A secondary battery and its preparation method and application

By synthesizing the coordination compound protective layer of aluminum ions and phytic acid in situ on the surface of the negative electrode of lithium magnesium alloy and optimizing the electrolyte components, the problem of low conductivity of lithium magnesium alloy negative electrode and ionic liquid electrolyte is solved, and the battery is significantly improved Electrochemical performance and cycle stability enable efficient secondary battery applications.

CN118693282BActive Publication Date: 2024-12-03SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411179161.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The lithium-magnesium alloy negative electrode has problems such as poor operability, low safety and poor electrochemical performance. The conductivity of existing ionic liquid electrolytes is too low, which limits the high capacity and high magnification applications of the battery.

Method used

The coordination compound protective layer of aluminum ions and phytic acid is synthesized in situ on the surface of the negative electrode of lithium magnesium alloy, and the electrolyte is optimized by the combination of specific organic solvents and halogen elements to improve the conductivity and interface properties of the electrolyte.

Benefits of technology

The electrochemical performance and kinetics of the lithium-magnesium alloy negative electrode are significantly improved, the cycle stability and conductivity of the battery are enhanced, and the secondary battery with excellent long-cycle electrical performance is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention provides a secondary battery and its preparation method and application, which relate to the technical field of secondary batteries. Specifically, its negative electrode is a lithium-magnesium alloy, and a protective layer is loaded on the surface; its electrolyte includes lithium salt, magnesium salt, ionic liquid and organic solvent; wherein, the protective layer includes a coordination compound of aluminum ion and phytic acid; the organic solvent includes one of a first solvent and a second solvent, the first solvent is a fluorine-containing ether compound, and the second solvent is an organic matter containing at least one of chlorine, bromine and iodine and fluorine; when the first solvent is selected, the electrolyte also includes an aromatic additive containing at least one of chlorine, bromine and iodine. On the one hand, the present invention performs in-situ surface synthesis on the negative electrode of the lithium-magnesium alloy to obtain a strong and high ionic conductivity protective layer; on the other hand, the composition of the electrolyte is optimized, and the conductivity of the electrolyte is improved by selecting a specific organic solvent or additive, thereby obtaining a secondary battery with excellent long-cycle electrical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a secondary battery and a preparation method and application thereof. Background Art

[0002] Since its introduction, lithium-ion batteries have dominated the portable electronic devices and electric vehicle markets due to their long service life and good stability. However, lithium resources in the earth's crust are not abundant and are unevenly distributed geographically. Limited lithium resources and their energy density have hindered the further development of lithium batteries. In contrast, the use of light metals with high reserves such as magnesium as negative electrode components is an inevitable trend to improve their energy density in the future. On the other hand, lithium has high capacity (10 times higher than graphite anode), the lowest redox potential (-3.04V) and low density (0.534g cm -3 ) and other advantages; however, lithium has high reactivity in air and is flammable when in contact with water, which also brings difficulties to battery manufacturing. In addition, lithium has a tendency to grow dendrites during electrochemical deposition, which leads to defects in electrical performance and safety performance such as dendrites penetrating the separator and even causing battery short circuit.

[0003] In contrast, magnesium metal anodes are less likely to form magnesium dendrites, and in this respect are much safer than lithium metal batteries. In addition, magnesium metal batteries have received great attention due to their high abundance and high capacity. Specifically, the reduction potential of magnesium metal is -2.4V, the density is 1.74 g cm -3 , and during its electrochemical reduction and oxidation process, magnesium undergoes two electron transfers, achieving 3833mAh mL -1 volume capacity.

[0004] However, pure magnesium metal anode batteries have at least the following disadvantages: (1) Mg metal is incompatible with most electrolytes. After the electrolyte is reduced by Mg, a passivation film is formed on the anode surface, which hinders the Mg 2+ Migration of Mg; (2) 2+ It has a higher charge density, has a stronger binding force with anions and solvents, and generates higher energy, requiring desolvation ability and overcoming high diffusion barriers. 2+ The diffusion kinetics in the electrode are relatively slow, and its high polarity easily destroys the cathode structure, resulting in poor electrochemical performance. 6 S 8 The upper limit of charging under this system is generally distributed at 3.5V, which does not meet the high voltage requirements.

[0005] In order to improve the above situation, lithium and magnesium can be used together to prepare the negative electrode, that is, a lithium-magnesium alloy negative electrode is used. For example: The patent with publication number CN202310358234.2 mechanically mixes lithium metal and magnesium powder to prepare a lithium-magnesium composite electrode material, and prepares it into a battery, and the electrolyte is an organic carbonate electrolyte. However, the mechanical mixing of lithium metal and magnesium powder not only has poor operability, low safety, and is difficult to commercialize, but also the organic carbonate solvent will form an insulating and passivation layer on the magnesium surface, and the organic component in the SEI film formed on the surface of the alloy negative electrode is high, resulting in a sharp drop in service life.

