Hydrogen-sensitive color-changing material and preparation method, hydrogen-sensitive color-changing coating and application and system thereof

By using photochemical deposition method in hydrogen discoloration sensor to grow metal catalysts on the surface of WO3 nanoparticles, the high cost and complex process of precious metal catalysts are solved, and high sensitivity hydrogen detection and rapid color recovery are achieved, which is suitable for low-concentration hydrogen environments.

CN118687769BActive Publication Date: 2024-11-22NANJING TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411163609.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-22
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Existing hydrogen discoloration sensors require precious metal catalysts. The preparation process is complex and costly, with low sensitivity and low contrast, making it difficult to quickly detect hydrogen leakage in a low-concentration hydrogen environment.

Method used

By dropping inorganic acid into a salt solution containing tungsten ions, forming a precursor solution, hydrothermal treatment and inert gas annealing, WO3 nanoparticles are formed, and a metal catalyst is grown on its surface by photochemical deposition method to form a high-sensitivity hydrogen-sensitive discoloration with a high sensitivity Material.

Benefits of technology

It realizes rapid positioning and response in a low-concentration and low-flow hydrogen environment, and quickly restores color after detection of hydrogen, reducing material costs and process complexity and improving sensitivity to hydrogen.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118687769B_ABST
    Figure CN118687769B_ABST
Patent Text Reader

Abstract

The present invention discloses a hydrogen-sensitive color-changing material and a preparation method, a hydrogen-sensitive color-changing coating and its application and system, and relates to the technical field of hydrogen-sensitive materials, wherein the preparation method comprises the following steps: dropping an inorganic acid into a salt solution containing tungsten ions to obtain a precursor solution; adding an acidulant, a capping agent, and a stabilizer to the precursor solution in sequence to obtain a mixed solution; subjecting the mixed solution to a hydrothermal treatment to generate a hydrothermal reaction to obtain WO3; subjecting WO3 to an annealing treatment under an inert gas atmosphere to obtain WO3 nanoparticles; and using a photochemical deposition method to in-situ grow a metal catalyst on the surface of the WO3 nanoparticles to obtain the hydrogen-sensitive color-changing material. The present invention solves the problems of complex process and high cost of catalyst doping in hydrogen-sensitive color-changing materials, and improves the sensitivity of hydrogen-sensitive color-changing materials to hydrogen.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen-sensitive materials, and in particular to a hydrogen-sensitive color-changing material and a preparation method thereof, a hydrogen-sensitive color-changing coating and an application and system thereof. Background Art

[0002] As a new energy source that can replace oil, hydrogen plays an important strategic role in the national energy level. In recent years, hydrogen has been widely used in the fields of synthetic methanol, petroleum refining, metal smelting, aerospace fuel, etc. However, due to the special physical and chemical properties of hydrogen itself, once it leaks, it is difficult to detect. From a safety perspective, more accurate, convenient and highly sensitive means are needed to detect its presence.

[0003] There are many types of hydrogen sensors. According to the different ways of displaying the test results, they can be roughly divided into two categories: electronic sensors and gas-induced chromic sensors. Electronic sensors often need to operate at higher temperatures to operate normally. From the perspective of intrinsic safety, it is easy to generate electric sparks when operating at high temperatures, so there are certain potential risks. The color-changing sensor can detect hydrogen at room temperature, which meets the intrinsic safety requirements, and can detect hydrogen leaks through visual methods. However, gas-induced chromic sensors often need to be doped with precious metal catalysts, so their preparation cost is expensive. In addition, the preparation process is also relatively complicated, the color change and bleaching recovery time is long, the sensitivity is not high, and the contrast is low. Summary of the invention

[0004] The main purpose of the present invention is to propose a hydrogen-sensitive color-changing material and a preparation method, a hydrogen-sensitive color-changing coating and its application and system, aiming to solve the problems of complex process and high cost of catalyst doping in hydrogen-sensitive color-changing materials and to improve the sensitivity of hydrogen-sensitive color-changing materials to hydrogen.

[0005] To achieve the above object, in a first aspect, the present invention provides a method for preparing a hydrogen-sensitive color-changing material, comprising the following steps:

[0006] dropping an inorganic acid into a salt solution containing tungsten ions to obtain a precursor solution;

[0007] Adding an acidulant, a capping agent, and a stabilizer to the precursor solution in sequence to obtain a mixed solution;

[0008] The mixed solution is subjected to a hydrothermal treatment to generate a hydrothermal reaction to obtain WO3;

[0009] WO3 is annealed in an inert gas atmosphere to obtain WO3 nanoparticles;

[0010] The metal catalyst is in-situ grown on the surface of the WO3 nanoparticles by using a photochemical deposition method to obtain the hydrogen-sensitive color-changing material.

[0011] In some embodiments, the step of dripping an inorganic acid into a salt solution containing tungsten ions to obtain a precursor solution comprises:

[0012] Add inorganic acid dropwise to the salt solution containing tungsten ions, adjust the pH of the salt solution to 0.8-1.2, and stir to obtain a precursor solution;

[0013] or,

[0014] Inorganic acid is added dropwise to the salt solution containing tungsten ions, the pH of the salt solution is adjusted to 1.5-2, and the solution is stirred to obtain a precursor solution.

[0015] In some embodiments, in the step of sequentially adding an acidulant, a capping agent, and a stabilizer to the precursor solution to obtain a mixed solution,

[0016] The acidulant comprises at least one of oxalic acid and phosphoric acid, and the molar ratio of the acidulant to tungsten ions is (1-1.5):1, and / or;

[0017] The end-capping agent includes at least one of ammonium chloride, ammonium acetate, ammonium tungstate, ammonium sulfate, ammonium dihydrogen phosphate, and ammonium carbonate, and the molar ratio of the end-capping agent to the acidulant is (0.3-0.5):1, and / or;

[0018] The stabilizer includes at least one of urea, ethylene glycol, and polyethylene glycol, and the molar ratio of the stabilizer to tungsten ions is (0.1-0.3):1, and / or; the annealing temperature is 200-900°C;

[0019] In the step of subjecting the mixed solution to hydrothermal treatment to generate a hydrothermal reaction to obtain WO3,

[0020] The temperature of the hydrothermal treatment is 120℃~180℃, and the time of the hydrothermal treatment is 7~10 h.

