A rare earth functional antibacterial fiber containing lanthanum and preparation method thereof

By using rare earth functional materials as antibacterial agents in antibacterial fibers and using their catalytic reactive oxygen generation ability, the toxicity and environmental pollution problems of antibacterial agents in existing antibacterial fibers are solved, and efficient and environmentally friendly antibacterial effects and simplified processes are achieved.

CN118685879BActive Publication Date: 2024-11-12TIANJIN BAOGANG RES INST OF RARE EARTHS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411179101.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Commonly used antibacterial agents such as silver ions and metal oxides in existing antibacterial fibers have problems such as high cost, high physiological toxicity, and drug resistance. In addition, traditional spinning technology has a high pollution to the environment, so we need to seek environmentally friendly and effective preparation of antibacterial fibers. method.

Method used

Rare earth functional materials are used as antibacterial additives. Through the optimization of the coating process, the rare earth functional composite materials are introduced into the surface of melt-spun polyurethane fibers with the help of the adhesive, and the catalytic reactive oxygen generation capacity of rare earth elements such as lanthanum, cerium and samarium are used. Prepare antibacterial fibers containing lanthanum rare earth functionally with high antibacterial properties.

Benefits of technology

It achieves an efficient bactericidal rate (>99%) for common bacteria, improves the firmness and environmental protection of the fibers, and does not require complex equipment and solvents in the process, reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118685879B_ABST
    Figure CN118685879B_ABST
Patent Text Reader

Abstract

The present invention provides a lanthanum-containing rare earth functional antibacterial fiber and a preparation method thereof. The antibacterial fiber contains a lanthanum-containing rare earth functional antibacterial additive, which is prepared from a rare earth functional material, a first high molecular polymer and a solvent in a mass ratio of (1-2): (3-6): (12-16). The lanthanum-containing rare earth functional antibacterial additive of the present invention can improve the antibacterial properties of fiber fabrics. The antibacterial performance evaluation of the lanthanum-containing rare earth functional antibacterial additive shows that the sterilization rate of common Gram-positive bacteria and Gram-negative bacteria in life is greater than 99%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of textile fibers, and in particular relates to a lanthanum-containing rare earth functional antibacterial fiber and a preparation method thereof. Background Art

[0002] Bacterial infection has always been a thorny public problem worldwide, and has long been a serious threat to human health and public safety. A large number of studies have shown that bacteria are the source of transmission of many diseases, such as cholera, tuberculosis, typhoid fever, tetanus, etc. In order to deal with bacterial infections, antibacterial materials in various forms have been developed and applied to different fields, such as antibacterial hydrogels, antibacterial fibers, antibacterial ceramics, etc. Among them, antibacterial fiber products have long been widely used in daily care for special populations, environmental fields, medical systems, and some household textiles.

[0003] Antibacterial fibers are usually made by adding antibacterial agents during the spinning process or after finishing. Commonly used antibacterial agents include silver ions, metal oxides, antibiotics, etc. However, these antibacterial agents have problems such as high cost, high physiological toxicity, and drug resistance, and are subject to certain restrictions in certain application areas. Natural medicinal plants have been widely used in Asia for a long time. They play a vital role in preventing and treating diseases. Therefore, some relatively safe and environmentally friendly natural antibacterial agents extracted from plants or animals have received increasing attention in the preparation of antibacterial fibers.

[0004] Polyurethane (PU) is one of the most widely used polymers. PU has excellent elasticity, breathability, biocompatibility and good processability, and is widely used in coatings, foams, clothing, biomedicine and other fields. In the field of large-scale fiber spinning, the main processing methods of PU are melt spinning, wet spinning and dry spinning, but dry spinning and wet spinning will inevitably cause a certain degree of environmental pollution due to the presence of solvents. Melt spinning has a fast production speed, a short process flow, and does not require complex equipment, solvents and precipitants. Therefore, the application of melt spinning technology will likely dominate the production of polyurethane fibers in the future.