[0006] Ionic liquids are liquids composed entirely of ions, and are often used in the field of electrolytes due to their strong chemical stability, wide voltage window, low volatility, and high thermal stability. However, ionic liquid electrolytes usually have high viscosity and low ionic conductivity due to factors such as strong ion-ion interactions and huge ion volumes, which limits the application of ionic liquid electrolytes in high-capacity and high-rate electrochemical systems.

[0007] In order to solve this problem, the prior art proposes to use fluorinated ether reagents as diluents (such as tetrafluoroethyl, tetrafluoropropyl ether, etc.) to reduce the viscosity of ionic liquid electrolytes. However, fluorinated ether reagents mainly form LiF-type SEI films on the surface of lithium-magnesium alloys. LiF has a strong affinity for lithium, but its conductivity is low. At the same time, traditional fluorinated ether reagents have too high fluorine content, and fluorine is a strong electron-withdrawing group, so fluorinated ether reagents have no solvation ability for lithium salts and magnesium salts, and cannot completely dissociate them, which leads to ultra-low conductivity of the electrolyte.

[0008] To further solve the above defects and achieve full dissolution of lithium / sodium salts in ionic liquid electrolytes, the anion and cation structures can be adjusted to meet different requirements such as high ionic conductivity, wide electrochemical stability window, and stable interface properties. However, in fact, the types of ionic liquids that can be used as electrolytes are very limited; it is currently difficult to achieve application promotion while solving the above conductivity defects through customized expansion of ionic liquids.

[0009] In view of this, the present invention is proposed. Summary of the invention

[0010] The first purpose of the present invention is to provide a secondary battery, which is used to solve the inherent defects of lithium-magnesium alloy negative electrodes on the one hand, and to solve the defect of too low conductivity of ionic liquid electrolytes on the other hand; in the present invention, on the one hand, a strong and high ionic conductivity protective layer is synthesized in situ on the surface of the lithium-magnesium alloy negative electrode to improve the plating / deplating uniformity and kinetics of Li-Mg, and on the other hand, the composition of the electrolyte is optimized, and the conductivity of the electrolyte is significantly improved by selecting a specific organic solvent (or additive) in combination with a conventional ionic liquid component, thereby obtaining a secondary battery with excellent long-cycle electrical performance.

[0011] The second object of the present invention is to provide a method for preparing the secondary battery, which is simple and easy to implement, has low equipment cost, and is easy to achieve mass production.

[0012] The third object of the present invention is to provide an electrical device.

[0013] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0014] A secondary battery comprises a positive electrode, a negative electrode, a separator and an electrolyte;

[0015] The negative electrode is a lithium-magnesium alloy, and the surface of the lithium-magnesium alloy is loaded with a protective layer; the electrolyte includes a lithium salt, a magnesium salt, an ionic liquid and an organic solvent;

[0016] Wherein, the protective layer comprises a coordination compound of aluminum ions and phytic acid;

[0017] The organic solvent includes one of a first solvent and a second solvent; the first solvent is a fluorine-containing ether compound, and the second solvent is an organic substance containing at least one of chlorine, bromine, and iodine and fluorine;

[0018] When the organic solvent includes the first solvent, the electrolyte of the secondary battery further includes an aromatic additive containing at least one of chlorine, bromine, and iodine.

[0019] A method for preparing the secondary battery comprises the following steps:

[0020] (1) Preparation of negative electrode: The lithium-magnesium alloy is immersed in a mixed solution containing an aluminum source and phytic acid, and then allowed to stand, solid-liquid separation and drying are performed in sequence to obtain a negative electrode;

[0021] (2) Assemble the positive electrode, negative electrode, electrolyte and separator to obtain a secondary battery.

[0022] An electrical device comprises the secondary battery.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention in situ synthesizes a protective layer comprising a coordination compound of aluminum ions and phytic acid on the surface of a lithium-magnesium alloy negative electrode. The protective layer further coordinates with magnesium when powered on, thereby significantly improving the electrical performance of the negative electrode. Specifically: (1.1) The electrolyte used in the present invention contains halogen elements. In such electrolytes, uneven magnesium deposition / stripping behavior will still lead to defects such as pitting and perforation of the magnesium negative electrode, thereby causing battery failure or even short circuit. The good water-oxygen tolerance and electrolyte wettability of the protective layer on the surface of the negative electrode (an ion-enhanced phytic acid layer) can effectively homogenize the distribution of magnesium ions on the surface of the negative electrode and avoid uneven magnesium dissolution / deposition. (1.2) In the present invention, aluminum ions achieve a functional effect similar to that of a "cross-linking agent". First, aluminum ions have a strong coordination ability with phytic acid. Second, when the secondary battery is working, there is aluminum-magnesium coordination. On the one hand, it can enhance the strength of the artificial SEI and avoid its rupture and failure during long cycles. On the other hand, the aluminum-magnesium coordination can reduce the energy barrier of the negative electrode and provide lithium-magnesium deposition on the surface of the negative electrode.