[0021] In some embodiments, the step of growing a metal catalyst in situ on the surface of the WO3 nanoparticles by photochemical deposition to obtain the hydrogen-sensitive color-changing material comprises:

[0022] Dispersing the solid metal salt in an organic solvent, ultrasonicating and stirring to obtain a dispersion;

[0023] Adding the WO3 nanoparticles and polyvinyl pyrrolidone into the dispersion to obtain a mixed solution;

[0024] The mixed solution is irradiated with ultraviolet light to cause a reduction reaction, so that the metal is reduced and then grows in situ on the surface of the WO3 nanoparticles to obtain the hydrogen-sensitive color-changing material.

[0025] Wherein, the organic solvent comprises at least one of methanol, ethanol, isopropanol, and / or;

[0026] The solid metal salt includes at least one of PdCl2, H2PtCl6·6H2O, PdC12·6H2O, HAuCl4·4H2O, AgClO4·H2O, and / or;

[0027] The mass ratio of the solid metal salt, the WO3 nanoparticles and the polyvinyl pyrrolidone is 1:100:(6-10), and / or;

[0028] The reduction reaction time is 10 to 30 minutes.

[0029] In a second aspect, the present invention further provides a hydrogen-sensitive color-changing material prepared by the preparation method provided in the first aspect of the present application.

[0030] In a third aspect, the present invention further provides a method for testing the hydrogen-sensitive color-changing material provided in the second aspect of the present application, comprising:

[0031] The color-changing performance of hydrogen-sensitive color-changing materials was tested using an optical fiber spectrometer, wherein the test conditions included: under standard atmospheric pressure, a temperature of 0-100°C, a mixed gas flow rate of hydrogen and inert gas of 200-1000 ml / min, or, in a volume of 2-5 cm containing hydrogen, 3 In the confined space, the hydrogen concentrations were 0.1%, 1%, 4%, 10% and 100% respectively, and the test wavelength was 1000nm.

[0032] In a fourth aspect, the present invention further provides a hydrogen-sensitive color-changing coating, comprising the hydrogen-sensitive color-changing material provided in the second aspect of the present application, wherein the WO3 nanoparticles comprise three-dimensional nanoparticles composed of nanosheets or nanorods.

[0033] In some embodiments, the hydrogen-sensitive color-changing coating further includes resin, grease, solvent and additives.

[0034] In a fifth aspect, the present invention further proposes the application of the hydrogen-sensitive color-changing coating of the fourth aspect to monitor hydrogen leakage.

[0035] In a sixth aspect, the present invention further proposes a hydrogen leakage monitoring method, which is applied to the hydrogen-sensitive color-changing coating of the fourth aspect, and the hydrogen leakage monitoring method comprises:

[0036] Acquire a color change database of the hydrogen-sensitive color-changing coating, wherein the color change database includes a corresponding relationship between color change data of the hydrogen-sensitive color-changing coating and hydrogen leakage;

[0037] Acquiring real-time color data of a hydrogen-sensitive color-changing coating disposed on the surface of the object to be tested;

[0038] The real-time hydrogen leakage amount is determined according to the real-time color data and the corresponding relationship.

[0039] In the seventh aspect, the present invention also proposes a hydrogen leakage monitoring system, comprising a hydrogen-sensitive color-changing coating arranged on the surface of the object to be tested, a video acquisition unit for collecting color information of the hydrogen-sensitive color-changing coating, and a control unit, a data transmission unit, a data storage processing unit and an alarm unit electrically connected to the video acquisition unit.

[0040] The technical solution of the present invention is to drip an inorganic acid into a salt solution containing tungsten ions to obtain a precursor solution; and to sequentially add an acidulant, a capping agent, and a stabilizer to the precursor solution to regulate the morphology of tungsten trioxide generated by a hydrothermal reaction, so that the self-assembled tungsten trioxide three-dimensional hierarchical structure has a large specific surface area. The oxygen vacancies of tungsten trioxide are regulated by annealing in an inert atmosphere, which greatly improves the sensitivity to hydrogen. In addition, in view of the complex process and high cost of noble metal catalyst doping, the present invention uses a photochemical deposition method to grow a metal catalyst in situ on the surface of the WO3 nanoparticles, which is not only green and environmentally friendly, but also simple in process. The obtained palladium nanoparticles have a small particle size and uniform distribution, and the amount of reactants is also small. The hydrogen-sensitive color-changing coating provided by the present invention can achieve rapid positioning and response in a low-concentration, low-flow hydrogen environment, and can recover to the initial color faster after detecting hydrogen discoloration. Due to the insufficient time and scope coverage of manual inspections in traditional industrial parks, there are personal safety issues. The present invention combines materials with video surveillance image recognition algorithms to form a hydrogen leakage detection system, which uses cameras and algorithms to identify the discoloration of coatings when encountering hydrogen to perform real-time monitoring of hydrogen leakage. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0042] Figure 1 is the XRD pattern of WO3 nanoparticles prepared in Example 2;

[0043] Figure 2 is the XRD pattern of WO3 nanoparticles prepared in Example 1;

[0044] Figure 3 This is a SEM characterization image of the three-dimensional nanoflower structure formed by self-assembly of tungsten trioxide nanosheets in Example 1;

[0045] Figure 4 This is a SEM characterization image of the three-dimensional nanoflower structure formed by self-assembly of tungsten trioxide nanorods in Example 2;

[0046] Figure 5 A TEM image of the hydrogen-sensitive color-changing material after doping with palladium nanoparticles in step (10) in Example 1;

[0047] Figure 6 This is another TEM image of the hydrogen-sensitive color-changing material after doping with palladium nanoparticles in step (10) in Example 1.

[0048] Figure 7 This is an EDS spectrum data diagram of the hydrogen-sensitive color-changing material after doping with palladium nanoparticles in step (10) in Example 1;

[0049] Figure 8 The element distribution diagram of the hydrogen-sensitive color-changing material after doping with palladium nanoparticles in step (10) in Example 1;

[0050] Figures 9 to 12 The diagrams respectively show that after the hydrogen-sensitive color-changing paint is applied to the substrate, as the hydrogen conduit below it moves to the right, the position where the hydrogen passes changes color accordingly;

[0051] Fig.13 A flowchart of a hydrogen leakage monitoring system provided in an embodiment of the present application;

[0052] Fig.14 This is the XPS graph of WO3 nanoparticles prepared in Comparative Example 1;

[0053] Fig.15 This is the XPS graph of the WO3 nanoparticles prepared in Example 1;

[0054] Fig.16 is a BET characterization diagram of WO3 nanoparticles (nanorod self-assembly) prepared in Example 2;

[0055] Fig.17 is a BET characterization diagram of WO3 nanoparticles (nanosheet self-assembly) prepared in Example 1;

[0056] Fig.18 This is the BET characterization diagram of WO3 nanoparticles prepared in Comparative Example 2.

