glycol, and 135 parts of water are mixed uniformly to obtain a primer;
[0056] S6. Evenly mix 3 parts of fluorosilicone emulsion, 40 parts of nano lithium silicate, 20 parts of component B, 0.2 parts of wetting agent and 22 parts of water to obtain a topcoat.
[0057] Example 3
[0058] S1. Dissolve 1.5 g of isophthalaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 20 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0059] S2, dissolving 1.5 g of 1,2,4-pyrogallol in 450 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 35 min, filtering, and drying to obtain a solid phenol compound modified foamed ceramic;
[0060] S3, dissolving 4 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 40 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0061] S4, 2 parts of the solid aldehyde compound modified foamed ceramic and 8 parts of the solid phenol compound modified foamed ceramic are mixed evenly to obtain component A; 30 parts of the polyacrylamide modified foamed ceramic are partially hydrolyzed to obtain component B;
[0062] S5, 100 parts of polysiloxane emulsion, 3 parts of film-forming aid, 0.35 parts of defoamer, 50 parts of silica sol, 0.9 parts of bactericide, 3 parts of thickener, 10 parts of component A, 3.5 parts of propylene glycol and 150 parts of water are mixed uniformly to obtain a primer;
[0063] S6. Evenly mix 5 parts of fluorosilicone emulsion, 50 parts of nano-lithium silicate, 30 parts of component B, 0.4 parts of wetting agent and 27 parts of water to obtain a topcoat.
[0064] Example 4
[0065] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0066] S2, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0067] S3, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0068] S4, 2.5 parts of the foamed ceramic modified by the solid aldehyde compound and 10 parts of the foamed ceramic modified by the solid phenol compound are mixed evenly to obtain component A; 25 parts of the foamed ceramic modified by partially hydrolyzing polyacrylamide are obtained to obtain component B;
[0069] S5, 80 parts of water-based chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 12.5 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed to obtain a primer;
[0070] S6. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0071] Example 5
[0072] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0073] S2, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0074] S3, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0075] S4, 3 parts of the foamed ceramic modified by the solid aldehyde compound and 12 parts of the foamed ceramic modified by the solid phenol compound are mixed evenly to obtain component A; 25 parts of the foamed ceramic modified by the partial hydrolysis of polyacrylamide are obtained to obtain component B;
[0076] S5, 80 parts of water-based chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 15 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed uniformly to obtain a primer;
[0077] S6. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0078] Example 6
[0079] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0080] S2, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0081] S3, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0082] S4, evenly mixing 5 parts of the foamed ceramic modified by the solid aldehyde compound and 20 parts of the foamed ceramic modified by the solid phenol compound to obtain component A; partially hydrolyzing 25 parts of the foamed ceramic modified by polyacrylamide to obtain component B;
[0083] S5, 80 parts of aqueous chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 25 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed uniformly to obtain a primer;
[0084] S6. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0085] Example 7
[0086] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0087] S2, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0088] S3, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0089] S4, 6 parts of the foamed ceramic modified by the solid aldehyde compound and 24 parts of the foamed ceramic modified by the solid phenol compound are mixed evenly to obtain component A; 25 parts of the foamed ceramic modified by partially hydrolyzing polyacrylamide are obtained to obtain component B;
[0090] S5, 80 parts of water-based chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 30 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed to obtain a primer;
[0091] S6. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0092] Example 8
[0093] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0094] S2, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0095] S3, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0096] S4, 7.5 parts of the solid aldehyde compound modified foamed ceramic and 7.5 parts of the solid phenol compound modified foamed ceramic are mixed evenly to obtain component A; 25 parts of the polyacrylamide modified foamed ceramic are partially hydrolyzed to obtain component B;
[0097] S5, 80 parts of water-based chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 15 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed uniformly to obtain a primer;
[0098] S6. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0099] Example 9
[0100] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0101] S2, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0102] S3, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0103] S4, 10 parts of the solid aldehyde compound modified foamed ceramic and 5 parts of the solid phenol compound modified foamed ceramic are mixed evenly to obtain component A; 25 parts of the polyacrylamide modified foamed ceramic are partially hydrolyzed to obtain component B;
[0104] S5, 80 parts of water-based chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 15 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed uniformly to obtain a primer;
[0105] S6. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0106] Example 10
[0107] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0108] S2, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0109] S3, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0110] S4, 12 parts of solid aldehyde compound modified foamed ceramics and 3 parts of solid phenol compound modified foamed ceramics are mixed evenly to obtain component A; 25 parts of polyacrylamide modified foamed ceramics are partially hydrolyzed to obtain component B;