[0025] (2) The present invention uses a combination of a fluorinated ether solvent and a halogenated aromatic additive, or a solvent containing F and X (X = Cl, Br, I), and realizes the role of electrolyte diluent through the combination of specific halogen elements and fluorine elements, which can not only reduce the viscosity of the ionic liquid and improve the mobility of (lithium) ions in the electrolyte, but also help the lithium ions to coordinate the aggregation of anions, thus constructing a strong high-Li + Conductive double halide SEI film; further, the double halide SEI film effectively enhances the mobility of lithium ions and inhibits the nucleation and growth of lithium dendrites. At the same time, the halogen element in the electrolyte can significantly improve the conductivity of the electrolyte, and the energy barrier of LiX (X=Cl, Br, I) formed by the halogen element is lower than that of LiF, which is conducive to reducing the SEI film energy barrier and improving the ion conduction between the positive and negative electrodes, thereby improving the electrochemical performance of the battery.

[0026] When a combination of a fluorinated ether solvent and a halogenated aromatic additive is used, the additive is a fluorinated ether diluent with weak solvation ability, and the molecular weight of the fluorine is strictly controlled, which can have a certain dissociation ability for lithium salts and magnesium salts; further, the aromatic additive has a low affinity for lithium ions, is not easy to coordinate with lithium ions, has a strong fluorine-donating ability, forms a π-π interaction with the ionic liquid, and can effectively reduce the viscosity of the electrolyte and promote lithium ion transmission. At the same time, the halogen element helps to build a strong high-Li + The conductive double halide SEI film forms a double halide SEI, which effectively enhances the mobility of lithium ions and inhibits the nucleation and growth of lithium dendrites. DETAILED DESCRIPTION

[0027] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but those skilled in the art will appreciate that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. Those who do not specify specific conditions in the embodiments are carried out according to conventional conditions or conditions recommended by the manufacturer. Those who do not specify the manufacturer for reagents or instruments used are conventional products that can be purchased commercially. In addition, the terms "one", "two", "1", "2" are only used for descriptive purposes and cannot be interpreted as indicating or implying relative importance.

[0028] A first aspect of the present invention is to provide a secondary battery including a positive electrode, a negative electrode, a separator and an electrolyte.

[0029] The negative electrode of the present invention is a lithium-magnesium alloy, and the surface of the lithium-magnesium alloy is loaded with a protective layer; wherein the protective layer includes a coordination compound of aluminum ions and phytic acid.

[0030] The electrolyte of the present invention includes lithium salt, magnesium salt, ionic liquid and organic solvent; wherein the organic solvent includes one of a first solvent and a second solvent; the first solvent is a fluorine-containing ether compound, and the second solvent is an organic matter containing at least one of chlorine, bromine and iodine and fluorine; when the organic solvent includes the first solvent, the electrolyte of the secondary battery also includes an aromatic additive containing at least one of chlorine, bromine and iodine.

[0031] As a preferred embodiment, the positive electrode of the secondary battery is selected from positive electrode materials capable of achieving high voltage output, including at least one of ternary positive electrode materials NCM, ternary positive electrode materials NCA, lithium cobalt oxide, lithium iron manganese oxide or lithium-rich manganese base.

[0032] As a preferred embodiment, in the lithium-magnesium alloy, the mass ratio of lithium to magnesium is (50~99.9):(0.1~50), including but not limited to any one of 50:50, 55:45, 60:40, 65:35, 70:30, 75:25, 80:20, 85:15, 90:10, 95:5, 99.9:0.1 or a ratio interval consisting of any two of them.

[0033] As a preferred implementation, the thickness of the protective layer is 5 nm to 1.5 μm.

[0034] As a preferred embodiment, the lithium salt includes at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(nonafluorobutylsulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium trifluoroacetate, lithium difluoroacetate, lithium hexafluorosilicate, lithium hexafluorophosphate or lithium tetrafluoroborate.