[0005] Rare earth ions have strong coordination ability, photostability, low teratogenicity, low toxicity and antibacterial properties. + Compared with traditional Chinese medicine, rare earth metals have obvious advantages. As antibacterial agents, rare earth metals can be continuously released to achieve long-lasting antibacterial activity. Summary of the invention

[0006] In view of this, the present invention aims to overcome the defects in the prior art and proposes a lanthanum-containing rare earth functional antibacterial fiber and a preparation method thereof. The present invention selects rare earth functional materials as antibacterial additive components and systematically studies their antibacterial properties and antibacterial mechanisms. Through an optimized coating process, with the help of an adhesive, the rare earth functional composite material is introduced into the surface of the melt-spun polyurethane fiber, and the antibacterial properties of the fiber are systematically evaluated.

[0007] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0008] In a first aspect, the present invention provides a lanthanum-containing rare earth functional antibacterial additive, which is prepared from a rare earth functional material, a first high molecular polymer and a solvent in a mass ratio of (1 ~ 2): (3 ~ 6): (12 ~ 16), wherein the rare earth functional material includes a rare earth carbonate compound and / or a rare earth nitrate compound; the first high molecular polymer includes one or more of polyamide (PA), polyurethane (PU), polyvinyl chloride (PVC), polyethylene terephthalate (PET), polyethylene (PE), polyvinyl alcohol (PVA), and polyethylenediamine (PEI).

[0009] Preferably, the rare earth functional material includes lanthanum carbonate hexahydrate (La2C3O9·6H2O), cerium carbonate hexahydrate (Ce2C3O9·6H2O), and samarium nitrate hexahydrate (SmN3O9·6H2O) in a mass ratio of (1-4): (2-6): (6-24).

[0010] Preferably, the mass ratio of the rare earth functional material, the high molecular polymer and the solvent is 1:4:15.

[0011] Preferably, the solvent is water.

[0012] In a second aspect, the present invention provides a method for preparing the above-mentioned lanthanum-containing rare earth functional antibacterial additive, comprising the following steps:

[0013] After the rare earth functional material and the solvent are mixed, the first high molecular polymer is added, and the temperature is raised to 90-95°C while stirring. After reacting for 2-3 hours, a mixed solution is obtained. The temperature of the obtained mixed solution is raised to 180-200°C, and the mixture is reacted overnight for more than 12 hours. The reacted solution is taken out, cooled to room temperature, and centrifuged to remove the supernatant. The precipitate after centrifugation is collected to obtain a lanthanum-containing rare earth functional antibacterial additive.

[0014] In a third aspect, the present invention further provides a lanthanum-containing rare earth functional antibacterial fiber, which is prepared from the following components in parts by weight:

[0015] 5-10 parts of rare earth functional material slurry;

[0016] 1-5 parts of silane coupling agent;

[0017] 85-94 parts of the second high molecular weight polymer;

[0018] The preparation method of the rare earth functional material slurry is as follows: taking the above-mentioned rare earth functional antibacterial additive containing lanthanum, adding water and an aqueous dispersant, stirring evenly, and then sand-milling to make its particle size distribution between 200 and 300 nm.

[0019] Preferably, the content of the lanthanum-containing rare earth functional antibacterial additive in the rare earth functional material slurry is 30-175 g of the lanthanum-containing rare earth functional antibacterial additive per liter of water.

[0020] Preferably, the preparation method of the rare earth functional material slurry is: take 30-70g of a lanthanum-containing rare earth functional antibacterial additive, add it to 400-1000mL of water, then add 2-6g of an aqueous dispersant, stir evenly and place it in a sand mill for sand grinding, the total sand grinding time is 4-8h, and after the sand grinding is completed, a rare earth functional material slurry that is evenly dispersed and has a particle size distribution between 200~300nm is obtained.

[0021] Preferably, the second high molecular polymer includes polyvinyl alcohol (PVA), polyethylene (PE), polyurethane (PU), polyethylenediamine (PEI) and polyamide (PA) in a mass ratio of 1:1:1:1:1.

[0022] In a third aspect, the present invention further provides a method for preparing the above-mentioned lanthanum-containing rare earth functional antibacterial fiber, comprising the following steps:

[0023] S1: Mix the above rare earth functional material slurry and silane coupling agent and add them into a high-speed kneader for high-speed mixing for 8 to 10 minutes;

[0024] S2: The dried second polymer is sequentially added into a high-speed kneader and mixed for 15 to 20 minutes, melt-blended at 200 to 250°C, extruded through an extruder, cooled and granulated to obtain an antibacterial masterbatch;

[0025] S3: The screw temperature of the screw extrusion spinning machine is set to 280-300° C., the antibacterial masterbatch is placed in the screw extrusion spinning machine and passed through a spinneret assembly to obtain a lanthanum-containing rare earth functional antibacterial fiber.

