A NF@Ni(OH)2@MnO x Monolithic catalyst and preparation method and application thereof
By loading the NF@Ni(OH)2@MnOx catalyst with nickel hydroxide and manganese oxide on the nickel foam matrix, the problem of insufficient stability and efficiency of nickel foam substrate catalyst in the prior art is solved, and organic pollutants are realized The efficient degradation and long-term stable operation are suitable for industrial applications.
Patent Information
- Application Number
- CN202411187285.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing ozone catalysts of nickel foam substrates have shortcomings in terms of stability and efficiency, especially the problem of decreasing catalytic activity during long-term use, limiting their widespread use in industrial applications.
The NF@Ni(OH)2@MnOx monolithic catalyst is used, which is loaded with Ni(OH)2 layer of nickel hydroxide on a foamed nickel matrix and re-loaded with manganese oxide MnOx thereon, using Ni(OH)2 As an electron shuttle layer, it enhances the activation ability of MnOx, improves the adsorption and decomposition efficiency of ozone, and forms reactive oxygen species to degrade organic pollutants.
It achieves efficient degradation of organic pollutants in gaseous and water bodies, with degradation rates up to more than 84% and more than 82%, and the catalyst maintains high activity within 720 minutes, significantly improves stability, extends the service cycle, and is suitable for industrial use. Production.
Smart Images

Figure CN118698558B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalyst materials. More specifically, it relates to a NF@Ni(OH)2@MnO x Monolithic catalyst and preparation method and application thereof. Background Art
[0002] In industrial production, due to the use of fossil fuels and the production of chemical products, various industrial wastewaters and industrial waste gases with different hazards and difficult to control will be generated. Both contain organic pollutants that are harmful to human health. Organic pollutants in industrial waste gas are highly volatile, highly active, and easy to diffuse. Direct discharge will not only have adverse effects on the natural environment, but also cause great harm to human health. In recent years, the "Air Pollutant Emission Standards" and "Technical Specifications for Organic Waste Gas Treatment Engineering" formulated by the state clearly point out that it is necessary to maintain the whole process control idea from source reduction, process control to terminal treatment, further standardize the pollution discharge behavior of enterprises, and control the generation and emission of organic waste gas. Among them, sulfur-containing organic waste gas is very likely to cause odor pollution and serious secondary environmental problems, which has an adverse effect on human normal life. Methyl mercaptan (CH3SH) is a typical representative with an ultra-low olfactory threshold. Long-term exposure to a low concentration of CH3SH environment will poison the human respiratory and nervous systems, and CH3SH will also corrode the reactor and cause the catalyst in the chemical industry to deactivate. Therefore, it is urgent to develop effective treatment technologies to degrade and adsorb organic pollutants in industrial waste gas. Industrial wastewater usually contains a large amount of organic pollutants that are harmful to aquatic organisms or human health. These organic substances have the characteristics of low concentration, high stability, and high hazard, and are difficult to be effectively removed by traditional processes. Therefore, research on new processes that can effectively remove difficult-to-degrade organic substances in water and thus effectively improve the quality of drinking water is of extremely important strategic significance to my country's sustainable development.
[0003] The current treatment strategies mainly include adsorption, absorption, photocatalysis, biodegradation, plasma and other technologies. Although each of the above methods can effectively remove organic pollutants, they also have their own shortcomings. For example, pollutants will desorb from the adsorbent and cause secondary pollution; the photocatalytic method is not efficient for the treatment of high-concentration organic waste gas or wastewater; traditional biodegradation reactors have poor removal performance for hydrophobic organic matter, and organic pollutants with biological toxicity will also reduce catalytic activity, etc. Catalytic ozone oxidation is a method of using catalysts to activate ozone to produce free radicals to degrade organic pollutants into harmless products (CO2, H2O, etc.). Compared with traditional treatment technologies, it consumes less energy to remove organic pollutants and produces fewer toxic products, and is considered to be one of the most effective methods. In the selection of catalysts, compared with precious metals, manganese-based oxides have the advantages of large reserves, rich varieties, and low prices. At the same time, manganese-based oxide catalysts with special morphology and crystal structure are easy to produce oxygen vacancies as ozone adsorption sites, and the outer electrons of manganese are easy to interact with ozone, activating ozone decomposition to produce active oxygen species to attack organic pollutants. Therefore, manganese-based oxides are considered to be one of the materials that effectively catalyze ozone oxidation. Although manganese-based oxide catalysts have made great research progress in the field of catalytic ozone oxidation, low stability and easy deactivation are still two major challenges for the expansion of the application of this technology.
[0004] Traditional catalyst applications usually involve coating powdered catalysts on carriers, which results in large bed pressure drop, general mass and heat transfer performance, and difficulty in recovery. Few people have paid attention to the effect of catalyst loading on catalytic activity, but this plays an important role in moving from laboratory to practical application. Therefore, the application of manganese-based monolithic catalysts in the field of organic pollutant treatment deserves in-depth study. Among them, the strategy of loading manganese oxides in a "top-down manner" with foamed metal as the substrate has been confirmed by research. Transition metals such as manganese, nickel, and cobalt can be directly loaded on the substrate without coating. In addition, the monolithic catalyst has a developed pore structure, with a pressure drop two to three orders of magnitude lower than that of the powdered catalyst at the same air velocity, and the catalyst wall is thin, with good mass and heat transfer effects, easy to recover and regenerate, and has certain advantages in simplifying the industrial application process and reducing costs. Studies have shown that by regulating the loading of different transition metals and their oxides on the basis of foamed nickel, it can be applied to the treatment of various organic pollutants such as toluene and methyl mercaptan. However, this type of catalyst also has application defects, among which poor stability is one of the problems that need to be solved urgently. For example, Chinese patent application CN112221513A synthesized a manganese dioxide / nickel cobaltate @ nickel foam core-shell heterogeneous catalyst, but the inventors of this application found in previous experimental studies that its ozone catalytic degradation efficiency was limited and its stability was poor. The activity of the catalyst decreased significantly with the reaction time, which limited its application in actual industrial production. Therefore, how to efficiently improve the stability of the nickel foam-supported manganese oxide monolithic catalyst is one of the directions worthy of attention in future research. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art ozone catalyst with nickel foam as the base, and provide a NF@Ni(OH)2@MnO x The application of catalysts in the treatment of organic pollutants.
