Catalyst for synthesizing single-walled carbon nanotube, preparation method and preparation device

By combining iron-based metal elements and tellurium elements on the graphene carrier, and using hydrothermal and microwave plasma reduction technology, the problem of catalyst fusion at high temperatures is solved, and high-quality single-walled carbon nanotubes can be efficiently prepared and costs reduced. and improved productivity.

CN118698566AActive Publication Date: 2024-09-27NINGBO XENWO NEW MATERIAL TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410651818.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-09-27
Estimated Expiration
2044-05-24

AI Technical Summary

Technical Problem

In the existing technology, single-walled carbon nanotube catalysts are easy to fuse under high temperature conditions, resulting in a decrease in catalytic activity, and the porous carrier is difficult to remove, which increases the preparation cost.

Method used

Iron-based metal elements are combined with Group VI tellurium elements and distributed on the surface of the graphene carrier. Gas is released through the hydrothermal reduction process to prevent the metal particles from agglomerating. Microwave plasma reduction is used to form uniform catalyst particles. Single-walled materials are prepared using chemical vapor deposition. Carbon nanotubes.

Benefits of technology

The high-temperature stability and activity maintenance of the catalyst particles are achieved, the preparation process is simplified, the cost is reduced, and the quality and yield of single-walled carbon nanotubes are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118698566A
    Figure CN118698566A
Patent Text Reader

Abstract

The invention relates to a catalyst for synthesizing a single-walled carbon nanotube, a preparation method and a preparation device, the catalyst comprises an iron-based metal element, a tellurium element and graphene, the molar content of the iron-based metal element is 85-98%, the molar content of the tellurium element is 1-5%, the molar content of carbon in the graphene is 1-10%, and the molar content of carbon in the graphene is 1-10%. The particle size of the catalyst is 10 to 40 nm; according to the scheme, the catalyst particles which are uniform in size and high in activity are prepared from the iron-based metal element and the VI-group tellurium element and are distributed on the surface of the graphene carrier, and the ultrahigh specific surface area of graphene is utilized, so that the catalyst particles and the graphene carrier form relatively strong binding force; and gas released by the graphite oxide in the hydrothermal reduction process can prevent metal particles attached to the surface of the graphene oxide from being agglomerated, and the metal particles are not easy to melt in the cracking reaction process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of single-walled carbon nanotubes, and in particular to a catalyst, a preparation method and a preparation device for synthesizing single-walled carbon nanotubes. Background Art

[0002] As a new type of one-dimensional nanomaterial, single-walled carbon nanotubes (SWCNTs or SWCNT or SWNT) are widely used in new energy, transparent display, antistatic, semiconductor, engineering plastics and other fields due to their excellent electrical conductivity, thermal conductivity, temperature resistance, chemical resistance and mechanical properties. However, the batch preparation technology of SWCNTs has always restricted its application in various fields. Therefore, how to achieve low-cost and scalable preparation of high-quality SWCNTs is an urgent problem to be solved.

[0003] At present, there are three main methods for preparing single-walled carbon nanotubes: arc method, laser ablation method and chemical vapor deposition method. The growth process of SWCNTs is as follows: carbon source molecules are cracked into highly active carbon atoms at high temperature on the catalyst surface, and then dissolved and diffused on the surface or bulk of the catalyst particles. When the carbon in the catalyst is saturated, carbon atoms precipitate on the surface of the catalyst particles to form SWCNTs.

[0004] Highly active nanoscale catalysts are the key factor in the successful preparation of high-quality single-walled carbon nanotubes. During the synthesis of SWCNTs, it is necessary to maintain the stability of the active components of the catalyst and prevent the catalyst particles from fusing into agglomerates, so as to effectively obtain SWCNTs with uniform diameter and large aspect ratio. In the patent application document with publication number CN117643893A, a multi-component catalyst is prepared by mixing, drying, calcining and other processes using raw materials such as metal catalyst salt, complexing agent and surfactant. Under the action of surfactant, the catalyst has a nanometer size, which ensures the high activity of the catalyst. However, in the subsequent catalytic reaction process, this nanoscale catalyst inevitably melts under high temperature conditions, resulting in a decrease in catalyst activity. In addition, porous materials such as zeolite and mesoporous silica are commonly used as catalyst carriers in the prior art. Although the porous structure plays a role in limiting the size of the catalyst, the zeolite and mesoporous silica carriers are difficult to remove, which brings certain inconveniences to the application of carbon nanotubes. In the patent documents with publication number CN116159566A and announcement number CN 114797864B, a carrier template is introduced in the catalyst preparation process to prevent the melting of the metal catalyst under high temperature conditions, but the introduced template increases the cost of subsequent purification and separation processes.