[0057] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0058] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0059] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0060] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features limited to "first" and "second" may explicitly or implicitly include at least one of the features. In addition, if "and / or" or "and / or" appears in the full text, its meaning includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0061] As a new energy source that can replace oil, hydrogen plays an important strategic role in the national energy level. In recent years, hydrogen has been widely used in the fields of synthetic methanol, petroleum refining, metal smelting, aerospace fuel, etc. However, due to the special physical and chemical properties of hydrogen itself, once it leaks, it is difficult to detect. From a safety perspective, more accurate, convenient and highly sensitive means are needed to detect its presence.

[0062] There are many types of hydrogen sensors. According to the different ways of displaying the test results, they can be roughly divided into two categories: electronic sensors and gas-induced chromic sensors. Electronic sensors often need to operate at higher temperatures to operate normally. From the perspective of intrinsic safety, it is easy to generate electric sparks when operating at high temperatures, so there are certain potential risks. The color-changing sensor can detect hydrogen at room temperature, which meets the intrinsic safety requirements, and can detect hydrogen leaks through visual methods. However, gas-induced chromic sensors often need to be doped with precious metal catalysts, so their preparation cost is expensive. In addition, the preparation process is also relatively complicated, the color change and bleaching recovery time is long, the sensitivity is not high, and the contrast is low.

[0063] In a first aspect, the present invention provides a method for preparing a hydrogen-sensitive color-changing material, comprising the following steps:

[0064] dropping an inorganic acid into a salt solution containing tungsten ions to obtain a precursor solution;

[0065] Adding an acidulant, a capping agent, and a stabilizer to the precursor solution in sequence to obtain a mixed solution;

[0066] The mixed solution is subjected to a hydrothermal treatment to generate a hydrothermal reaction to obtain WO3;

[0067] WO3 is annealed in an inert gas atmosphere to obtain WO3 nanoparticles;

[0068] The metal catalyst is in-situ grown on the surface of the WO3 nanoparticles by using a photochemical deposition method to obtain the hydrogen-sensitive color-changing material.

[0069] The technical solution of the present invention uses the steps of dripping an inorganic acid into a salt solution containing tungsten ions to obtain a precursor solution; and sequentially adding an acidulant, a capping agent, and a stabilizer into the precursor solution to regulate the morphology of tungsten trioxide generated by a hydrothermal reaction, so that the formed self-assembled tungsten trioxide three-dimensional hierarchical structure has a large specific surface area. The oxygen vacancies of tungsten trioxide are regulated by annealing in an inert atmosphere, which greatly improves the sensitivity to hydrogen.

[0070] In one embodiment of the present invention, the step of dripping an inorganic acid into a salt solution containing tungsten ions to obtain a precursor solution comprises: dripping an inorganic acid into a salt solution containing tungsten ions, adjusting the pH of the salt solution to 0.8-1.2, and stirring to obtain a precursor solution.

[0071] In another embodiment of the present invention, the step of dripping hydrochloric acid into a salt solution containing tungsten ions to obtain a precursor solution includes: dripping an inorganic acid into the salt solution containing tungsten ions, adjusting the pH of the salt solution to 1.5-2, and stirring to obtain a precursor solution.

[0072] It should be noted that in the embodiment of the present invention, by controlling the pH value of the salt solution containing tungsten ions, the morphology of the WO3 nanoparticles obtained in the subsequent steps can be regulated. Specifically, when an inorganic acid is dripped into the salt solution containing tungsten ions and the pH of the salt solution is adjusted to 0.8-1.2, WO3 nanoparticles formed by self-assembly of nanosheets are obtained. When an inorganic acid is dripped into the salt solution containing tungsten ions and the pH of the salt solution is adjusted to 1.5-2, WO3 nanoparticles formed by self-assembly of nanorods are obtained.

[0073] In an embodiment of the present invention, in the step of sequentially adding an acidulant, a capping agent, and a stabilizer to the precursor solution to obtain a mixed solution, the acidulant comprises at least one of oxalic acid and phosphoric acid, and the molar ratio of the acidulant to tungsten ions is (1-1.5):1, and / or;

[0074] The capping agent includes at least one of ammonium chloride, ammonium acetate, ammonium tungstate, ammonium sulfate, ammonium dihydrogen phosphate, and ammonium carbonate, and the molar ratio of the capping agent to the acidifier is (0.3-0.5):1, and / or; the stabilizer includes at least one of urea, ethylene glycol, and polyethylene glycol, and the molar ratio of the stabilizer to tungsten ions is (0.1-0.3):1.

[0075] It should be noted that in the embodiments of the present invention, the acidifiers such as oxalic acid and tungstic acid lose a water molecule in the water environment through hydrogen bonding and interlayer water. This process can slow down the nucleation rate and prevent the nucleus from continuing to grow. The slowing down of the nucleation rate is beneficial to the subsequent self-assembly process. The capping agent such as NH4Cl is beneficial to the formation of tungsten oxide nanorods. The capping agent contains NH 4+ , NH 4+ It can selectively adsorb on the crystal planes parallel to the c-axis of the tungsten oxide crystal nucleus. Then the growth of these crystal planes will be hindered, while the crystal planes perpendicular to the c-axis will grow faster, resulting in preferential growth along the c-axis. In addition, NH 4+ can be inserted into the hexagonal channels to stabilize the hexagonal structure. 4+ The addition of can promote the formation and stable growth of h-WO3 nuclei during the reaction process, thereby generating h-WO3. In addition, hydrogen bonds in the solution can induce the self-assembly of primary self-aggregates, while van der Waals forces are conducive to enhancing the stability of the formed superstructure (such as flower-like hierarchical structures). 4+ The h-WO3 nuclei tend to aggregate together. Low concentrations of stabilizers have a directional growth effect, while high concentrations of stabilizers have a joint growth effect. Under excessive stabilizer bonding, the nanowires will grow epitaxially and evolve into irregular nanosheets. And it will improve the stability of the material at high temperatures.

[0076] Therefore, under the synergistic effect of the above-mentioned acidifier, capping agent and stabilizer, it is beneficial to stack multi-level and multi-layer nanosheets or nanorods together, thereby facilitating the hierarchical self-assembly of tungsten trioxide, that is, forming a three-dimensional hierarchical structure of self-assembled tungsten trioxide.