[0006] The purpose of the present invention is to provide a NF@Ni(OH)2@MnO x catalyst.
[0007] Another object of the present invention is to provide a method for degrading organic pollutants by ozone catalytic oxidation.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] A NF@Ni(OH)2@MnO x The application of catalyst in the field of treating organic pollutants, the NF@Ni(OH)2@MnO x The catalyst comprises a nickel foam NF substrate, a nickel hydroxide Ni(OH)2 layer supported on the substrate, and a manganese oxide MnO2 supported on the nickel hydroxide Ni(OH)2 layer.x ; wherein the NF@Ni(OH)2@MnO x The molar ratio of Ni to Mn in the catalyst is 0.07~4.30:1.
[0010] NF@Ni(OH)2@MnO of the present invention x The catalyst uses nickel foam (NF) material with high porosity and good mass transfer effect as the substrate, and then loads Ni(OH)2 intermediate active oxidation layer, so that the catalyst presents a wrinkled morphology with large specific surface area, which not only expands the MnO x The loading of MnO increases the adsorption sites of ozone. Ni(OH)2 acts as a unique electron shuttle layer to enhance the x The internal potential between NF and ozone promotes the activation of ozone into active oxygen species; and its larger interlayer space is conducive to the diffusion and mass transfer of molecules, so that the intermediate products produced during the catalytic degradation of organic pollutants can be quickly desorbed and migrated, avoiding the deactivation of the catalyst, thereby achieving efficient removal of organic pollutants.
[0011] Organic pollutants in the NF@Ni(OH)2@MnO x The MnO2 is adsorbed on the surface of the catalyst, and due to the presence of the intermediate Ni(OH)2 oxide layer, the catalyst presents a wrinkled morphology with a large specific surface area. x The loading capacity and adsorption sites of ozone increase, and ozone is rapidly activated into active oxygen species (•OH and •O2 − ), and then attack organic pollutants such as methyl mercaptan, causing them to be deeply mineralized into non-toxic products such as carbon dioxide and water. In addition, the larger interlayer space of Ni(OH)2 facilitates the diffusion and mass transfer of molecules, allowing the intermediate products produced during the degradation process to be quickly desorbed and migrated, avoiding the deactivation of the catalyst. The catalyst can continuously and stably activate ozone to produce active oxygen species to remove organic pollutants, and can maintain a high activity for a long time (stable operation for 720 min). The degradation rate of gaseous organic pollutants can reach more than 84%; the degradation effect of various organic pollutants in water bodies can reach more than 82%.
[0012] In the present invention, the source of the organic pollutants may be industrial waste gas or industrial waste water; wherein, industrial waste water includes printing and dyeing waste water, coal coking waste water, electroplating waste water, and pharmaceutical waste water.
[0013] Furthermore, the organic pollutants are one or more of alkane compounds, aromatic compounds, organic alcohol compounds, phenolic compounds, organic acids or antibiotics.
[0014] Preferably, the organic pollutants are one or more of methane, propane, n-hexane, benzene, toluene, xylene, methyl mercaptan, styrene, naphthalene, acetone, acetaminophen, chlorophenol, bisphenol A, ethylenediaminetetraacetic acid, citric acid, p-toluenesulfonic acid, ibuprofen (IBP), and sulfamethoxazole (SMX).
[0015] Furthermore, the NF@Ni(OH)2@MnO x The catalyst was prepared according to the following steps:
[0016] S1. Pretreating the nickel foam NF to remove oxide impurities on the surface of the NF;
[0017] S2. Mixing the nickel source, the precipitant and the NF obtained in S1 in water, performing a hydrothermal reaction, and post-treating to obtain a nickel foam NF@Ni(OH)2 loaded with a Ni(OH)2 layer;
[0018] S3. Mix the manganese source, oxidant or reductant, and NF@Ni(OH)2 prepared in S2 in water, perform hydrothermal reaction, and post-treat to obtain NF@Ni(OH)2@MnO x catalyst;
[0019] Wherein, the nickel source and the manganese source are added according to a molar ratio of 0.05-3:1;
[0020] The precipitant is a compound that can decompose to produce NH3.
[0021] The present invention utilizes the property of the precipitant to decompose and generate NH3 in a hydrothermal reaction to provide a suitable weakly alkaline environment to convert the nickel source into Ni(OH)2.
[0022] In the technical solution of the present invention, an oxidant or a reductant is added to the manganese source because the valence of manganese in the manganese source varies. High-valence manganese requires the addition of a reductant to reduce it, while low-valence manganese requires an oxidant to oxidize it.
[0023] Furthermore, the nickel source is one or more of NiCl2·6H2O, Ni(CH3COO)2·4H2O, Ni(NO3)2·6H2O or NiSO4·7H2O.