[0026] The raw materials of the lanthanum-containing rare earth functional antibacterial additive of the present invention include lanthanum carbonate hexahydrate, cerium carbonate hexahydrate and samarium nitrate hexahydrate as rare earth compounds. The lanthanum, cerium and samarium rare earth elements can catalyze the production of active oxygen due to their unique electrical layer structure and infrared radiation. The active oxygen has very strong oxidizing properties and can cause radical oxidation reactions of microorganisms, thereby killing and inhibiting the growth of microorganisms. This catalytic ability will be significantly enhanced when these three groups of elements are combined together.

[0027] Compared with the prior art, the present invention has the following advantages:

[0028] (1) The lanthanum-containing rare earth functional antibacterial additive provided by the present invention can improve the antibacterial performance of fiber fabrics. The antibacterial performance evaluation of the lanthanum-containing rare earth functional antibacterial additive shows that the bactericidal rate against common Gram-positive bacteria and Gram-negative bacteria in life is greater than 99%;

[0029] (2) The introduction of polyurethane (PU) and polyethylenediamine (PEI) into the antibacterial fiber of the present invention improves the firmness of the antibacterial fiber;

[0030] (3) In the present invention, the particle size distribution of the lanthanum-containing rare earth functional antibacterial additive in the preparation of the lanthanum-containing rare earth functional antibacterial fiber is between 200 and 300 nm. Within this particle size range, it can be attached to the surface of microorganisms, cut off the nutrient exchange between the microorganisms and the outside world, and then cause the death of the microorganisms. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a scanning electron microscope image of a lanthanum-containing rare earth functional antibacterial additive;

[0032] Figure 2 This is a particle size distribution diagram of the rare earth functional antibacterial additive containing lanthanum;

[0033] Figure 3 This is a diagram showing the catalytic active oxygen effect of lanthanum-containing rare earth functional antibacterial additives;

[0034] Figure 4 This is a comparison diagram of the catalytic active oxygen effects of lanthanum-containing rare earth functional antibacterial additives;

[0035] Figure 5 The effect of coating the plates for Escherichia coli and Staphylococcus aureus;

[0036] Figure 6 The following is a comparison chart of spinning products for different application examples. DETAILED DESCRIPTION

[0037] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0038] The present invention will be described in detail below with reference to the embodiments.

[0039] Lanthanum carbonate (La2C3O9·6H2O), cerium carbonate (Ce2C3O9·6H2O), samarium nitrate (SmN3O9·6H2O), polyamide (PA), polyurethane (PU), polyvinyl chloride (PVC), polyethylene terephthalate (PET), polyethylene (PE), polyvinyl alcohol (PVA), polyethylene diamine (PEI), and aqueous dispersants were purchased from Aladdin Chemical Co., Ltd. All chemicals were used without further treatment, and distilled water (ρ=18.2 MΩ·cm, 25℃) was from Millipore milli-Q water purification system. Escherichia coli ( E. coli ) and Staphylococcus aureus ( S. aureus ) were obtained from Beijing Sihuan Biopharmaceutical Co., Ltd. Unless otherwise specified, all biochemical reagents were conventional; the experimental methods described were conventional methods unless otherwise specified.

[0040] The present invention is described in detail below in conjunction with embodiments.

[0041] Example 1

[0042] Add 150 mL of deionized water to a 250 mL beaker, take 10 g of rare earth functional material, the mass ratio of lanthanum carbonate (La2C3O9·6H2O), cerium carbonate (Ce2C3O9·6H2O), and samarium nitrate hexahydrate (SmN3O9·6H2O) in the rare earth functional material is 1:3:6, add 40 g of the first polymer, the mass ratio of polyvinyl alcohol (PVA), polyethylene (PE), and polyethylenediamine (PEI) in the first polymer is 1:1:2, stir at a constant speed of 200 rpm on a magnetic stirrer, and raise the temperature to 90°C. After reacting for 3 h, transfer the above mixed solution to a round-bottom flask, adjust the oil bath temperature to 200°C, and react overnight for more than 12 h. The solution after the reaction was taken out and cooled to room temperature. The mixed solution was divided into 50 mL centrifuge tubes and centrifuged at 12000 rpm for 20 min. The supernatant was removed and the precipitate after centrifugation was collected in an Ep tube. The precipitate obtained was the lanthanum-containing rare earth functional antibacterial additive.