[0077] In an embodiment of the present invention, in the step of subjecting the mixed solution to hydrothermal treatment to generate a hydrothermal reaction to obtain WO3, the hydrothermal treatment temperature is 120°C to 180°C and the hydrothermal treatment time is 7 to 10 h.

[0078] In an embodiment of the present invention, WO3 is annealed in an inert gas atmosphere to obtain WO3 nanoparticles, and the annealing temperature is 200-900°C; for WO3 nanoparticles formed by self-assembly of nanorods, they are hexagonal, and when the annealing temperature reaches above 400 degrees Celsius, the hexagonal WO3 will be transformed into monoclinic WO3, therefore, the optimal annealing temperature for the hexagonal WO3 is 300-400 degrees Celsius, and for WO3 nanoparticles formed by self-assembly of nanosheets, they are monoclinic, and the optimal annealing temperature is 400-600 degrees Celsius.

[0079] In an embodiment of the present invention, the step of growing a metal catalyst in situ on the surface of the WO3 nanoparticles by photochemical deposition to obtain the hydrogen-sensitive color-changing material comprises:

[0080] Dispersing the solid metal salt in an organic solvent, ultrasonicating and stirring to obtain a dispersion;

[0081] Adding the WO3 nanoparticles and polyvinyl pyrrolidone into the dispersion to obtain a mixed solution;

[0082] The mixed solution is irradiated with ultraviolet light to cause a reduction reaction, so that the metal is reduced and then grows in situ on the surface of the WO3 nanoparticles to obtain the hydrogen-sensitive color-changing material.

[0083] In order to solve the problems of complex process and high cost of doping precious metal catalysts, the present invention uses photochemical deposition to grow metal catalysts in situ on the surface of the WO3 nanoparticles. This is not only green and environmentally friendly, but also simple in process. The obtained palladium nanoparticles have small particle size and uniform distribution, and the amount of reactants used is also small.

[0084] In an embodiment of the present invention, the organic solvent comprises at least one of methanol and ethanol.

[0085] The solid metal salt includes at least one of PdCl2, H2PtCl6·6H2O, PdC12·6H2O, HAuCl4·4H2O, AgClO4·H2O, and / or;

[0086] The mass ratio of the solid metal salt, the WO3 nanoparticles and the polyvinyl pyrrolidone is 1:100:(6-10), and / or;

[0087] The reduction reaction time is 10 to 30 minutes.

[0088] In a second aspect, the present invention further provides a hydrogen-sensitive color-changing material prepared by the preparation method provided in the first aspect of the present application.

[0089] In a third aspect, the present invention further provides a method for testing the hydrogen-sensitive color-changing material provided in the second aspect of the present application, comprising:

[0090] The color-changing performance of hydrogen-sensitive color-changing materials was tested using an optical fiber spectrometer, wherein the test conditions included: under standard atmospheric pressure, a temperature of 0-100°C, a mixed gas flow rate of hydrogen and inert gas of 200-1000 ml / min, or, in a volume of 2-5 cm containing hydrogen, 3 In the confined space, the hydrogen concentrations were 0.1%, 1%, 4%, 10% and 100% respectively, and the test wavelength was 1000nm.

[0091] It should be noted that, in the embodiment of the present invention, the hydrogen-sensitive color change performance test system used includes a mass flow controller (MFC), a test chamber, a spectrometer, a light source and a computer. The mass flow controller controls the concentration, time and flow rate of the target gas (hydrogen) and the carrier gas (nitrogen, argon and other inert gases) mixed / unmixed according to the test conditions. In order to perform hydrogen-sensitive sensing measurements, the prepared hydrogen-sensitive color-changing material (sensor) is placed in the test chamber, and then the target gas flow is injected under the required time, temperature and other test conditions. A fiber optic spectrometer (HR-2XR300-25 - operated by "OceanView" software) is used to measure the color change of the sample before and after gas exposure.

[0092] The inventors found that the test conditions are: under standard atmospheric pressure, room temperature (e.g., 0-35°C), a mixed gas flow rate of hydrogen and inert gas of 200 ml / min, or, in a volume of 2 cm containing hydrogen, 3 In the confined space, the hydrogen concentrations were 0.1%, 1%, 4%, 10%, and 100%, respectively, and the test wavelength was 1000nm. This test condition is the best test condition and can better test the color-changing performance of hydrogen-sensitive color-changing materials.

[0093] In a fourth aspect, the present invention further provides a hydrogen-sensitive color-changing coating, comprising the hydrogen-sensitive color-changing material provided in the second aspect of the present application, wherein the WO3 nanoparticles comprise three-dimensional nanoparticles composed of nanosheets or nanorods.

[0094] In some embodiments, the hydrogen-sensitive color-changing coating further includes resin, grease, solvent and additives.

[0095] In a fifth aspect, the present invention further proposes the application of the hydrogen-sensitive color-changing coating of the fourth aspect for monitoring hydrogen leakage. The hydrogen-sensitive color-changing coating provided by the present invention can achieve rapid positioning and response in a low-concentration, low-flow hydrogen environment, and can restore to the initial color more quickly after detecting hydrogen color change.

[0096] In a sixth aspect, the present invention further proposes a hydrogen leakage monitoring method, which is applied to the hydrogen-sensitive color-changing coating of the fourth aspect, and the hydrogen leakage monitoring method comprises:

[0097] Acquire a color change database of the hydrogen-sensitive color-changing coating, wherein the color change database includes a corresponding relationship between color change data of the hydrogen-sensitive color-changing coating and hydrogen leakage;

[0098] Acquiring real-time color data of a hydrogen-sensitive color-changing coating disposed on the surface of the object to be tested;

[0099] The real-time hydrogen leakage amount is determined according to the real-time color data and the corresponding relationship.

[0100] Since there is a problem with the current hydrogen-sensitive materials, the more the amount of initial hydrogen-sensitive active material in the hydrogen-sensitive color-changing coating, the faster the response time, the higher the sensitivity, and the better other properties. However, the more the amount of initial hydrogen-sensitive active material, the darker the initial color of the material, and the smaller the color difference after the color change after encountering hydrogen, which may not be easily observed by the naked eye. Therefore, the hydrogen leakage monitoring method provided in the present invention obtains the color change database of the hydrogen-sensitive color-changing coating and obtains the real-time color data of the hydrogen-sensitive color-changing coating set on the surface of the object to be tested; determines the real-time hydrogen leakage amount according to the real-time color data and the corresponding relationship, and can identify color changes that cannot be observed by the naked eye, so that the millisecond-level hydrogen leakage detection color change response will be achieved.