[0024] Furthermore, the manganese source is one or more of KMnO4, MnSO4 or MnCl2.
[0025] Furthermore, the oxidant is (NH4)2S2O8 or KMnO4; the reducing agent is (NH4)2C2O4 or (NH4)2SO4.
[0026] Preferably, the precipitant is urea or ammonium carbonate.
[0027] Furthermore, in step S2, the temperature of the hydrothermal reaction is 100-150°C, and the time of the hydrothermal reaction is 4-8 h; preferably, in step S2, the temperature of the hydrothermal reaction is 120°C, and the time of the hydrothermal reaction is 6 h.
[0028] Further, in step S3, the temperature of the hydrothermal reaction is 100-200 °C, and the time of the hydrothermal reaction is 8-24 h; preferably, in step S3, the temperature of the hydrothermal reaction is 100-180 °C, and the time of the hydrothermal reaction is 10-14 h; more preferably, in step S3, the temperature of the hydrothermal reaction is 180 °C, and the time of the hydrothermal reaction is 12 h.
[0029] Furthermore, in step S1, the nickel foam NF pretreatment specifically comprises the following steps: washing the nickel foam with acetone, hydrochloric acid and deionized water in sequence, drying and setting aside.
[0030] Furthermore, the post-treatment is washing three times with deionized water after cooling to room temperature and drying.
[0031] Preferably, in step S2, the dosages of the nickel source and the precipitant are 1.25-75 mmol / L and 10-600 mmol / L, respectively.
[0032] More preferably, in step S2, the dosages of the nickel source and the precipitant are 6.25 mmol / L and 50 mmol / L respectively.
[0033] Preferably, in step S3, the dosage of the manganese source is 2.5-250 mmol / L; the dosage of the oxidant or reductant is 1.25-125 mmol / L.
[0034] More preferably, in step S3, the dosage of the manganese source is 25 mmol / L, and the dosage of the oxidant or reductant is 12.5 mmol / L.
[0035] At the same time, the present invention also provides a NF@Ni(OH)2@MnO x The catalyst, the NF@Ni(OH)2@MnO x The catalyst comprises a nickel foam NF substrate, nickel hydroxide Ni(OH)2 supported on the substrate, and manganese oxide MnO2 supported on the nickel hydroxide Ni(OH)2 layer. x ;
[0036] The NF@Ni(OH)2@MnO x The catalyst was prepared according to the following method:
[0037] S1. The nickel foam NF is pretreated to remove oxide impurities on the surface of the NF and dried for later use;
[0038] S2. Mixing the nickel source, the precipitant and the NF obtained in S1 in water, performing a hydrothermal reaction, and post-treating to obtain a nickel foam NF@Ni(OH)2 loaded with a Ni(OH)2 oxide layer;
[0039] S3. Mix the manganese source, oxidant or reductant, and NF@Ni(OH)2 prepared in S2 in water, perform hydrothermal reaction, and post-treat to obtain NF@Ni(OH)2@MnO x catalyst;
[0040] Wherein, the nickel source and the manganese source are added according to a molar ratio of 0.05-0.25:1;
[0041] The precipitant is a compound that can decompose to produce NH3.
[0042] The present invention adds a nickel source and a manganese source according to a specific mass ratio to prepare NF@Ni(OH)2@MnO x The catalyst has high ozone catalytic activity. In the application example, a mixed gas with an initial concentration of 40 ppm of the organic pollutant methyl mercaptan was input into the device, the gas flow rate was controlled at 0.15 L / min, the reaction time was 60 min, and the final degradation rate of methyl mercaptan was 100%.
[0043] In addition, the present invention provides a method for degrading organic pollutants by ozone catalytic oxidation, which comprises the following steps: x Catalyst mixture; wherein the NF@Ni(OH)2@MnO x The catalyst is nickel foam NF, which first loads nickel hydroxide Ni(OH)2 intermediate oxide layer and then loads manganese oxide MnO x .
[0044] Wherein, the source of the pollutants is industrial waste gas or industrial waste water.
[0045] Furthermore, in the method, the concentration of ozone is 1.7~7.7 mg / L, and the gas flow rate is controlled at 0.10~0.2 L / min; further, the initial concentration of organic pollutants in the industrial wastewater is 40~100 ppm; the initial concentration of organic pollutants in the industrial wastewater is 40~100 mg / L.
[0046] The present invention has the following beneficial effects:
[0047] (1) The monolithic catalyst NF@Ni(OH)2@MnO xIt has good application effect in the field of treating organic pollutants. NF@Ni(OH)2@MnO x Catalytic ozone produces active oxygen species that convert organic pollutants into non-toxic small molecules such as water and carbon dioxide. The degradation rate of gaseous organic pollutants can reach more than 84%, and it can operate stably for 720 minutes. At the same time, it can maintain good catalytic activity in an environment with a humidity of 0-60%. At the same time, the degradation effect of various organic pollutants in water bodies can reach more than 82%. It makes up for the defect of low stability of existing integral catalysts. While improving the removal effect of organic pollutants, it can avoid frequent replacement of catalysts, extend the service life, and expand the potential for practical application.
[0048] (2) The monolithic catalyst NF@Ni(OH)2@MnO x Compared with powdered catalysts, it has the advantages of relatively simple preparation, easy recovery, and feasible regeneration, and is more suitable for actual industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 NF@0.25-Ni(OH)2@MnO of Example 1 x Sample picture of the monolithic catalyst.