[0111] S5, 80 parts of water-based chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 15 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed uniformly to obtain a primer;
[0112] S6. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0113] Embodiment 11
[0114] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0115] S2, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0116] S3, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0117] S4, 13 parts of solid aldehyde compound modified foamed ceramics and 2 parts of solid phenol compound modified foamed ceramics are mixed evenly to obtain component A; 25 parts of polyacrylamide modified foamed ceramics are partially hydrolyzed to obtain component B;
[0118] S5, 80 parts of water-based chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 15 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed uniformly to obtain a primer;
[0119] S6. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0120] Example 12
[0121] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0122] S2, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0123] S3, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0124] S4, 14 parts of the solid aldehyde compound modified foamed ceramic and 1 part of the solid phenol compound modified foamed ceramic are mixed evenly to obtain component A; 25 parts of the polyacrylamide modified foamed ceramic are partially hydrolyzed to obtain component B;
[0125] S5, 80 parts of water-based chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 15 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed uniformly to obtain a primer;
[0126] S6. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0127] Comparative Example 1
[0128] S1. Dissolve 2 g of trimesaldehyde in 450 mL of ethanol, add 30 g of foamed ceramic, perform ultrasonic treatment for 30 min, filter, and dry to obtain a solid aldehyde compound modified foamed ceramic;
[0129] S2, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0130] S3, modifying 10 parts of foamed ceramics with solid aldehyde compounds to obtain component A; partially hydrolyzing polyacrylamide to modify 25 parts of foamed ceramics to obtain component B;
[0131] S4, 80 parts of aqueous chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 10 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed uniformly to obtain a primer;
[0132] S5. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0133] Comparative Example 2
[0134] S1, dissolving 2 g of phloroglucinol in 450 mL of ethanol, adding 30 g of foamed ceramics, ultrasonicating for 45 min, filtering, and drying to obtain a solid phenolic compound modified foamed ceramics;
[0135] S2, dissolving 3 g of partially hydrolyzed polyacrylamide in 500 mL of ethanol, adding 30 g of foamed ceramic, ultrasonicating for 50 min, filtering, and drying to obtain partially hydrolyzed polyacrylamide modified foamed ceramic;
[0136] S3, 10 parts of foamed ceramics modified by solid phenolic compounds to obtain component A; 25 parts of foamed ceramics modified by partial hydrolysis of polyacrylamide to obtain component B;
[0137] S4, 80 parts of aqueous chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 10 parts of component A, 2.5 parts of propylene glycol, and 147 parts of water were mixed uniformly to obtain a primer;
[0138] S5. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of component B, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0139] Comparative Example 3
[0140] S1, 80 parts of water-based chlorinated polypropylene emulsion, 20 parts of polysiloxane emulsion, 2 parts of film-forming aid, 0.25 parts of defoamer, 40 parts of silica sol, 0.5 parts of bactericide, 2 parts of thickener, 10 parts of foamed ceramic, 2.5 parts of propylene glycol, and 147 parts of water are mixed uniformly to obtain a primer;
[0141] S2. Evenly mix 4 parts of fluorosilicone emulsion, 45 parts of nano-lithium silicate, 25 parts of foamed ceramic, 0.3 parts of wetting agent and 25 parts of water to obtain a topcoat.
[0142] The primer and topcoat obtained in Examples 1 to 12 and Comparative Examples 1 to 3 were coated on a substrate to prepare a test sample. The substrate was the substrate specified in GB / T 9265-2009. Coating method: the primer was coated on the substrate and baked at 50°C for 30 minutes to obtain a primer layer with a thickness of 1 mm; the topcoat was coated on the primer layer and baked at 50°C for 35 minutes to obtain a topcoat layer. The alkali resistance test was performed with reference to the method in GB / T 9265-2009, and the time when the paint film was free of abnormalities, that is, the time when it did not bubble, fall off, or powder fall off was recorded. The water resistance test was performed with reference to Method A in GB / T 1733-1993, and the time when the paint film was free of abnormalities, that is, the time when it did not bubble, fall off, or powder fall off was recorded. The test results are recorded in Table 1.
[0143] Table 1 Alkali resistance and water resistance
[0144]
[0145] It can be seen from Table 1 that the paint film provided by the present invention has good alkali resistance and water resistance.
[0146] Compared with Comparative Examples 1 to 3, Examples 1 to 12 include solid aldehyde compound modified foamed ceramics, solid phenol compound modified foamed ceramics and partially hydrolyzed polyacrylamide modified foamed ceramics, Comparative Example 1 includes solid aldehyde compound modified foamed ceramics and partially hydrolyzed polyacrylamide modified foamed ceramics, Comparative Example 2 includes solid phenol compound modified foamed ceramics and partially hydrolyzed polyacrylamide modified foamed ceramics, and Comparative Example 3 includes unmodified foamed ceramics. The alkali resistance no abnormality time and water resistance no abnormality time of the paint films obtained in Examples 1 to 12 are higher than those in Comparative Examples 1 to 3, indicating that the combination of solid aldehyde compound modified foamed ceramics, solid phenol compound modified foamed ceramics and partially hydrolyzed polyacrylamide modified foamed ceramics can improve the alkali corrosion resistance and water resistance of the imitation stone paint.