[0101] Among them, the acquisition of real-time color data can be achieved by using surveillance cameras, and the color change database of hydrogen-sensitive color-changing paint can be obtained through a large amount of data collected by a laboratory fiber optic spectrometer. A database including the correspondence between the color change data of hydrogen-sensitive color-changing paint and the amount of hydrogen leakage is established. In actual application scenarios, the color recognized by the surveillance camera will be compared with the established standard database to infer the amount of leakage.

[0102] In the seventh aspect, the present invention also proposes a hydrogen leakage monitoring system, comprising a hydrogen-sensitive color-changing coating arranged on the surface of the object to be tested, a video acquisition unit for collecting color information of the hydrogen-sensitive color-changing coating, and a control unit, a data transmission unit, a data storage processing unit and an alarm unit electrically connected to the video acquisition unit.

[0103] The time and coverage of manual inspections in traditional industrial parks are insufficient, and there are personal safety issues. In addition, the hydrogen-sensitive material in this type of hydrogen-sensitive color-changing coating has a very fast recovery time, and its highly reversible properties make it impossible for the material itself to continuously record or store information.

[0104] In view of this, the present invention combines hydrogen-sensitive color-changing paint with a video surveillance image recognition algorithm to form a hydrogen leak detection system, which uses a camera and an algorithm to identify the color change of the paint when it encounters hydrogen, so as to perform real-time monitoring of hydrogen leaks. This solves the problem that the reversible color-changing material itself cannot record or store information. Among them, the image recognition algorithm in the embodiment of the present invention can be a conventional algorithm in the prior art, as long as it can realize the function of identifying the color change of the paint when it encounters hydrogen.

[0105] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0106] Example 1

[0107] This embodiment provides a method for preparing a hydrogen-sensitive color-changing material and a hydrogen-sensitive color-changing material prepared by the preparation method. The preparation method comprises:

[0108] WO3 nanoparticles preparation:

[0109] (1) Dissolve 5 mmol of sodium tungstate in 50 mL of deionized water and stir continuously for 20 min to obtain a transparent mixed solution A.

[0110] (2) Add 5 mL of 6 mol / L HCl dropwise into the above solution, adjust the pH to 1.0, and stir for 30 min to obtain a light yellow mixed solution.

[0111] (3) 0.54 g of oxalic acid, 1.07 g of ammonium chloride and 0.2 g of urea were added to the above light yellow mixed solution in sequence to obtain mixed solution B, and the mixture was magnetically stirred for 2 h.

[0112] (4) The mixed solution B was placed in a Teflon liner, sealed in a stainless steel autoclave, and hydrothermally treated at 170 °C for 10 h.

[0113] (5) The mixture after the hydrothermal treatment was cooled to room temperature, washed with deionized water and anhydrous ethanol three times respectively, and then dried in an oven at 50°C overnight.

[0114] (6) The obtained powder was annealed in a nitrogen atmosphere. The annealing process was as follows: the heating rate was 5°C / min, the temperature was heated to 600°C and the holding time was 2h, and the cooling rate was 2°C / min. WO3 nanoparticles formed by self-assembly of WO3 nanosheets were obtained.

[0115] Photochemical deposition method doped with palladium noble metal catalyst:

[0116] (7) Disperse 0.25 mM PdC12 in methanol, ultrasonicate for 2 h, and vigorously stir for 1 h to obtain a dispersion.

[0117] (8) Add 200 mg of the synthesized WO3 nanoparticles, 10 ml of the palladium precursor solution and 5 mg of PVP to 40 ml of methanol, and then add the dispersion obtained in step (7) to obtain a deposition solution.

[0118] (9) The deposition solution was exposed to UV light and stirred vigorously for 30 min to deposit palladium on the WO3 nanoparticles.

[0119] (10) The solution was centrifuged, washed with methanol three times, and finally dried in an oven at 50°C overnight to obtain a hydrogen-sensitive color-changing material.

[0120] Example 2

[0121] This embodiment provides a method for preparing a hydrogen-sensitive color-changing material and a hydrogen-sensitive color-changing material prepared by the preparation method. The preparation method comprises:

[0122] WO3 nanoparticles preparation:

[0123] (1) Dissolve 5 mmol of sodium tungstate in 50 mL of deionized water and stir continuously for 20 min to obtain a transparent mixed solution A.

[0124] (2) Add 5 mL of 6 mol / L HCl dropwise into the above solution, adjust the pH to 1.5, and stir for 30 min to obtain a light yellow mixed solution.

[0125] (3) 0.54 g of oxalic acid, 1.07 g of ammonium chloride and 0.2 g of urea were added to the above light yellow mixed solution in sequence to obtain mixed solution B, and the mixture was magnetically stirred for 2 h.

[0126] (4) The mixed solution B was placed in a Teflon liner, sealed in a stainless steel autoclave, and hydrothermally treated at 170 °C for 10 h.

[0127] (5) The mixture after the hydrothermal treatment was cooled to room temperature, washed with deionized water and anhydrous ethanol three times respectively, and then dried in an oven at 50°C overnight.

[0128] (6) The obtained powder was annealed in a nitrogen atmosphere. The annealing process was as follows: the heating rate was 5°C / min, the temperature was kept at 300°C for 2 h, and the cooling rate was 2°C / min. WO3 nanoparticles formed by self-assembly of WO3 nanorods were obtained.

[0129] Photochemical deposition method doped with palladium noble metal catalyst:

[0130] (7) Disperse 0.25 mM PdC12 in methanol, ultrasonicate for 2 h, and vigorously stir for 1 h to obtain a dispersion.

[0131] (8) Add 200 mg of the synthesized WO3 nanoparticles, 10 ml of the palladium precursor solution and 5 mg of PVP to 40 ml of methanol, and then add the dispersion obtained in step (7) to obtain a deposition solution.

[0132] (9) The deposition solution was exposed to UV light and stirred vigorously for 30 min to deposit palladium on the WO3 nanoparticles.

[0133] (10) The solution was centrifuged, washed with methanol three times, and finally dried in an oven at 50°C overnight to obtain a hydrogen-sensitive color-changing material.

[0134] Example 3

[0135] This embodiment provides a method for preparing a hydrogen-sensitive color-changing material and a hydrogen-sensitive color-changing material prepared by the preparation method. The preparation method comprises:

[0136] WO3 nanoparticles preparation:

[0137] (1) Dissolve 5 mmol of sodium tungstate in 50 mL of deionized water and stir continuously for 20 min to obtain a transparent mixed solution A.