[0050] Figure 2 NF@0.25-Ni(OH)2@MnO of Example 1 x Scanning electron microscopy image of the monolithic catalyst.
[0051] Figure 3 For the application example NF@0.25-Ni(OH)2@MnO x Schematic diagram of the catalytic oxidation system of the overall catalyst combined with ozone.
[0052] Figure 4 NF@0.25-Ni(OH)2@MnO of Example 1 x XRD pattern of the monolithic catalyst, where Figure 4 (a) is NF@0.25-Ni(OH)2@MnO x XRD pattern of monolithic catalyst, Figure 3 (b) is the XRD pattern of various powdered materials collected during the preparation process.
[0053] Figure 5 The figures are effect diagrams of catalytic ozone purification of methyl mercaptan by Example 1, Example 4, Example 5, Comparative Examples 1 to 8 and ozone alone.
[0054] Figure 6 This is the degradation effect diagram of Application Example 3. DETAILED DESCRIPTION
[0055] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0056] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0057] Example 1 NF@0.25-Ni(OH)2@MnO x Preparation
[0058] A nickel foam loaded with Ni(OH)2 intermediate oxide layer and then loaded with MnO x The monolithic catalyst is prepared by the following steps:
[0059] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0060] S2. 0.5 mmol NiCl2·6H2O and 4 mmol urea were ultrasonically homogenized in 80 mL deionized water, and the NF obtained in S1 was placed in the mixture for hydrothermal reaction at 120 °C for 6 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain nickel foam NF@Ni(OH)2 with a Ni(OH)2 oxide layer.
[0061] S3. 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 were mixed with NF@Ni(OH)2 prepared in S2 in 80 mL water, and subjected to ultrasonication for 10 min. The mixture was hydrothermally reacted at 180 °C for 12 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain NF@0.25-Ni(OH)2@MnO. x (0.25 represents the value of the amount of nickel source added substance / the amount of manganese source added substance).
[0062] Example 2 NF@0.25-Ni(OH)2@MnO x Preparation
[0063] A nickel foam loaded with Ni(OH)2 intermediate oxide layer and then loaded with MnO x The monolithic catalyst is prepared by the following steps:
[0064] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0065] S2. 0.5 mmol NiCl2·6H2O and 4 mmol urea were ultrasonically homogenized in 80 mL deionized water, and the NF obtained in S1 was placed in the mixture for hydrothermal reaction at 120 °C for 6 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain nickel foam NF@Ni(OH)2 with a Ni(OH)2 oxide layer.
[0066] S3. 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 were mixed with NF@Ni(OH)2 prepared in S2 in 80 mL water, and subjected to ultrasonication for 10 min, followed by hydrothermal reaction at 140 °C for 12 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain NF@0.25-Ni(OH)2@MnO x (0.25 represents the value of the amount of nickel source added substance / the amount of manganese source added substance).
[0067] Compared with Example 1, the difference is that the hydrothermal reaction temperature of step S3 is 140° C., and the other preparation conditions and methods are the same.
[0068] Example 3 NF@0.25-Ni(OH)2@MnO x Preparation
[0069] A nickel foam loaded with Ni(OH)2 intermediate oxide layer and then loaded with MnO x The monolithic catalyst is prepared by the following steps:
[0070] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0071] S2. 0.5 mmol NiCl2·6H2O and 4 mmol urea were ultrasonically homogenized in 80 mL deionized water, and the NF obtained in S1 was placed in the mixture for hydrothermal reaction at 120 °C for 6 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain nickel foam NF@Ni(OH)2 with a Ni(OH)2 oxide layer.
[0072] S3. 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 were mixed with NF@Ni(OH)2 prepared in S2 in 80 mL water, and subjected to ultrasonic treatment for 10 min. The mixture was hydrothermally reacted at 100 °C for 12 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain NF@0.25-Ni(OH)2@MnO x (0.25 represents the value of the amount of nickel source added substance / the amount of manganese source added substance).
[0073] Compared with Example 1, the difference is that the hydrothermal reaction temperature of step S3 is 100° C., and the other preparation conditions and methods are the same.
[0074] Example 4 NF@3-Ni(OH)2@MnO x Preparation
[0075] A nickel foam loaded with Ni(OH)2 intermediate oxide layer and then loaded with MnO x The monolithic catalyst is prepared by the following steps:
[0076] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0077] S2. 6 mmol NiCl2·6H2O and 48 mmol urea were ultrasonically homogenized in 80 mL deionized water, and the NF obtained in S1 was placed in the mixture for hydrothermal reaction at 120 °C for 6 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain nickel foam NF@Ni(OH)2 with a Ni(OH)2 oxide layer.
[0078] S3. 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 were mixed with NF@Ni(OH)2 prepared in S2 in 80 mL water, and subjected to ultrasonication for 10 min, followed by hydrothermal reaction at 180 °C for 12 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain NF@3-Ni(OH)2@MnO x (3 represents the value of the amount of nickel source added substance / the amount of manganese source added substance).
[0079] Compared with Example 1, the difference is that the ratio of the added nickel source to the manganese source is 3:1, and the other preparation conditions and methods are the same.
[0080] Example 5 NF@0.05-Ni(OH)2@MnO x Preparation
[0081] A nickel foam loaded with Ni(OH)2 intermediate oxide layer and then loaded with MnO x The monolithic catalyst is prepared by the following steps:
[0082] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0083] S2. 0.1 mmol NiCl2·6H2O and 0.8 mmol urea were ultrasonically homogenized in 80 mL deionized water, and the NF obtained in S1 was placed in the mixture for hydrothermal reaction at 120 °C for 6 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain nickel foam NF@Ni(OH)2 with a Ni(OH)2 oxide layer.