[0043] Example 2

[0044] Add 160 mL of deionized water to a 250 mL beaker, take 20 g of rare earth functional material, the mass ratio of lanthanum carbonate (La2C3O9·6H2O), cerium carbonate (Ce2C3O9·6H2O), and samarium nitrate hexahydrate (SmN3O9·6H2O) in the rare earth functional material is 1:3:6, add 30 g of the first polymer, the first polymer is composed of polyvinyl alcohol (PVA), polyvinyl chloride (PVC), and polyurethane (PU) in a mass ratio of 1:1:1, stir at a constant speed of 200 rpm on a magnetic stirrer, and raise the temperature to 90°C. After reacting for 3 h, transfer the above mixed solution to a round-bottom flask, adjust the oil bath temperature to 200°C, and react overnight for more than 12 h. The solution after the reaction was taken out and cooled to room temperature. The mixed solution was divided into 50 mL centrifuge tubes and centrifuged at 12000 rpm for 20 min. The supernatant was removed and the precipitate after centrifugation was collected in an Ep tube. The precipitate obtained was the lanthanum-containing rare earth functional antibacterial additive.

[0045] Example 3

[0046] Add 120 mL of deionized water and 10 g of rare earth functional material into a 250 mL beaker. The mass ratio of lanthanum carbonate (La2C3O9·6H2O), cerium carbonate (Ce2C3O9·6H2O), and samarium nitrate hexahydrate (SmN3O9·6H2O) in the rare earth functional material is 3:2:24. Add 60 g of the first polymer, which is composed of polyamide (PA), polyethylene (PE), and polyethylene terephthalate (PET) in a mass ratio of 1:1:1. Stir at a constant speed of 200 rpm on a magnetic stirrer, and raise the temperature to 90°C. After reacting for 3 h, transfer the mixed solution to a round-bottom flask, adjust the oil bath temperature to 200°C, and react overnight for more than 12 h. The solution after the reaction was taken out and cooled to room temperature. The mixed solution was divided into 50 mL centrifuge tubes and centrifuged at 12000 rpm for 20 min. The supernatant was removed and the precipitate after centrifugation was collected in an Ep tube. The precipitate obtained was the lanthanum-containing rare earth functional antibacterial additive.

[0047] Example 4

[0048] The difference between Example 4 and Example 1 is that the first high molecular polymer is polyethylene (PE) with a mass of 40 g.

[0049] Example 5

[0050] The difference between Example 5 and Example 1 is that the first high molecular polymer is polyamide (PA) with a mass of 40 g.

[0051] Example 6

[0052] The difference between Example 6 and Example 1 is that the first high molecular polymer is 20 g of polyvinyl chloride (PVC) and 20 g of polyethylene terephthalate (PET).

[0053] Example 7

[0054] The difference between Example 7 and Example 1 is that the first high molecular polymer is 10 g of polyamide (PA), 10 g of polyurethane (PU), 10 g of polyvinyl chloride (PVC), and 10 g of polyethylene terephthalate (PET).

[0055] Example 8

[0056] The difference between Example 8 and Example 1 is that the first high molecular polymer is 5g of polyamide (PA), 5g of polyurethane (PU), 5g of polyvinyl chloride (PVC), 5g of polyethylene terephthalate (PET), 10g of polyethylene (PE), and 10g of polyvinyl alcohol (PVA).

[0057] Example 9

[0058] The difference between Example 9 and Example 1 is that the first high molecular polymer is 5g polyamide (PA), 5g polyurethane (PU), 5g polyvinyl chloride (PVC), 5g polyethylene terephthalate (PET), 5g polyethylene (PE), 5g polyvinyl alcohol (PVA), and 10g polyethylenediamine (PEI).