[0138] (2) Add 5 mL of 3 mol / L HCl dropwise into the above solution, adjust the pH to 0.8, and stir for 30 min to obtain a light yellow mixed solution.

[0139] (3) 0.4 g of oxalic acid, 0.9 g of ammonium chloride and 0.1 g of urea were added to the above light yellow mixed solution in sequence to obtain mixed solution B, and the mixture was stirred magnetically for 2 h.

[0140] (4) The mixed solution B was placed in a Teflon liner, sealed in a stainless steel autoclave, and hydrothermally treated at 160 °C for 12 h.

[0141] (5) The mixture after the hydrothermal treatment was cooled to room temperature, washed with deionized water and anhydrous ethanol three times respectively, and then dried in an oven at 50°C overnight.

[0142] (6) The obtained powder was annealed in an argon atmosphere. The annealing process was specifically as follows: the heating rate was 5°C / min, the temperature was raised to 600°C and the holding time was 2h, and the cooling rate was 2°C / min. WO3 nanoparticles formed by self-assembly of WO3 nanosheets were obtained.

[0143] Photochemical deposition method doped with palladium noble metal catalyst:

[0144] (7) Disperse 0.25 mM PdC12 in methanol, ultrasonicate for 2 h, and vigorously stir for 1 h to obtain a dispersion.

[0145] (8) Add 200 mg of the synthesized WO3 nanoparticles, 10 ml of the palladium precursor solution and 5 mg of PVP to 40 ml of methanol, and then add the dispersion obtained in step (7) to obtain a deposition solution.

[0146] (9) The deposition solution was exposed to UV light and stirred vigorously for 30 min to deposit palladium on the WO3 nanoparticles.

[0147] (10) The solution was centrifuged, washed with methanol three times, and finally dried in an oven at 50°C overnight to obtain a hydrogen-sensitive color-changing material.

[0148] Example 4

[0149] This embodiment provides a method for preparing a hydrogen-sensitive color-changing material and a hydrogen-sensitive color-changing material prepared by the preparation method. The preparation method comprises:

[0150] WO3 nanoparticles preparation:

[0151] (1) Dissolve 5 mmol of sodium tungstate in 50 mL of deionized water and stir continuously for 20 min to obtain a transparent mixed solution A.

[0152] (2) Add 5 mL of 3 mol / L HCl dropwise into the above solution, adjust the pH to 2, and stir for 30 min to obtain a light yellow mixed solution.

[0153] (3) Add 0.5 g of oxalic acid, 1.1 g of ammonium chloride and 0.3 g of urea to the above light yellow mixed solution in sequence to obtain mixed solution B, and stir magnetically for 2 h.

[0154] (4) The mixed solution B was placed in a Teflon liner, sealed in a stainless steel autoclave, and hydrothermally treated at 180 °C for 8 h.

[0155] (5) The mixture after the hydrothermal treatment was cooled to room temperature, washed with deionized water and anhydrous ethanol three times respectively, and then dried in an oven at 50°C overnight.

[0156] (6) The obtained powder was annealed in an argon atmosphere. The annealing process was specifically as follows: the heating rate was 5°C / min, the temperature was raised to 300°C and the holding time was 2h, and the cooling rate was 2°C / min. WO3 nanoparticles formed by self-assembly of WO3 nanorods were obtained.

[0157] Photochemical deposition method doped with palladium noble metal catalyst:

[0158] (7) Disperse 0.25 mM PdC12 in methanol, ultrasonicate for 2 h, and vigorously stir for 1 h to obtain a dispersion.

[0159] (8) Add 200 mg of the synthesized WO3 nanoparticles, 10 ml of the palladium precursor solution and 5 mg of PVP to 40 ml of methanol, and then add the dispersion obtained in step (7) to obtain a deposition solution.

[0160] (9) The deposition solution was exposed to UV light and stirred vigorously for 30 min to deposit palladium on the WO3 nanoparticles.

[0161] (10) The solution was centrifuged, washed with methanol three times, and finally dried in an oven at 80°C overnight to obtain a hydrogen-sensitive color-changing material.

[0162] Example 5

[0163] 10 mg of the hydrogen-sensitive color-changing material prepared in Example 1 was mixed with 400 mg of acrylic resin, 100 mg of varnish, 400 mg of acetone and 90 mg of PDMS. The thickness was controlled by adjusting the height of the scraper using a coating machine. A film with a thickness of 2 μm was coated using the coating machine. The film was the hydrogen-sensitive color-changing coating.

[0164] Example 6

[0165] 10 mg of the hydrogen-sensitive color-changing material prepared in Example 2 was mixed with 400 mg of acrylic resin, 100 mg of varnish, 400 mg of acetone and 90 mg of PDMS. The thickness was controlled by adjusting the spin coating time and rotation speed using a spin coater. The rotation speed was 3500 rpm and the spin coating time was 1.5 minutes to obtain a hydrogen-sensitive color-changing coating film.

[0166] Example 7

[0167] This embodiment provides a method for testing the hydrogen-sensitive color-changing material of Embodiment 1. In this embodiment, a hydrogen-sensitive color-changing performance testing system includes a mass flow controller (MFC), a test chamber, a spectrometer, a light source and a computer.

[0168] include:

[0169] The color-changing performance of hydrogen-sensitive color-changing materials was tested using a fiber optic spectrometer (HR-2XR300-25 - operated by "OceanView" software). The test conditions included: the test conditions were: under standard atmospheric pressure, the temperature was room temperature (25°C), the flow rate of the mixed gas of hydrogen and inert gas was 200ml / min, the hydrogen concentrations were 0.1%, 1%, 4%, 10%, 100%, respectively, and the test wavelength was 1000nm.

[0170] Example 8

[0171] This embodiment provides a method for testing the hydrogen-sensitive color-changing material of Embodiment 1. In this embodiment, a hydrogen-sensitive color-changing performance testing system includes a mass flow controller (MFC), a test chamber, a spectrometer, a light source and a computer.

[0172] include:

[0173] The color change performance of hydrogen-sensitive color-changing materials was tested using a fiber optic spectrometer (HR-2XR300-25 - operated by "OceanView" software). The test conditions included: under standard atmospheric pressure, room temperature (25°C), and a volume of 2cm containing hydrogen. 3 In the confined space, the hydrogen concentrations were 0.1%, 1%, 4%, 10% and 100% respectively, and the test wavelength was 1000nm.