[0035] As a preferred embodiment, the magnesium salt includes at least one of magnesium bis(trifluoromethylsulfonyl)imide, magnesium fluorosilicate, magnesium trifluoromethanesulfonate, magnesium benzoate, magnesium potassium fluoride silicate, magnesium nitrate, magnesium metaborate, magnesium hypophosphite, magnesium phosphate, magnesium hexafluorophosphate, ammonium magnesium phosphate, trimagnesium phosphate, magnesium borate or magnesium tetrafluoroborate.

[0036] As a preferred embodiment, in the electrolyte, the sum of the concentrations of the lithium salt and the magnesium salt is 0.2 mol / L~5 mol / L, including but not limited to any one of 0.2, 0.4, 0.5, 0.6, 0.8, 1, 1.2, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 (mol / L) or a numerical range consisting of any two of them.

[0037] As a more preferred embodiment, in the electrolyte, the mass ratio of the lithium salt to the magnesium salt is (50~99.9):(0.1~50), including but not limited to any one of 50:50, 55:45, 60:40, 65:35, 70:30, 75:25, 80:20, 85:15, 90:10, 95:5, 99.9:0.1 or a ratio interval consisting of any two of them.

[0038] As a more preferred embodiment, the difference between the mass ratio of the lithium salt to the magnesium salt and the mass ratio of lithium to magnesium in the lithium-magnesium alloy should be less than 15%.

[0039] As a preferred embodiment, the ionic liquid is a cationic liquid electrolyte, including but not limited to imidazoles, pyrrolidinyls, and phosphorus-containing cations; in some more preferred embodiments, the ionic liquid includes 1-n-butyl-1-methylpyrrolidine bis(trifluoromethylsulfonyl)imide, 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide, 1,2,3-trimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-2,3-dimethylimidazolium hexafluorophosphate, 1-ethyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-2,3-dimethylimidazolium bis(fluorosulfonyl)imide, 1-ethyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-2,3-dimethylimidazolium bis(fluorosulfonyl)imide, 1-ethyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1 -Butyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-hexyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-octyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-decyl-2,3-dimethylimidazolium tetrafluoroborate, 1-decyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-decyl-2,3-dimethylimidazolium hexafluoroborate At least one of fluorophosphate, 1-dodecyl-2,3-dimethylimidazolium tetrafluoroborate, 1-dodecyl-2,3-dimethylimidazolium hexafluorophosphate, 1-tetradecyl-2,3-dimethylimidazolium hexafluorophosphate, 1-tetradecyl-2,3-dimethylimidazolium tetrafluoroborate, 1-hexadecyl-2,3-dimethylimidazolium tetrafluoroborate, and 1-hexadecyl-2,3-dimethylimidazolium hexafluorophosphate.

[0040] As a preferred embodiment, in the electrolyte, the amount of the ionic liquid is less than the amount of the organic solvent by volume; in some more preferred embodiments, the amount ratio of the ionic liquid to the organic solvent is (5~45): (55~95) by volume.

[0041] As a preferred embodiment, the first solvent is a fluorine-containing ether compound, and the fluorine-containing ether compound contains only carbon, fluorine, oxygen and hydrogen; in some more preferred embodiments, the fluorine-carbon ratio of the fluorine-containing ether compound is ≤3, and the number of fluorine atoms in the fluorine-containing ether compound is ≤10.

[0042] As a more preferred embodiment, the first solvent includes at least one of bis(2,2,2-trifluoroethyl) ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, difluoromethyl-2,2,2-trifluoroethyl ether, bis-(1,2,2,2-tetrafluoroethyl) ether, 2,2,2-trifluoroethyl methyl ether, 1,2,2-trifluoroethyl trifluoromethyl ether, fluoromethyl-1,1,1,3,3,3-hexafluoroisopropyl ether, and defluorinated ether 1-653.

[0043] As a preferred embodiment, the second solvent is at least one of a halogenated ether, a halogenated alkane or a halogenated aromatic hydrocarbon, and the halogen elements in the second solvent include F and X, and X is at least one of Cl, Br or I; in some more preferred embodiments, the fluorine-carbon ratio of the second solvent is ≤3.

[0044] As a more preferred embodiment, the second solvent includes at least one of 1,2-dichlorotrifluoroethyl trifluoromethyl ether, 2-chloro-1,1,2-trifluoroethyl methyl ether, 2-chloro-1,1,2-trifluoroethyl ethyl ether, 2-bromo-1,2,2-trifluoroethyl trifluoromethyl ether, 1,1-dichloro-2,2,2-trifluoroethyl difluoromethyl ether, 1,1-dichloro-2,2,2-trifluoroethyl chlorodifluoromethyl ether, isoflurane, fluorocarbon, 2,2,2-trifluoroiodoethane, 2,3,4-trifluoroiodobenzene, 2,4,6-trifluoroiodobenzene, 2,2,3,3-tetrafluoroiodopropane, 1,1,2,2-tetrafluoroiodoethane, 1,1,2,2-tetrafluoroiodoethane, 1,1,2,3,3,3-hexafluoroiodopropane, and 4-(4-isopropylcyclohexyl)-2,6-difluoroiodobenzene.