[0059] Take 50g of the lanthanum-containing rare earth functional antibacterial additive prepared in Examples 1-9, add them to 450mL of water, add 5g of aqueous 2800 dispersant, stir evenly, and place them in a sand mill for sand milling. The total sand milling time is 6 hours. After the sand milling is completed, a uniformly dispersed rare earth functional antibacterial additive slurry is obtained.

[0060] Figure 1 The SEM scanning electron microscope image of the lanthanum-containing rare earth functional antibacterial additive prepared in Example 1 is shown. A particle size analyzer is used to monitor the particle size distribution of the lanthanum-containing rare earth functional antibacterial additive in the slurry. Figure 2 It can be seen that the particle size of the rare earth functional antibacterial additive containing lanthanum in the slurry is stable at around 295 nm. The particle size of the antibacterial additive containing lanthanum in the slurry prepared in Example 2-9 is stable at 200-300 nm.

[0061] Comparative Example 1

[0062] The difference between Comparative Example 1 and Example 1 is that the rare earth functional material is lanthanum carbonate (La2C3O9·6H2O) with a mass of 10 g.

[0063] Comparative Example 2

[0064] The difference between Comparative Example 2 and Example 1 is that the rare earth functional material is 1 g of lanthanum carbonate (La2C3O9·6H2O) and 4 g of cerium carbonate hexahydrate (Ce2C3O9·6H2O).

[0065] Comparative Example 3

[0066] The difference between Comparative Example 3 and Example 1 is that the rare earth functional material is 1 g of lanthanum carbonate (La2C3O9·6H2O) and 6 g of samarium nitrate hexahydrate (SmN3O9·6H2O).

[0067] Comparative Example 4

[0068] The difference between Comparative Example 4 and Example 1 is that the rare earth functional material is lanthanum chloride, with a mass of 10 g.

[0069] Comparative Example 5

[0070] The difference between Comparative Example 3 and Example 1 is that the mass of the rare earth functional material is 30 g.

[0071] Comparative Example 6

[0072] The difference between Comparative Example 4 and Example 1 is that the mass of the rare earth functional material is 8 g.

[0073] Experimental Example 1 Effect of catalytic generation of active oxygen by lanthanum-containing rare earth functional antibacterial additives

[0074] In this experimental example 1, 2',7'-dichlorofluorescein diacetate (DCFH-DA) fluorescent probe is used to detect the catalytic active oxygen generation effect of lanthanum-containing rare earth functional antibacterial additives. DCFH-DA can be oxidized by active oxygen to 2'-7' dichlorofluorescein (DCF). DCF is a fluorescent compound that can be detected by a fluorescence spectrophotometer, and its excitation spectrum and emission spectrum are 495 nm and 529 nm, respectively.

[0075] The specific detection process is as follows: 0.146g of DCFH-DA (300μM) is added to a 2mL centrifuge tube, and 1mL of dimethyl sulfoxide is added to the centrifuge tube to prepare a mother solution, mixed and dissolved, and placed in a -20°C refrigerator for use. 0.05g of the lanthanum-containing rare earth functional antibacterial additive prepared in Examples 1-9 and Comparative Examples 1-6 is weighed into a 50mL centrifuge tube, 5mL of sodium acetate buffer is added to the centrifuge tube, and then 5mL of peroxidizing solution is added, and finally 10μL of DCFH-DA probe mother solution is added. After the shaking reaction, the fluorescence intensity at 525nm is detected by a fluorescence spectrophotometer when the excitation wavelength is 488 within 0-80min, and the active oxygen catalytic generation effect of the experimental material is judged according to the fluorescence intensity.

[0076] The experimental results of Example 1 are as follows Figure 3 As shown, Figure 3 From bottom to top, they are 0 min, 4 min, 8 min, 12 min, 16 min, 20 min, 24 min, 28 min, 32 min, 36 min, 40 min, 44 min, 48 min, 52 min, 56 min, 60 min, 64 min, 68 min and 72 min. It can be seen that the rare earth functional antibacterial additive containing lanthanum has a strong fluorescence signal, and as the reaction time increases, the fluorescence signal gradually increases, indicating that the rare earth functional antibacterial additive containing lanthanum can effectively catalyze the production of a large amount of reactive oxygen. As the reaction time increases, the accumulation of reactive oxygen increases. The accumulated reactive oxygen can destroy the cell membrane of microorganisms, thereby achieving the effect of inhibiting the growth of microorganisms.