[0147] The alkali resistance-free abnormality time and water resistance-free abnormality time of the paint films obtained in Examples 4 to 6 are higher than those in Example 1 and Example 7, indicating that the mass ratio of the solid aldehyde compound modified foamed ceramic and the solid phenol compound modified foamed ceramic to the partially hydrolyzed polyacrylamide modified foamed ceramic is 0.5 to 1:1, which can further improve the alkali corrosion resistance and water resistance of the imitation stone paint.
[0148] The alkali resistance and water resistance of the paint films obtained in Examples 8 to 12 are longer than those in Example 5, indicating that the quality of the foamed ceramic modified by the solid aldehyde compound is ≥ the quality of the foamed ceramic modified by the solid phenol compound, which can further improve the alkali corrosion resistance and water resistance of the stone-like paint.
[0149] The alkali resistance and water resistance of the paint films obtained in Examples 9 to 12 are longer than those in Example 8, indicating that the mass of the foamed ceramic modified by the solid aldehyde compound is ≥2 times the mass of the foamed ceramic modified by the solid phenol compound, which can further improve the alkali corrosion resistance and water resistance of the stone-like paint.
[0150] The alkali resistance-free abnormality time and water resistance-free abnormality time of the paint films obtained in Examples 10 to 11 are higher than those in Example 9 and Example 12, indicating that the mass ratio of the solid aldehyde compound modified foamed ceramic to the solid phenol compound modified foamed ceramic is 12:3 to 13:2, which can further improve the alkali corrosion resistance and water resistance of the imitation stone paint.
[0151] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. Application of solid waste base sand in stone-like paint, characterized in that: The solid waste base sand comprises component A and component B, wherein component A comprises solid aldehyde compound modified foamed ceramic and solid phenol compound modified foamed ceramic, and component B comprises partially hydrolyzed polyacrylamide modified foamed ceramic; the imitation stone paint comprises primer and topcoat, and the raw materials of the primer comprise the following components in parts by weight: 100 parts of emulsion A, 1-3 parts of film-forming aid, 0.15-0.35 parts of defoamer, 30-50 parts of silica sol, 0.3-0.9 parts of bactericide, 1-3 parts of thickener, 1.5-3.5 parts of propylene glycol, 135-150 parts of water, and 10-30 parts of component A; the raw materials of the topcoat comprise the following components in parts by weight: 3-5 parts of emulsion B, 40-50 parts of nano lithium silicate, and 10-30 parts of component B. 20-30 parts, 0.2-0.4 parts of wetting agent, 22-27 parts of water; the solid aldehyde compound is one or two of isophthalaldehyde and trimesic acid; the solid phenol compound is one or more of phloroglucinol, pyrogallol, and 1,2,4-pyrogallol.
2. The use according to claim 1, characterized in that: The mass ratio of the component A to the component B is 0.5-1:
1.
3. The use according to claim 2, characterized in that: The mass of the foamed ceramic modified by the solid aldehyde compound is greater than the mass of the foamed ceramic modified by the solid phenol compound.
4. The use according to claim 3, characterized in that: The mass of the solid aldehyde compound modified foamed ceramic is ≥2 times the mass of the solid phenol compound modified foamed ceramic.
5. The use according to claim 4, characterized in that: The mass ratio of the solid aldehyde compound modified foamed ceramic to the solid phenol compound modified foamed ceramic is 12:3-13:
2.
6. The use according to claim 5, characterized in that: The raw materials of the solid aldehyde compound modified foamed ceramic include solid aldehyde compound and foamed ceramic in a mass ratio of 1 to 2:30; The raw materials of the solid phenol compound modified foamed ceramic include solid phenol compound and foamed ceramic in a mass ratio of 1 to 2:30; The raw materials of the partially hydrolyzed polyacrylamide modified foamed ceramic include partially hydrolyzed polyacrylamide and foamed ceramic in a mass ratio of 2 to 4:
30.
7. The use according to any one of claims 1 to 6, characterized in that: The preparation method of the solid waste base sand comprises: uniformly mixing solid aldehyde compound modified foamed ceramics and solid phenol compound modified foamed ceramics to obtain component A; and partially hydrolyzing polyacrylamide modified foamed ceramics as component B.
8. The use according to claim 1, characterized in that: The emulsion A comprises one or both of water-based chlorinated polypropylene emulsion and polysiloxane emulsion; the emulsion B is fluorosilicone emulsion.
Citation Information
Patent Citations
Silicic ester modified phenol / formaldehyde novolaks and their use for the production of resin coated substrates
CN103562247A