[0084] S3. 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 were mixed with NF@Ni(OH)2 prepared in S2 in 80 mL water, and subjected to ultrasonication for 10 min. The mixture was hydrothermally reacted at 180 °C for 12 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain NF@0.05-Ni(OH)2@MnO. x (0.05 represents the value of the amount of nickel source added / the amount of manganese source added).
[0085] Compared with Example 1, the difference is that the ratio of the added nickel source to the manganese source is 0.05:1, and the other preparation conditions and methods are the same.
[0086] Comparative Example 1 Preparation of NF
[0087] A nickel foam monolithic catalyst, the preparation method steps are as follows:
[0088] The nickel foam with a shape of 2 cm×4 cm was washed with acetone, hydrochloric acid and deionized water to remove the surface oxide, and then placed in a 70 ℃ oven for 12 h to obtain NF.
[0089] Comparative Example 2 Preparation of NF@Ni(OH)2
[0090] A method for preparing a monolithic catalyst of nickel foam loaded Ni(OH)2 is as follows:
[0091] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0092] S2. 0.5 mmol NiCl2·6H2O and 4 mmol urea were ultrasonically homogenized in 80 mL deionized water, and the NF obtained in S1 was put into the mixture for hydrothermal reaction at 120 °C for 6 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain nickel foam NF@Ni(OH)2 with a Ni(OH)2 oxide layer.
[0093] Comparative Example 3 NF@MnO x Preparation
[0094] A kind of nickel foam loaded with MnO x The preparation method of the monolithic catalyst is as follows:
[0095] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0096] S2. 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 were homogenized in 80 mL deionized water and then the NF obtained in S1 was added for hydrothermal reaction at 180 °C for 12 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain NF@MnO x .
[0097] Comparative Example 4 Ni(OH)2@MnO x Preparation
[0098] A method for in-situ oxidation of nickel foam to Ni(OH)2 and then loading MnO x The preparation method is as follows:
[0099] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0100] S2. The NF prepared in S1 was placed in a sodium hydroxide solution (concentration of 1 mol / L), reacted for 30 min, washed three times with deionized water, and then dried at 70 °C for 12 h;
[0101] S3. The sample prepared in S2 was mixed with 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 in 80 mL water, and subjected to ultrasonication for 10 min, followed by hydrothermal reaction at 180 °C for 12 h. After cooling to room temperature, it was washed three times with deionized water and then dried at 70 °C for 12 h to obtain Ni(OH)2@MnO x .
[0102] In this comparative example, no nickel source is added externally, and the foamed nickel and the manganese source are directly subjected to hydrothermal reaction.
[0103] Comparative Example 5 NF@MnO x Preparation of @0.25-Ni(OH)2
[0104] A nickel foam first loaded with MnO x The monolithic catalyst loaded with Ni(OH)2 is prepared by the following steps:
[0105] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0106] S2. After 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 were homogenized in 80 mL deionized water, the NF obtained in S1 was placed in the mixture and subjected to hydrothermal reaction at 180 °C for 12 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h.
[0107] S3. 0.5 mmol NiCl2·6H2O and 4 mmol urea were added to the MnO prepared in S2. x The nickel foam was mixed in 80 mL of water, ultrasonicated for 10 min, and then hydrothermally reacted at 120 °C for 6 h. After cooling to room temperature, it was washed three times with deionized water and then dried at 70 °C for 12 h to obtain NF@MnO. x @0.25-Ni(OH)2 (0.25 represents the value of the amount of nickel source added / the amount of manganese source added).
[0108] The difference between this comparative example and Example 1 is that this comparative example first loads MnO x Then Ni(OH)2 is loaded. In Example 1, Ni(OH)2 is loaded first and then MnO x , the rest of the experimental parameters were the same.
[0109] Comparative Example 6 NF@0.25-Co(OH)2@MnO x Preparation
[0110] A nickel foam loaded with Co(OH)2 intermediate oxide layer and then loaded with MnO x The monolithic catalyst is prepared by the following steps:
[0111] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0112] S2. 0.5 mmol CoCl2·6H2O and 4 mmol urea were ultrasonically homogenized in 80 mL deionized water, and the NF obtained in S1 was placed in the mixture for hydrothermal reaction at 120 °C for 6 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain nickel foam NF@Co(OH)2 with a Co(OH)2 oxide layer.
[0113] S3. 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 were mixed with NF@Co(OH)2 prepared in S2 in 80 mL water, and then subjected to ultrasonication for 10 min, hydrothermally reacted at 180 °C for 12 h, cooled to room temperature, washed three times with deionized water, and then dried at 70 °C for 12 h to obtain NF@0.25-Co(OH)2@MnO x (0.25 represents the value of the amount of nickel source added substance / the amount of manganese source added substance).
[0114] The difference between this comparative example and Example 1 is that NiCl2·6H2O is replaced by CoCl2·6H2O in step S1, and the remaining experimental steps and parameters are consistent with those in Example 1.
[0115] Comparative Example 7 NF@0.25-FeOOH@MnO x Preparation
[0116] A nickel foam loaded with FeOOH intermediate oxide layer and then loaded with MnO x The monolithic catalyst is prepared by the following steps:
[0117] S1. Wash the nickel foam (NF) with a shape of 2 cm × 4 cm with acetone, hydrochloric acid, and deionized water in turn, and place it in an oven at 70 °C for 12 h for later use;
[0118] S2. 0.5 mmol FeCl2·4H2O and 4 mmol urea were ultrasonically homogenized in 80 mL deionized water, and the NF obtained in S1 was placed in the mixture for hydrothermal reaction at 120 °C for 6 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain nickel foam NF@FeOOH with a FeOOH oxide layer.