[0077] Figure 4 The effect diagrams of Examples 1-9 and Comparative Examples 1-6 of the catalytic active oxygen of the rare earth functional antibacterial additive containing lanthanum are shown. The fluorescence signal intensity at 525nm was selected for the experiment. It can be seen from the data diagram that the signal intensity of the 9 examples is all above 100,000, while the signal intensity of the 6 comparative examples is around 10,000, indicating that the examples can effectively catalyze the generation of active oxygen. Although the comparative examples have the effect of catalyzing active oxygen, the catalytic intensity is far less than that of the examples of the present invention.

[0078] Test Example 2 Gram-positive bacteria Staphylococcus aureus ( S. aureus ) and Gram-negative bacteria Escherichia coli ( E. coli )

[0079] 100 μL of the frozen-thawed bacterial glycerol mixture ( S. aureus and E. coli ) were added to 900 μL of Luria-Bertani (LB) liquid medium and incubated at 37°C and 180 rpm in a shaker for 14 to 16 h to obtain suspensions of different types of bacteria with an optical density at 600 nm (OD 600 ) is used to evaluate the UV absorption value of S. aureus and E. coli The invention controls the OD 600 =0.4 ~ 0.6.

[0080] Test Example 3 Agar plate antibacterial test

[0081] The OD in Experimental Example 2 600 =0.4 ~ 0.6 S. aureus and E. coli The culture medium was diluted 10 4After 10 times the dilution, 0.1 mL of the diluted bacterial suspension was taken and spread on an LB agar plate. The above experiment was used as the control group. Repeat the above operation to prepare 3 groups of blank control groups.

[0082] The OD in Experimental Example 2 600 =0.4 ~ 0.6 S. aureus and E. coli The culture medium was diluted 10 3 After 2 times, 0.1 mL of the bacterial solution was transferred to a 2 mL Eppendorf tube after high-pressure sterilization, and 0.9 mL of 100 mg / L blank control, lanthanum-containing rare earth functional antibacterial additives prepared in Examples 1-9 and Comparative Examples 1-6 were added thereto. After being fully mixed by pipetting with a gun tip, the Eppendorf tube was transferred to a test tube rack and placed in a 37°C constant temperature incubator for incubation for 1 to 2 h.

[0083] Pipette 0.1 mL of rare earth functional antimicrobial agent and S. aureus The incubated suspension was spread on LB agar plates and the above operation was repeated to prepare 3 experimental groups. E. coli The incubated suspension was spread on LB agar plates and repeated for 3 groups.

[0084] like Figure 5 As shown in the blank control group S. aureus and E. coli The growth of S. aureus and E. coli All bacteria in the coated agar plates died. The variable was that the introduction of the new lanthanum-containing functional additive caused the bacterial survival rate to drop to 0%.

[0085] Application Example: Preparation of rare earth functional antibacterial fiber containing lanthanum

[0086] 1) 100 g of the rare earth functional antibacterial additive slurry prepared in Example 1, 25 g of A151 (vinyl triethoxysilane) and 25 g of A171 (vinyl trimethoxysilane) were mixed and added into a high-speed kneader for high-speed mixing for 10 min;

[0087] 2) 18 g of polyvinyl alcohol (PVA), 18 g of polyethylene (PE), 18 g of polyurethane (PU), 18 g of polyethylenediamine (PEI) and 18 g of polyamide (PA) were placed in an oven for drying;

[0088] 3) Polyvinyl alcohol (PVA), polyethylene (PE), polyurethane (PU), polyethylenediamine (PEI) and polyamide (PA) were sequentially added into a high-speed kneader and mixed at high speed for 20 min, melt-blended at 250 °C, extruded through an extruder, cooled and granulated to obtain an antibacterial masterbatch;

[0089] 4) The screw temperature of the screw extrusion spinning machine is set to 300° C., the antibacterial masterbatch is placed in the screw extrusion spinning machine and passed through a spinneret assembly to obtain a lanthanum-containing rare earth functional antibacterial fiber.

[0090] Comparative application example 1

[0091] The difference between the comparative application example 1 and the above application examples is that the high molecular polymer does not include polyurethane (PU).

[0092] Comparative Example 2

[0093] The difference between the comparative application example 2 and the above application examples is that the high molecular polymer does not contain polyethylene diamine (PEI).