[0045] As a preferred embodiment, the aromatic additive includes at least one of phenyl, benzyl or anisole, and the halogen element in the aromatic additive includes F and X, and X is at least one of Cl, Br or I; in some more preferred embodiments, the aromatic additive includes [bis(trifluoroacetoxy)iodo]benzene, p-fluorobenzyl chloride, m-fluorobenzyl chloride, o-fluorobenzyl chloride, 2,5-difluorochlorobenzene, 3,4-difluorobenzyl chloride, 2-chloro-6-fluorobenzyl chloride, 2,4-difluorochloro Benzene, 2,6-difluorobenzyl chloride, 2-chloro-6-fluoroanisole, 4-chloro-3-fluoroanisole, 4-chloro-2-fluoroanisole, p-fluorobromobenzene, 3-fluorobromoethylbenzene, 2-fluorobenzyl bromide, p-fluorobenzyl bromide, 4-(difluorobromomethyl)bromobenzene, 2,4-difluorobenzyl bromide, 3-chloro-4-fluorobenzyl bromide, 2-bromo-4-fluorobenzyl bromide, 3,4-difluorobenzyl bromide, 3,4-difluorobromobenzene, 2,6-difluorobenzyl bromide, 2,4-difluorobromobenzene, 2-chloro-6-fluorobenzyl bromide, 2,4,5- trifluorobromobenzene, 3,4,5-trifluorobromobenzyl, 4,5-dichloro-2-fluorobromobenzene, 4-chloro-2,6-difluorobromobenzyl, 3,4-dichloro-2-fluorobromobenzene, 2,3,4,5-tetrafluorobromobenzyl, 2,3,4,6-tetrafluorobromobenzene, 4-methoxytetrafluorobromobenzyl, 2,3,4,5-tetrafluorobromobenzene, 2,4-dimethyl-3-fluorobromobenzene, 2-amino-3,4-difluorobromobenzene, o-fluoroiodobenzene, 4-fluoroiodobenzene, 3-fluoroiodobenzene, 2.4.5-trifluoroiodobenzene, 3 ,5-difluoroiodobenzene, 3,5-difluoroiodobenzene, 2-bromo-6-fluoroiodobenzene, 3-chloro-2-fluoroiodobenzene, 5-chloro-2-fluoroiodobenzene, 3-bromo-4-fluoroiodobenzene, 2-chloro-6-fluoroiodobenzene, 4-chloro-3-fluoroiodobenzene, 2,4-difluoroiodobenzene, 2-bromo-4-fluoroiodobenzene, 3,4,5-trifluoroiodobenzene, 2,4,6-trifluoroiodobenzene, 2,3,4-trifluoroiodobenzene, 4-bromo-2,5-difluoroiodobenzene, 4-chloro-3,5-difluoroiodobenzene.

[0046] As a preferred implementation manner, the mass ratio of the aromatic additive to the electrolyte is 0.05% to 2.0%.

[0047] The second aspect of the present invention is to provide a method for preparing the secondary battery, which mainly includes the following steps: (1) preparing the negative electrode, specifically, a method for preparing the load of lithium-magnesium alloy and its protective layer; (2) assembling the functional components of the secondary battery.

[0048] Furthermore, the preparation method includes the following steps: immersing the lithium-magnesium alloy in a mixed solution containing an aluminum source and phytic acid, and then standing, solid-liquid separation and drying in sequence to obtain a negative electrode; assembling the positive electrode, negative electrode, electrolyte and separator to obtain a secondary battery.

[0049] As a preferred embodiment, the aluminum source includes at least one of aluminum nitrate or lithium aluminate.

[0050] As a preferred embodiment, in the mixed solution, liquid phytic acid can be regarded as a solvent, and the molar concentration of the aluminum source is 0.5 mmol / L to 100 mmol / L.

[0051] As a preferred implementation manner, the volume usage relationship between the aluminum-magnesium alloy and the mixed liquid should satisfy: the aluminum-magnesium alloy can be completely immersed in the mixed liquid.

[0052] As a preferred embodiment, the thickness of the protective layer is regulated by the molar concentration of the aluminum source in the mixed solution and the standing time; in some more preferred embodiments, the standing time is 5 min to 60 min.

[0053] As a preferred embodiment, the preparation method of the electrolyte comprises: fully mixing a lithium salt, a magnesium salt, an ionic liquid and an organic solvent; the sufficient mixing can be assisted by means such as stirring, oscillation, centrifugation, ultrasound, etc. to achieve uniformity between the components in the electrolyte, and the present invention does not impose specific restrictions on the means of sufficient mixing.