[0119] S3. 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 were mixed with NF@FeOOH prepared in S2 in 80 mL water, and subjected to ultrasonication for 10 min, followed by hydrothermal reaction at 180 °C for 12 h. After cooling to room temperature, the mixture was washed three times with deionized water and then dried at 70 °C for 12 h to obtain NF@0.25-FeOOH@MnO x (0.25 represents the value of the amount of nickel source added substance / the amount of manganese source added substance).
[0120] The difference between this comparative example and Example 1 is that NiCl2·6H2O is replaced by FeCl2·4H2O in step S1, and the remaining experimental steps and parameters are consistent with those in Example 1.
[0121] Comparative Example 8 Powder MnO x Preparation
[0122] S1. Add 2 mmol KMnO4 and 1 mmol (NH4)2C2O4 to 80 mL of deionized water, mix them evenly under ultrasonication, and then transfer the mixed solution to a hydrothermal reactor for hydrothermal reaction. The temperature was controlled at 180 °C and the reaction time was 12 h.
[0123] S2. Collect the sample after the reaction in S1, wash the impurities on the surface with deionized water and filter it, then place it in a 70 ℃ oven for 12 h to obtain powdered MnO x .
[0124] Comparative Example 9 NF@NiCo2O4@MnO x Preparation
[0125] Comparative Example 9 was synthesized according to the prior art: preparation method of manganese dioxide / nickel cobaltate@nickel foam core-shell heterogeneous catalyst (Chinese patent application: CN112221513A).
[0126] A nickel foam loaded with NiCo2O4 intermediate oxide layer and then loaded with MnO x The monolithic catalyst is prepared by the following steps:
[0127] S1. Wash the nickel foam of 2 cm×4 cm with acetone, hydrochloric acid and deionized water in turn, add 4 mmol Ni(NO)3·6H2O, 8 mmol Co(NO)3·6H2O and 24 mmol urea to 80 mL of a mixed solution of deionized water and anhydrous ethanol in a volume ratio of 1:1, place the nickel foam in it after ultrasonic homogenization, and transfer it to a hydrothermal reactor for hydrothermal reaction at a temperature of 120 ℃ for 8 h.
[0128] S2. The nickel foam with NiCo2O4 layer in S1 was placed in 80 mL solution of 2 mmol KMnO4 and 1 mmol (NH4)2C2O4. After ultrasonic treatment for 10 min, it was transferred to a reactor for hydrothermal reaction at 180 °C for 12 h.
[0129] S3. After the reaction in S2 was completed, the sample was washed with deionized water to remove impurities on the surface, and then dried in an oven at 70 °C for 12 h to obtain NF@NiCo2O4@MnO x .
[0130] Structural characterization and preparation process
[0131] Experimental materials: NF@0.25-Ni(OH)2@MnO prepared in Example 1 x Monolithic catalyst.
[0132] from Figure 1 It can be seen that the NF@0.25-Ni(OH)2@MnO x The monolithic catalyst is a 2 cm × 4 cm sheet with a rough surface and a flexible structure. Black matter (MnO x ) are evenly dispersed on the surface of the carrier.
[0133] from Figure 2 It can be seen that the NF@0.25-Ni(OH)2@MnO x The monolithic catalyst retains the pore structure of nickel foam NF, and the pore wall is rough and wrinkled, which is attributed to the Ni(OH)2 and MnO x The uniform dispersion of Ni(OH)2 array also avoids the flower-like MnO x Excessive aggregation on the pore wall of nickel foam. In addition, the EDS energy spectrum analysis results of the scanning electron microscope roughly determined the molar ratio of Ni and Mn in the catalysts prepared in Example 1, Example 4 and Example 5, which were specifically 0.36, 4.30 and 0.07, respectively. Since there is also nickel foam in the catalyst, it has a certain influence on the determination result of the nickel element, that is, there are two sources of Ni in the above test results (Ni(OH)2 and nickel foam), so the above data are only Ni(OH)2 and MnO in the catalyst. x The loading capacity was semi-quantitatively analyzed, but from the results, the final Ni(OH)2 and MnO x The trend of the loading amount is consistent with the ratio trend of the initial nickel source and manganese source addition, which is consistent with the expectations of the experimental design and the differences in experimental performance. x Successful loading on nickel foam.
[0134] Figure 3 The reaction device of the catalytic ozone oxidation system described in the present invention places a catalyst in a reactor, and controls the flow rates of air, ozone, methyl mercaptan, and water vapor to input a mixed gas of a certain concentration. The mixed gas first enters the reactor containing the catalyst through a sensor S1 (monitoring the concentration of methyl mercaptan). After the catalytic reaction, the remaining gas flows out, and the concentration of methyl mercaptan after catalytic degradation is monitored by a sensor S2.
[0135] Figure 4 The NF@0.25-Ni(OH)2@MnO x Monolithic catalyst ( Figure 4 (a)) and various powdered materials collected during the preparation process ( Figure 4 XRD spectrum of (b) in Figure 2. As shown in the figure, Ni(OH)2@MnO xDifferent peaks are shown at 12.8°, 18.1°, 28.7°, 38.9°, 42.1°, 49.9°, and 60.2°, corresponding to the diffraction planes of (110), (200), (130), (211), (301), (141), and (251), respectively (PDF#97−002-0227), while the characteristic peaks at 33.5° and 61.3° can be attributed to the (101) and (110) planes of Ni(OH)2.