[0174] Example 9

[0175] This embodiment provides a hydrogen leakage monitoring method, which is applied to the hydrogen-sensitive color-changing coating of embodiment 1, and comprises:

[0176] Acquire a color change database of the hydrogen-sensitive color-changing coating, wherein the color change database includes a corresponding relationship between color change data of the hydrogen-sensitive color-changing coating and hydrogen leakage;

[0177] Acquiring real-time color data of a hydrogen-sensitive color-changing coating disposed on the surface of the object to be tested;

[0178] The real-time hydrogen leakage amount is determined according to the real-time color data and the corresponding relationship.

[0179] Example 10

[0180] This embodiment provides a hydrogen leakage monitoring system, comprising a hydrogen-sensitive color-changing coating prepared by Example 4 and disposed on the surface of a test object, a video acquisition unit for collecting color information of the hydrogen-sensitive color-changing coating, and a control unit, a data transmission unit, a data storage processing unit and an alarm unit electrically connected to the video acquisition unit. The working principle thereof can be found in Fig.13 .

[0181] Comparative Example 1

[0182] The difference between this comparative example and Example 1 is that step (6) is not provided and annealing treatment is not performed. The preparation method specifically comprises:

[0183] WO3 nanoparticles preparation:

[0184] (1) Dissolve 5 mmol of sodium tungstate in 50 mL of deionized water and stir continuously for 20 min to obtain a transparent mixed solution A.

[0185] (2) Add 5 mL of 6 mol / L HCl dropwise into the above solution, adjust the pH to 1.5, and stir for 30 min to obtain a light yellow mixed solution.

[0186] (3) 0.54 g of oxalic acid, 1.07 g of ammonium chloride and 0.2 g of urea were added to the above light yellow mixed solution in sequence to obtain mixed solution B, and magnetically stirred for 2 h.

[0187] (4) The mixed solution B was placed in a Teflon liner, sealed in a stainless steel autoclave, and hydrothermally treated at 170 °C for 10 h.

[0188] (5) The mixed solution after the hydrothermal treatment was cooled to room temperature, washed with deionized water and anhydrous ethanol for three times respectively, and then dried in an oven at 50°C overnight to obtain WO3 nanoparticles formed by self-assembly of WO3 nanosheets.

[0189] Photochemical deposition method doped with palladium noble metal catalyst:

[0190] (6) Disperse 0.25 mM PdC12 in methanol, ultrasonicate for 2 h, and vigorously stir for 1 h to obtain a dispersion.

[0191] (7) Add 200 mg of the synthesized WO3 nanoparticles, 10 ml of the palladium precursor solution and 5 mg of PVP to 40 ml of methanol, and then add the dispersion obtained in step (7) to obtain a deposition solution.

[0192] (8) The deposition solution was exposed to UV light and stirred vigorously for 30 min to deposit palladium on the WO3 nanoparticles.

[0193] (9) The solution was centrifuged, washed with methanol three times, and finally dried in an oven at 50°C overnight to obtain a hydrogen-sensitive color-changing material.

[0194] Comparative Example 2

[0195] The difference between this comparative example and Example 1 is that step (3) is not provided, and oxalic acid, ammonium chloride and urea are not added. The preparation method specifically comprises:

[0196] WO3 nanoparticles preparation:

[0197] (1) Dissolve 5 mmol of sodium tungstate in 50 mL of deionized water and stir continuously for 20 min to obtain a transparent mixed solution A.

[0198] (2) Add 5 mL of 6 mol / L HCl dropwise into the above solution, adjust the pH to 1.0, and stir for 30 min to obtain a light yellow mixed solution.

[0199] (3) The light yellow mixed solution was placed in a Teflon liner, sealed in a stainless steel autoclave, and hydrothermally treated at 170 °C for 10 h.

[0200] (4) The mixture after the hydrothermal treatment was cooled to room temperature, washed with deionized water and anhydrous ethanol three times respectively, and then dried in an oven at 50°C overnight.

[0201] (5) The obtained powder was annealed in a nitrogen atmosphere. The annealing process was as follows: the heating rate was 5°C / min, the temperature was raised to 600°C and the holding time was 2h, and the cooling rate was 2°C / min. WO3 nanoparticles were obtained.

[0202] Photochemical deposition method doped with palladium noble metal catalyst:

[0203] (6) Disperse 0.25 mM PdC12 in methanol, ultrasonicate for 2 h, and vigorously stir for 1 h to obtain a dispersion.

[0204] (7) Add 200 mg of the synthesized WO3 nanoparticles, 10 ml of the palladium precursor solution and 5 mg of PVP to 40 ml of methanol, and then add the dispersion obtained in step (7) to obtain a deposition solution.

[0205] (8) The deposition solution was exposed to UV light and stirred vigorously for 30 min to deposit palladium on the WO3 nanoparticles.

[0206] (9) The solution was centrifuged, washed with methanol three times, and finally dried in an oven at 50°C overnight to obtain a hydrogen-sensitive color-changing material.

[0207] Performance Testing

[0208] (1) XRD test was performed on the WO3 nanoparticles prepared in Example 1 and Example 2. The results are shown in Figure 1 and Figure 2 .

[0209] Figure 1 The hexagonal tungsten trioxide (nanorods) obtained in Example 2, Figure 2 The product obtained in Example 1 is monoclinic tungsten trioxide (nanosheet).

[0210] (2) Figure 3 This is a SEM characterization image of the three-dimensional nanoflower structure formed by self-assembly of tungsten trioxide nanosheets in Example 1. Figure 4 This is a SEM characterization image of the three-dimensional nanoflower structure formed by self-assembly of tungsten trioxide nanorods in Example 2.

[0211] (3) Figure 5 , 6 They are TEM images of the hydrogen-sensitive color-changing material after doping with palladium nanoparticles in step (10) in Example 1, Figure 5 The lattice spacing of WO3 was measured, and the hydrogen-sensitive color change Figure 6 The lattice spacing of Pd was measured in . Figure 7 , 8 They are respectively the EDS spectrum data diagram and element distribution diagram of the hydrogen-sensitive color-changing material after doping with palladium nanoparticles in step (10) in Example 1, which show the mass percentage and atomic percentage of the three elements in the material.