[0054] As a preferred embodiment, the assembly can be performed by conventional methods in the art. As long as an electrical component with secondary battery function can be obtained, any assembly process or combination characteristics of components are not limited.

[0055] The third aspect of the present invention is to provide an electric device, wherein the electric device includes the secondary battery. It is understood that the electric device can be any device that relies on electric energy to work or operate, including but not limited to new energy vehicles, building electrical equipment, industrial electrical appliances, household and agricultural electrical appliances, etc.; when including the secondary battery, any electric device equipped with the secondary battery can belong to an embodiment of the present invention.

[0056] Example

[0057] S1: Preparation of electrolyte:

[0058] In Examples 1 to 9: lithium salt, magnesium salt, ionic liquid, organic solvent and additive are weighed or measured respectively; wherein the mass ratio of lithium in the lithium salt to magnesium in the magnesium salt is 7:3, and the volume ratio of ionic liquid to organic solvent is 30:70; the ionic liquid and the organic solvent are first mixed, and then the lithium salt and the magnesium salt are added to the liquid phase to obtain a mixed solution, based on the sum of the concentrations of the lithium salt and the magnesium salt being 3 mol / L; the additive is then added so that the added amount accounts for 1.0% of the total mass of the electrolyte; and then the electrolyte is obtained after stirring for 10 hours;

[0059] In Examples 10 to 18: lithium salt, magnesium salt, ionic liquid and organic solvent are weighed or measured respectively; wherein the mass ratio of lithium in the lithium salt to magnesium in the magnesium salt is 7:3, and the volume ratio of the ionic liquid to the organic solvent is 30:70; the ionic liquid and the organic solvent are first mixed, and then the lithium salt and the magnesium salt are added to the liquid phase at a sum of the concentrations of the lithium salt and the magnesium salt of 3 mol / L, and then stirred for 10 hours to obtain an electrolyte.

[0060] Specifically, the components of lithium salt, magnesium salt, ionic liquid, organic solvent and additive in each embodiment are shown in Table 1 and Table 2 below; when there is more than one component selection in a certain column, the mass ratios of the multiple components will be additionally given in Table 1 and Table 2.

[0061] Table 1

[0062]

[0063] Table 2

[0064]

[0065] S2: Preparation of positive electrode: LiNi 9 Co 1 Mn 1 O 2 , conductive agent SuperP, adhesive PVDF and carbon nanotubes (CNT) are mixed evenly in a mass ratio of 96.5:2.5:1.0:0.5 to form a lithium-ion battery positive electrode slurry, which is coated on an aluminum foil for a current collector, dried at 85°C and then cold pressed; then trimmed, cut and slit, and then dried at 85°C under vacuum conditions for 8 hours to form a lithium metal battery positive electrode sheet.

[0066] S3: Preparation of negative electrode sheet: Use commercially available 10μm-grade lithium-magnesium alloy (lithium:magnesium mass ratio is 80:20) to cut and obtain negative electrode substrate sheet; then use aluminum nitrate as solute and phytic acid as solvent to prepare a 5mM (mmol / L) reaction solution, stir evenly, soak the lithium-magnesium alloy in the reaction solution for 10 minutes, then take out and dry to obtain the negative electrode sheet.

[0067] S4: Battery assembly: A four-positive and five-negative lithium-magnesium battery is made through a lamination process, and a 10μm-grade PP film is used as the separator; the capacity is 2.1Ah, and the above-mentioned electrolyte is injected to obtain a soft-pack battery sample for testing.

[0068] Embodiment 19

[0069] It is basically the same as Example 1, except that:

[0070] In step S2, the nickel-cobalt-lithium-manganese oxide ternary material LiNi 9 Co1 Mn 1 O 2 Replaced by LiNiCoAlO 2 .

[0071] Embodiment 20

[0072] It is basically the same as Example 1, except that:

[0073] In step S3 , the mass ratio of lithium to magnesium in the lithium-magnesium alloy in the negative electrode substrate is 90:10.

[0074] Embodiment 21

[0075] It is basically the same as Example 1, except that:

[0076] In step S3, aluminum nitrate is used as the solute and phytic acid is used as the solvent to prepare a 0.5 mM reaction solution.

[0077] Embodiment 22

[0078] It is basically the same as Example 1, except that:

[0079] In step S3, aluminum nitrate is used as the solute and phytic acid is used as the solvent to prepare a 100 mM reaction solution.

[0080] Comparative Example 1

[0081] It is basically the same as Example 1, except that:

[0082] In step S1 , the additive component is removed.