[0136] Application Example 1
[0137] Experimental materials: monolithic catalysts prepared in Examples 1 to 5 and Comparative Examples 1 to 8.
[0138] Experimental method: The monolithic catalyst samples of Examples 1 to 5 and Comparative Examples 1 to 8 were placed in a methyl mercaptan degradation reaction device, and a mixed gas with an initial methyl mercaptan concentration of 40 ppm was input from the inlet end to the device through an ozone and methyl mercaptan generator. The gas flow rate was controlled at 0.15 L / min, and the reaction time was 60 min. The catalyst was used to decompose ozone, generate various active oxygen species to degrade organic pollutants such as methyl mercaptan, and convert them into non-toxic small molecules such as carbon dioxide and water. A methyl mercaptan detector was installed at the inlet end and the outlet end to measure the initial concentration and emission concentration of methyl mercaptan. The degradation rate was calculated by the following formula to evaluate the degradation effect of different catalysts on methyl mercaptan in the catalytic ozone oxidation system:
[0139] Formula 1
[0140] In formula 1: R is the degradation efficiency of organic pollutants; C0 is the initial concentration of organic pollutants at the inlet end (ppm); C t is the concentration of organic pollutants at the outlet (ppm).
[0141] Experimental results: The degradation of methyl mercaptan in Application Example 1 is shown in Table 1. Figure 5 As shown in Table 1 and Figure 5 The data clearly show that the NF@Ni(OH)2@MnO prepared in this embodiment of the present invention x The degradation efficiency of the monolithic catalyst for methyl mercaptan is much higher than that of the catalyst materials in Comparative Examples 1 to 8, and it has a significant purification effect on organic pollutants. It is worth noting that when the ratio of the amount of nickel source to manganese source added is 0.25, the amount of MnO prepared is 0. x The material obtained when the hydrothermal temperature is 180°C, that is, Example 1, has the best effect on catalytic ozone degradation of methyl mercaptan, with a degradation rate close to 100%. x The order of loading of MnO and Ni(OH)2 can be seen from the experimental results. xThe catalyst material prepared by loading Ni(OH)2 (Comparative Example 5) is similar to the catalyst material prepared by loading Ni(OH)2 first and then MnO under the same experimental conditions. x Compared with the catalyst material prepared by (Example 1), the degradation rate of methyl mercaptan catalyzed by ozone was reduced by 19.8%; while the degradation rate of methyl mercaptan catalyzed by ozone was significantly reduced by 56.7% and 62.1% compared with Example 1 by the catalyst material prepared by intermediate loading Co(OH)2 (Comparative Example 6) and FeOOH (Comparative Example 7). The above experimental results show that only the nickel foam loaded with Ni(OH)2 intermediate oxide layer and then loaded with MnO x The monolithic catalyst has a better ozone catalytic degradation effect. The present invention utilizes Ni(OH)2 and MnO x The synergistic effect of the catalyst can enhance the ozone catalytic degradation effect, replace the Ni(OH)2 intermediate oxide layer or change the Ni(OH)2, MnO x The loading order of the catalyst will significantly reduce the ozone catalytic degradation effect.
[0142] Table 1 Degradation efficiency test results
[0143]
[0144] Application Example 2
[0145] Experimental materials: NF@0.25-Ni(OH)2@MnO prepared in Example 1 x Monolithic catalyst.
[0146] Experimental method: NF@0.25-Ni(OH)2@MnO prepared in Example 1 x The sample was placed in a methyl mercaptan degradation device, and a mixed gas of methyl mercaptan, ozone and water vapor was formed in the device through ozone, methyl mercaptan and water vapor generators. The degradation of methyl mercaptan by the catalyst was measured under different humidity conditions (0%, 10%, 30%, 60%), and the humidity resistance of the catalyst sample of Example 1 was evaluated.
[0147] Experimental results: The degradation of methyl mercaptan in Application Example 2 is shown in Table 2. As can be seen from Table 2, the monolithic catalyst NF@0.25-Ni(OH)2@MnO x It exhibits excellent catalytic ozonation performance in degrading methyl mercaptan under various humidity conditions, has strong moisture resistance, is suitable for a variety of environmental conditions, and can be widely used in the removal of gaseous organic pollutants.
[0148] Table 2 Humidity resistance test results
[0149]
[0150] Application Example 3
[0151] Experimental materials: monolithic catalysts prepared in Example 1, Comparative Example 3 and Comparative Example 9.
[0152] Experimental method: The catalyst samples prepared in Example 1, Comparative Example 3 and Comparative Example 9 were placed in a methyl mercaptan degradation device, and a mixed gas with an initial methyl mercaptan concentration of 40 ppm was input into the device through ozone and a methyl mercaptan generator. The gas flow rate was controlled at 0.15 L / min, and the reaction time was 720 min. The degradation stability of the catalyst was tested.
[0153] Experimental results: From Figure 6 It can be seen that the NF@0.25-Ni(OH)2@MnO prepared in Example 1 of the present application x The catalytic ozone oxidation degradation of methyl mercaptan is relatively good; the degradation stability is relatively high, the reaction can continue for 720 min, and the catalytic activity does not decrease significantly, which is significantly better than that of comparative example 3 (NF@MnO x ) and Comparative Example 9. The above results show that the monolithic catalyst NF@0.25-Ni(OH)2@MnO x The stability during the degradation process is significantly better than existing technologies or materials, and represents a significant technological advancement.