[0005] Therefore, it is urgent to develop an efficient single-walled carbon nanotube catalyst and an efficient preparation method thereof to improve the problems existing in the above-mentioned prior art. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the present application provides a catalyst for synthesizing single-walled carbon nanotubes, which is prepared by using iron-based metal elements and group VI tellurium elements and is uniform in size and highly active. The catalyst particles are distributed on the surface of a graphene carrier, and the ultra-high specific surface area of ​​the graphene is used to form a strong binding force with the catalyst particles. The gas released by the graphene oxide during the hydrothermal reduction process can prevent the metal particles attached to the surface of the graphene oxide from agglomerating, and makes it less likely for the metal particles to fuse during the cracking reaction.

[0007] In order to solve the above technical problems, the technical solution adopted in the present application is: a catalyst for synthesizing single-walled carbon nanotubes, the catalyst comprising iron-based metal elements, tellurium elements and graphene, wherein the molar content of the iron-based metal elements is 85-98%, the molar content of the tellurium elements is 1-5%, the molar content of carbon in the graphene is 1-10%, and the size of the catalyst particles is 10-40nm.

[0008] Furthermore, the molar content of the iron-based metal element is 88-95%, the molar content of the tellurium element is 2-4%, and the molar content of carbon in the graphene is 4-7% (the sum of the molar contents of the above components satisfies 100%).

[0009] Furthermore, the graphene is a single-layer or multi-layer structure with a specific surface area of ​​300 to 1000 m 2 / g, and the flake diameter is 50 to 500 nm (graphene obtained by gradient centrifugation can be used).

[0010] Furthermore, the specific surface area of ​​the graphene is 750 m 2 / g~1000m 2 / g, and the flake diameter is 100~300nm.

[0011] Furthermore, the iron-based metal element is one or more of iron, cobalt and nickel.

[0012] Furthermore, the iron-based metal elements are two or more of iron, cobalt and nickel.

[0013] Furthermore, the iron-based metal elements are iron and nickel or iron and cobalt, and the molar ratio of iron to cobalt or iron to nickel is 5 to 10:1.

[0014] Furthermore, the sources of the iron, cobalt and nickel are water-soluble compounds, such as one or more of sulfates, nitrates and acetates containing the above elements (which can be referred to as precursors containing iron-based metal elements).

[0015] Furthermore, the source material of the tellurium element is one of telluric acid or hypotelluric acid (which can be called a precursor containing the tellurium element).

[0016] Furthermore, the present invention also provides a method for preparing the above-mentioned catalyst for synthesizing single-walled carbon nanotubes, the steps comprising:

[0017] (1) weighing a precursor containing an iron-based metal element and a tellurium element and dissolving it in an aqueous solution of graphene oxide, adding ammonia water dropwise to the solution, and adjusting the pH to 8 to 10 to obtain a solution A;

[0018] (2) placing solution A in a reaction kettle, wherein the volume of solution A accounts for 60-80% of the volume of the reaction kettle; then hydrothermally reacting at 150° C.-200° C. for 10-12 hours; then cooling, centrifuging and drying to obtain a crude catalyst precursor B;

[0019] (3) ball-milling the crude catalyst precursor B, and then sieving it with a sieve to obtain a catalyst precursor C;

[0020] (4) placing the catalyst precursor C in a powder feeder, introducing argon and hydrogen at the gas inlet, turning on the microwave power supply to form microwave plasma in the reduction chamber, and then adding the catalyst precursor C into the reduction chamber through the powder feeder for a reduction reaction. After the reduction reaction, the catalyst precursor C is cooled. During the cooling process, the particles are shaped to form catalyst powders of uniform size.

[0021] Furthermore, the graphene oxide described in step (1) is a single-layer or multi-layer structure, with a sheet diameter of 50 to 500 nm and a specific surface area of ​​300 to 1000 m 2 / g (the reduction process of graphene oxide into graphene is a deoxidation process, which has little effect on the sheet diameter, so the raw material graphene oxide adopts the above specifications).

[0022] Furthermore, the iron-based metal element in step (1) is one or more of iron, cobalt and nickel.