[0083] Comparative Example 2

[0084] It is basically the same as Example 2, except that:

[0085] In step S1, the amount of additive added accounts for 3.5% of the total mass of the electrolyte.

[0086] Comparative Example 3

[0087] It is basically the same as Example 2, except that:

[0088] In step S1, the organic solvent is perfluoroheptyl ether.

[0089] Comparative Example 4

[0090] It is basically the same as Example 1, except that:

[0091] In step S1 , the volume ratio of the ionic liquid to the organic solvent is 50:50.

[0092] Comparative Example 5

[0093] It is basically the same as Example 10, except that:

[0094] In step S1 , the volume ratio of the ionic liquid to the organic solvent is 60:40.

[0095] Comparative Example 6

[0096] It is basically the same as Example 1, except that:

[0097] In step S3, the negative electrode substrate sheet is directly used as the negative electrode sheet.

[0098] The electrical performance of the soft-pack batteries corresponding to the above embodiments and comparative examples was tested; the testing method is as follows:

[0099] (1) First effect: At 25±3℃, charge at a constant current of 0.05C to 4.2V, then charge at a constant voltage of 4.2V to a cut-off current of 0.05C, and record the charge capacity as C1; then discharge at a constant current of 0.05C to 2.8V, and record the discharge capacity as D1; ​​First effect = (D1 / C1) × 100%.

[0100] (2) Capacity retention rate at the 100th cycle: At 25±3℃, charge the battery at a constant current of 0.33C to 4.2V, charge it at a constant voltage of 4.2V to a cut-off current of 0.05C, and then discharge it at a constant current of 1C to 2.8V. The discharge capacity is recorded as C1. Repeat the charge and discharge process 100 times each, and obtain the 100th discharge capacity CN. The capacity retention rate at the 100th cycle = (CN / C1) × 100%.

[0101] (3) Average Coulombic efficiency of the first 100 cycles: Same as the test in step 2, the calculation method is as follows: Coulombic efficiency of each cycle CE = discharge capacity / charge capacity × 100%, average Coulombic efficiency of the first 100 cycles CE = SUM (CE 1 ~CE n ) / 100×100%.

[0102] (4) 5C / 0.5C capacity retention rate: At 25±3℃, charge at 0.5C constant current to 4.2V, charge at 4.2V constant voltage to a cut-off current of 0.05C, and then discharge the battery at 0.5C constant current to 2.8V; cycle for 5 times, record the discharge capacity of each cycle, and take the average as A; charge at 0.5C constant current to 4.2V, charge at 4.2V constant voltage to a cut-off current of 0.05C, and then discharge the battery at 3C constant current to 2.8V; cycle for 5 times, record the discharge capacity of each cycle, and take the average as B. 5C / 0.5C capacity retention rate = B / A×100%.

[0103] (5) 10C / 0.5C capacity retention rate: At 25±3℃, charge at 0.5C constant current to 4.2V, charge at 4.2V constant voltage to a cut-off current of 0.05C, and then discharge at 0.5C constant current to 2.8V; cycle for 5 times, record the discharge capacity of each cycle, and take the average as C; charge at 0.5C constant current to 4.2V, charge at 4.2V constant voltage to a cut-off current of 0.05C, and then discharge at 10C constant current to 2.8V; cycle for 5 times, record the discharge capacity of each cycle, and take the average as D. 10C / 0.5C capacity retention rate = D / C × 100%.

[0104] The results are shown in Table 3 below.

[0105] Table 3

[0106]

[0107] According to the data in Table 3, the following conclusions can be drawn:

[0108] (1) The first efficiency of the batteries provided in Examples 1 to 22 is as high as 88.59% to 90.16%, the capacity retention rate at the 100th cycle is 94.19% to 96.92%, the average coulombic efficiency in the first 100 cycles is 99.90% to 99.99%, the 5C / 0.5C capacity retention rate is 84.83% to 86.98%, and the 10C / 0.5C capacity retention rate is 70.92% to 74.39%, which has a high first efficiency, excellent rate performance and cycle performance.

[0109] (2) Based on the data of Comparative Examples 1 to 3 and Examples 1 to 9, it can be found that when the fluorinated ether solvent and the halogen-containing aromatic additive are used in combination, the electrical performance of the battery can be most effectively improved; relatively, the absence of the halogen-containing aromatic additive (Comparative Example 1), the excessive amount of the halogen-containing aromatic additive (Comparative Example 2), and the presence of F atoms greater than 10 in the fluorinated ether solvent (Comparative Example 3) will all lead to a certain degree of decrease in the electrical performance of the resulting battery.