[0154] Application Example 4
[0155] Experimental materials: NF@0.25-Ni(OH)2@MnO prepared in Example 1 x .
[0156] Experimental method: In order to expand the application field of the catalyst of the present invention, NF@0.25-Ni(OH)2@MnO prepared in Example 1 of the present application was used. x Used to catalyze the degradation of pollutants in different industrial wastewaters. Various pollutants present in printing and dyeing wastewater, coal coking wastewater, electroplating wastewater, pharmaceutical wastewater and other water bodies were selected for degradation, namely acetaminophen (ACT), 4-chlorophenol (4-CP), bisphenol A (BPA), ethylenediaminetetraacetic acid (EDTA), citric acid (CA), p-toluenesulfonic acid (p-TSA), ibuprofen (IBP), sulfamethoxazole (SMX). For each group of experiments, the flake NF@0.25-Ni(OH)2@MnO xIt was fixed vertically in the middle of the reactor, and 100 mL of simulated wastewater (pollutant concentration of 50.0 mg / L, pH=7.0) was added to it. Ozone with a concentration of 1.5 mg / L was continuously bubbled into the water body using an ozone generator at a flow rate of 200 mL / min, and the concentration of gaseous ozone was continuously monitored by an online ozone analyzer. After 15 minutes of reaction, 3 mL of sample was taken from the reaction solution and immediately purged with N2 to remove residual ozone. The concentration of pollutants was determined by high performance liquid chromatography (HPLC) to evaluate the degradation effect of different pollutants.
[0157] Experimental results: The degradation of different water pollutants in Application Example 4 is shown in Table 3. It can be seen that the NF@0.25-Ni(OH)2@MnO prepared in Example 1 of the present application x It also has a good effect on catalytic ozone degradation of different pollutants in water. This result shows that the catalyst described in this application has a wide range of applications and has good prospects and universality.
[0158] Table 3 Degradation effects of different pollutants in wastewater
[0159]
[0160] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A NF@Ni(OH)2@MnO x The application of the catalyst in the ozone catalytic oxidation degradation of organic pollutants is characterized in that: The NF@Ni(OH)2@MnO x The catalyst comprises a nickel foam NF substrate, a nickel hydroxide Ni(OH)2 layer supported on the substrate, and a manganese oxide MnO2 supported on the nickel hydroxide Ni(OH)2 layer. x ; The NF@Ni(OH)2@MnO x The catalyst was prepared according to the following steps: S1. Pretreating the nickel foam NF to remove oxide impurities on the surface of the NF; S2. Mixing the nickel source, the precipitant and the NF obtained in S1 in water, performing a hydrothermal reaction, and post-treating to obtain a nickel foam NF@Ni(OH)2 loaded with a Ni(OH)2 layer; S3. Mix the manganese source, oxidant or reductant, and NF@Ni(OH)2 prepared in S2 in water, perform hydrothermal reaction, and post-treat to obtain NF@Ni(OH)2@MnO x catalyst; Wherein, the nickel source and the manganese source are added according to a molar ratio of 0.05-3:1; The precipitant is urea or ammonium carbonate; The organic pollutants are one or more of methyl mercaptan, acetaminophen, 4-chlorophenol, bisphenol A, p-toluenesulfonic acid, ibuprofen, and sulfamethoxazole.
2. The application according to claim 1, characterized in that: The nickel source is one or more of NiCl2·6H2O, Ni(CH3COO)2·4H2O, Ni(NO3)2·6H2O or NiSO4·7H2O.
3. The application according to claim 1, characterized in that: The manganese source is one or more of KMnO4, MnSO4 or MnCl2.
4. The use according to claim 1, characterized in that: The oxidizing agent is (NH4)2S2O8 or KMnO4; the reducing agent is (NH4)2C2O4.
5. The use according to claim 1, characterized in that: In step S2, the temperature of the hydrothermal reaction is 100-150° C., and the time of the hydrothermal reaction is 4-8 h.
6. The use according to claim 1, characterized in that: In step S3, the temperature of the hydrothermal reaction is 100-200° C., and the time of the hydrothermal reaction is 8-24 h.
7. A method for degrading organic pollutants by ozone catalytic oxidation, characterized in that: The specific steps are: organic pollutants, ozone and NF@Ni(OH)2@MnO x Catalyst mixture; wherein the NF@Ni(OH)2@MnO x The catalyst is nickel foam NF, which first loads nickel hydroxide Ni(OH)2 intermediate oxide layer and then loads manganese oxide MnO x ; The NF@Ni(OH)2@MnO x The catalyst was prepared according to the following steps: S1. Pretreating the nickel foam NF to remove oxide impurities on the surface of the NF; S2. Mixing the nickel source, the precipitant and the NF obtained in S1 in water, performing a hydrothermal reaction, and post-treating to obtain a nickel foam NF@Ni(OH)2 loaded with a Ni(OH)2 layer; S3. Mix the manganese source, oxidant or reductant, and NF@Ni(OH)2 prepared in S2 in water, perform hydrothermal reaction, and post-treat to obtain NF@Ni(OH)2@MnO x catalyst; Wherein, the nickel source and the manganese source are added according to a molar ratio of 0.05-3:1; The precipitant is urea or ammonium carbonate; The organic pollutants are one or more of methyl mercaptan, acetaminophen, 4-chlorophenol, bisphenol A, p-toluenesulfonic acid, ibuprofen, and sulfamethoxazole.