[0212] (4) Fig.14 This is the XPS graph of the WO3 nanoparticles prepared in Comparative Example 1. Fig.15 This is the XPS graph of the WO3 nanoparticles prepared in Example 1, where green OL is lattice oxygen, blue Ov is vacancy oxygen, and red Oa is adsorbed oxygen. It can be seen that both vacancy oxygen and adsorbed oxygen after the reaction have increased to a certain extent, indicating that the amount of defective oxygen has increased after annealing. Oxygen defects are generally believed to introduce a low energy level in the conduction band, making electron transitions easier. This accelerates electron transmission, thereby improving the reaction kinetics.

[0213] (5) Fig.16 is the BET characterization diagram of WO3 nanoparticles (nanorod self-assembly) prepared in Example 2, Fig.17 This is the BET characterization diagram of the WO3 nanoparticles (self-assembled nanosheets) prepared in Example 1. It can be seen that the dandelion-shaped WO3 nanoflowers self-assembled from hexagonal nanorods have a larger specific surface area of ​​65.3080 m 2 / g.

[0214] (6) Fig.18 This is the BET characterization diagram of WO3 nanoparticles prepared in Comparative Example 2. It can be seen that Fig.16 , Fig.17 and Fig.18By comparison, the BET of the WO3 nanoparticles prepared by adding an acidifier, a capping agent, and a stabilizer in Examples 1 and 2 is larger. In fact, the WO3 nanoparticles prepared in Comparative Example 2 do not have the morphology of nanoflowers. The WO3 nanoparticles prepared in Comparative Example 2 are just stacked nanosheets, so the specific surface area is smaller.

[0215] (7) The hydrogen-sensitive color-changing paint is placed on a substrate, and a hydrogen conduit is placed below the substrate. As the hydrogen conduit below the substrate moves to the right, the color change of the position where the hydrogen passes is observed. For details, see Figure 9-12 .

[0216] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a hydrogen-sensitive color-changing material, characterized in that: The following steps are involved: Dropping an inorganic acid into a salt solution containing tungsten ions, adjusting the pH of the salt solution to 0.8-1.2, or adjusting the pH of the salt solution to 1.5-2, to obtain a precursor solution; Adding an acidulant, a capping agent, and a stabilizer to the precursor solution in sequence to obtain a mixed solution; The mixed solution is subjected to a hydrothermal treatment to generate a hydrothermal reaction to obtain WO3; WO3 is annealed in an inert gas atmosphere to obtain WO3 nanoparticles; A metal catalyst is grown in situ on the surface of the WO3 nanoparticles by a photochemical deposition method to obtain the hydrogen-sensitive color-changing material; Wherein, the acidulant comprises at least one of oxalic acid and phosphoric acid, and the molar ratio of the acidulant to tungsten ions is (1-1.5):1; The end-capping agent includes at least one of ammonium chloride, ammonium acetate, ammonium tungstate, ammonium sulfate, ammonium dihydrogen phosphate, and ammonium carbonate, and the molar ratio of the end-capping agent to the acidulant is (0.3-0.5):1; The stabilizer includes at least one of urea, ethylene glycol, and polyethylene glycol, and the molar ratio of the stabilizer to the tungsten ion is (0.1-0.3):1; The step of growing a metal catalyst in situ on the surface of the WO3 nanoparticles by photochemical deposition to obtain the hydrogen-sensitive color-changing material comprises: Dispersing the solid metal salt in an organic solvent, ultrasonicating and stirring to obtain a dispersion; Adding the WO3 nanoparticles and polyvinyl pyrrolidone into the dispersion to obtain a mixed solution; The mixed solution is irradiated with ultraviolet light to cause a reduction reaction, so that the metal is reduced and then grows in situ on the surface of the WO3 nanoparticles to obtain the hydrogen-sensitive color-changing material.

2. The preparation method according to claim 1, characterized in that The annealing temperature is 200-900° C.; and / or, In the step of subjecting the mixed solution to hydrothermal treatment to generate a hydrothermal reaction to obtain WO3, The temperature of the hydrothermal treatment is 120℃~180℃, and the time of the hydrothermal treatment is 7~10 h.

3. The preparation method according to claim 1, characterized in that: In the step of growing a metal catalyst in situ on the surface of the WO3 nanoparticles by photochemical deposition to obtain the hydrogen-sensitive color-changing material, The organic solvent includes at least one of methanol, ethanol, and isopropanol; and / or the solid metal salt includes at least one of PdC12, H2PtCl6·6H2O, PdC12·6H2O, HAuCl4·4H2O, and AgClO4·H2O; and / or the mass ratio of the solid metal salt, the WO3 nanoparticles, and the polyvinyl pyrrolidone is 1:100:(6-10); and / or the reduction reaction time is 10 to 30 minutes.

4. A hydrogen-sensitive color-changing material prepared by the preparation method according to any one of claims 1 to 3.

5. A method for testing the hydrogen-sensitive color-changing material according to claim 4, characterized in that: include: The color-changing performance of hydrogen-sensitive color-changing materials was tested using an optical fiber spectrometer, wherein the test conditions included: at standard atmospheric pressure, a temperature of 0-100°C, a mixed gas flow rate of hydrogen and inert gas of 200-1000 ml / min; or, in a volume of 2-5 cm containing hydrogen, 3 In the confined space, the hydrogen concentrations were 0.1%, 1%, 4%, 10% and 100% respectively, and the test wavelength was 1000nm.

6. A hydrogen-sensitive color-changing coating, characterized in that: The hydrogen-sensitive color-changing material as claimed in claim 4, wherein the WO3 nanoparticles include three-dimensional nanoparticles composed of nanosheets or nanorods.

7. An application of the hydrogen-sensitive color-changing coating as claimed in claim 6, characterized in that: Used to monitor hydrogen leaks.

8. A method for monitoring hydrogen leakage, characterized in that: The hydrogen leakage monitoring method is applied to the hydrogen-sensitive color-changing coating according to claim 6, and the hydrogen leakage monitoring method comprises: Acquire a color change database of the hydrogen-sensitive color-changing coating, wherein the color change database includes a corresponding relationship between color change data of the hydrogen-sensitive color-changing coating and hydrogen leakage; Acquiring real-time color data of a hydrogen-sensitive color-changing coating disposed on the surface of the object to be tested; The real-time hydrogen leakage amount is determined according to the real-time color data and the corresponding relationship.

9. A hydrogen leak monitoring system, characterized in that: It comprises the hydrogen-sensitive color-changing paint as claimed in claim 6, which is arranged on the surface of the object to be tested, a video acquisition unit for collecting color information of the hydrogen-sensitive color-changing paint, and a control unit, a data transmission unit, a data storage processing unit and an alarm unit electrically connected to the video acquisition unit.