[0110] (3) Based on the data of Comparative Examples 4-5 and Examples 10-18, it can be found that when the amount of ionic liquid used is less than that of the organic solvent, the electrical performance of the battery can be most effectively improved; conversely, when the volume ratio of the ionic liquid to the organic solvent is the same (Comparative Example 4) or when the volume of the ionic liquid is greater than that of the organic solvent (Comparative Example 5), the electrical performance of the resulting battery will decrease to a certain extent.

[0111] (4) Based on the data of Comparative Example 6 and Examples 1 to 22, it can be found that the examples in situ synthesize a protective layer comprising a coordination compound of aluminum ions and phytic acid on the surface of the lithium-magnesium alloy negative electrode. The protective layer further coordinates with magnesium when powered, thereby achieving a significant improvement in the electrical performance of the negative electrode. Compared with the conventional lithium-magnesium alloy negative electrode, the electrical performance of the battery can be effectively improved.

[0112] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A secondary battery, characterized in that: The negative electrode of the secondary battery is a lithium-magnesium alloy, and the surface of the lithium-magnesium alloy is loaded with a protective layer; the electrolyte of the secondary battery includes a lithium salt, a magnesium salt, an ionic liquid and an organic solvent; Wherein, the protective layer comprises a coordination compound of aluminum ions and phytic acid; The organic solvent includes one of a first solvent and a second solvent; the first solvent is a fluorine-containing ether compound, and the second solvent is an organic substance containing at least one of chlorine, bromine, and iodine and fluorine; When the organic solvent includes the first solvent, the electrolyte of the secondary battery further includes an aromatic additive containing at least one of chlorine, bromine, and iodine.

2. The secondary battery according to claim 1, characterized in that: The active material of the positive electrode of the secondary battery includes at least one of a ternary positive electrode material NCM, a ternary positive electrode material NCA, lithium cobalt oxide, lithium iron manganese oxide or a lithium-rich manganese base.

3. The secondary battery according to claim 1, characterized in that: In the lithium-magnesium alloy, the mass ratio of lithium to magnesium is (50-99.9): (0.1-50).

4. The secondary battery according to claim 1, characterized in that: The lithium salt includes at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(nonafluorobutylsulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium trifluoroacetate, lithium difluoroacetate, lithium hexafluorosilicate, lithium hexafluorophosphate or lithium tetrafluoroborate; And / or, the magnesium salt includes at least one of magnesium bis(trifluoromethylsulfonyl)imide, magnesium fluorosilicate, magnesium trifluoromethanesulfonate, magnesium benzoate, magnesium potassium fluoride silicate, magnesium nitrate, magnesium metaborate, magnesium hypophosphite, magnesium phosphate, magnesium hexafluorophosphate, ammonium magnesium phosphate, trimagnesium phosphate, magnesium borate or magnesium tetrafluoroborate.

5. The secondary battery according to claim 1, characterized in that: The ionic liquid includes at least one of a cationic imidazolium ionic liquid or a cationic pyrrolidine ionic liquid; In terms of volume, the ionic liquid is less than the organic solvent.

6. The secondary battery according to claim 1, characterized in that: In the first solvent, the constituent elements of the fluorine-containing ether compound are: carbon, fluorine, oxygen and hydrogen; The fluorine-carbon ratio of the fluorine-containing ether compound is ≤3, and the number of fluorine atoms in the fluorine-containing ether compound is ≤10.

7. The secondary battery according to claim 1, characterized in that: The second solvent is at least one of a halogen-containing ether, a halogen-containing alkane or a halogen-containing aromatic hydrocarbon; The fluorine-to-carbon ratio of the second solvent is ≤3.

8. The method for preparing a secondary battery according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) Preparation of negative electrode: The lithium-magnesium alloy is immersed in a mixed solution containing an aluminum source and phytic acid, and then allowed to stand, solid-liquid separation and drying are performed in sequence to obtain a negative electrode; (2) Assemble the positive electrode, negative electrode, electrolyte and separator to obtain a secondary battery.

9. The method for preparing a secondary battery according to claim 8, characterized in that: The aluminum source includes at least one of aluminum nitrate or lithium aluminate; The molar concentration of the aluminum source is 0.5 mmol / L to 100 mmol / L.

10. An electrical device, characterized in that: The electrical device comprises the secondary battery as claimed in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Lithium-magnesium composite electrode material, lithium metal battery, preparation method and application

    CN116060615A

  • Film-forming liquid for artificial SEI film on surface of negative electrode of rechargeable magnesium battery and preparation method for same

    CN113540395A

  • Secondary battery and preparation method thereof, battery module, battery pack and electric device

    CN117561623A

  • Phytic acid based metallogel and applications thereof

    US20170229725A1

  • Cathode active material for lithium secondary battery and method of manufacturing the same