[0094] Comparative Application Example 3

[0095] The difference between the comparative application example 3 and the above application examples is that the particle size distribution of the lanthanum-containing rare earth functional antibacterial additive is between 300 and 400 nm.

[0096] Application Examples and Comparative Examples The yarns spun in Application Examples 1-3 are compared with Figure 6 As shown, from Figure 6 It can be seen that when the particle size of the rare earth functional antibacterial additive of lanthanum is about 300nm, and polyurethane (PU) and polyethylene diamine (PEI) are added together during the weaving process, the yarn is smooth and has a delicate surface. When only one of polyurethane (PU) and polyethylene diamine (PEI) is added, the surface of the yarn is rough and uneven. When the particle size of the rare earth functional antibacterial additive is larger (300 ~ 400 nm), the surface of the yarn is uneven and has more thorns, which cannot be used in practice.

[0097] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A lanthanum-containing rare earth functional antibacterial additive, characterized in that: The lanthanum-containing rare earth functional antibacterial additive is prepared from a rare earth functional material, a first high molecular polymer and a solvent in a mass ratio of (1 to 2): (3 to 6): (12 to 16), wherein the rare earth functional material comprises a rare earth carbonate compound and / or a rare earth nitrate compound; the first high molecular polymer comprises one or more of polyamide, polyurethane, polyvinyl chloride, polyethylene terephthalate, polyethylene, polyvinyl alcohol and polyethylenediamine; The rare earth functional material comprises lanthanum carbonate hexahydrate, cerium carbonate hexahydrate, and samarium nitrate hexahydrate in a mass ratio of (1-4): (2-6): (6-24); The mass ratio of the rare earth functional material, the first high molecular polymer and the solvent is 1:4:15; The preparation method of the lanthanum-containing rare earth functional antibacterial additive comprises the following steps: After the rare earth functional material and the solvent are mixed, the first high molecular polymer is added, and the temperature is raised to 90-95°C while stirring. After reacting for 2-3 hours, a mixed solution is obtained. The temperature of the obtained mixed solution is raised to 180-200°C, and the mixture is reacted overnight for more than 12 hours. The reacted solution is taken out, cooled to room temperature, and centrifuged to remove the supernatant. The precipitate after centrifugation is collected to obtain a lanthanum-containing rare earth functional antibacterial additive.

2. The lanthanum-containing rare earth functional antibacterial additive according to claim 1, characterized in that: The solvent is water.

3. A lanthanum-containing rare earth functional antibacterial fiber, characterized in that: The lanthanum-containing rare earth functional antibacterial fiber is prepared from the following components in parts by weight: 5-10 parts of rare earth functional material slurry; 1-5 parts of silane coupling agent; 85-94 parts of the second high molecular weight polymer; The second high molecular polymer includes polyvinyl alcohol, polyethylene, polyurethane, polyethylenediamine and polyamide in a mass ratio of 1:1:1:1:1; The preparation method of the rare earth functional material slurry is: take the lanthanum-containing rare earth functional antibacterial additive according to claim 1 or 2, add water and an aqueous dispersant, stir evenly, and then sand grind it to make its particle size distribution between 200 and 300 nm.

4. The lanthanum-containing rare earth functional antibacterial fiber according to claim 3, characterized in that: The content of the lanthanum-containing rare earth functional antibacterial additive in the rare earth functional material slurry is 30-175 g of the lanthanum-containing rare earth functional antibacterial additive per liter of water.

5. The method for preparing the lanthanum-containing rare earth functional antibacterial fiber according to claim 3 comprises the following steps: S1: Mix the rare earth functional material slurry and the silane coupling agent described in claim 3 and add them into a high-speed kneader for high-speed mixing for 8 to 10 minutes; S2: The dried second polymer is sequentially added into a high-speed kneader and mixed for 15 to 20 minutes, melt-blended at 200 to 250°C, extruded through an extruder, cooled and granulated to obtain an antibacterial masterbatch; S3: The screw temperature of the screw extrusion spinning machine is set to 280-300° C., the antibacterial masterbatch is placed in the screw extrusion spinning machine and passed through a spinneret assembly to obtain a lanthanum-containing rare earth functional antibacterial fiber.