[0023] Furthermore, the iron-based metal elements described in step (1) are two or more of iron, cobalt and nickel, and the most preferred are iron and nickel or iron and cobalt, with the molar ratio of iron to cobalt or iron to nickel being 5 to 10:1.

[0024] Furthermore, the precursor containing iron-based metal elements in step (1) may be nitrate, chloride, carbonate, sulfate or acetate of iron, cobalt or nickel.

[0025] Furthermore, the precursor containing iron-based metal elements in step (1) can be one or more of ferric chloride, cobalt chloride, nickel chloride, cobalt nitrate, nickel nitrate, ferric nitrate, ferric sulfate, nickel sulfate, and cobalt sulfate.

[0026] Furthermore, the molar content of carbon in the graphene oxide described in step (1) is 1-10%, the molar content of iron-based metal elements is 85-98%, and the molar content of tellurium in telluric acid or telluric acid is 1-5%.

[0027] Furthermore, the carbon molar content of the graphene oxide described in step (1) is 4-7%, the molar content of the iron-based metal element is 88-95%, and the molar content of the tellurium element in telluric acid or telluric acid is 2-4% (the sum of the molar contents of the above components satisfies 100%).

[0028] Furthermore, the pH in step (1) is 9 to 10, and the most preferred pH value is 9.5. Studies have shown that the pH in step (1) directly affects the content of catalyst particles distributed on the graphene surface. Studies have shown that when pH = 9.5, the distribution of catalyst particles on the graphene surface is the best, and good catalytic activity can be obtained.

[0029] Furthermore, the centrifugal separation described in step (2) specifically utilizes the density difference of the graphene-loaded catalyst particle precursor to separate it from water using centrifugal force. Compared with the filtration method, this method can obtain a composite catalyst precursor with a more uniform size, and some free nanoparticles or incompletely reacted ions can be easily separated from the product.

[0030] Furthermore, the drying in step (2) is baking at 150-200° C. in an air atmosphere, which can quickly dry the water in the precursor.

[0031] Furthermore, the ball milling described in step (3) is dry milling using a planetary ball mill, wherein the precursor (catalyst precursor crude product B) and zirconium beads with a particle size of 0.5 to 3 mm (the filling rate of zirconium beads in the ball mill is 30% to 50%) are placed in a ball mill jar of the ball mill for ball milling. During the ball milling process, the ball mill revolves around the turntable axis while performing a reverse planetary rotation motion around its own axis. The zirconium beads and the precursor in the jar collide and rub against each other during high-speed motion, thereby achieving the purpose of uniform crushing.

[0032] Furthermore, the ground powder in step (3) is sieved through a 200-mesh filter to obtain a composite catalyst precursor powder with uniform particle size.

[0033] Furthermore, the power of the microwave plasma in step (4) is 4-75 kW, and the temperature of the microwave plasma is 4000-6000 K, which can be adjusted within the above range according to the output of the reduced powder and the size of the reduction chamber.

[0034] Furthermore, the powder feeder in step (4) has a powder supply rate of 10 to 500 g / h.

[0035] Furthermore, the gas supply rate of the gas inlet in step (4) is 0.1 to 50 m 3 / h, wherein the volume ratio of argon to hydrogen is 1 / 1 to 3 / 1 (i.e., 1-3:1); the role of the hydrogen in the inlet gas in the catalyst preparation is to reduce the catalyst precursor in the form of oxide into a single catalyst particle, so that it has a higher catalytic activity; and the inert gas argon provides a good environment for the complete reduction of graphene oxide into graphene.

[0036] Furthermore, the cooling in step (4) is performed by setting a cooling cavity in the cavity, wherein an annular air knife is provided in the cooling cavity, the angle and air volume of the annular air knife are adjustable, the angle between the annular air knife and the inner wall of the cooling cavity is 30 to 60°, the cooling gas is nitrogen or argon, and the air volume in the cooling air knife is 0.5 to 50 m 3 / h; The function of the cooling gas is to quickly cool and shape the catalyst during its descent, reduce the probability of particle collision in the high-temperature field area, and prevent the particles from melting and growing, which would lead to a decrease in activity.

[0037] The present application also provides a method for preparing single-walled carbon nanotubes using the above-mentioned catalyst in combination with chemical vapor deposition, specifically: using a corundum tube with a diameter of 60-100 cm as a reactor, methane as a carbon source with a flow rate of 0.05-0.2 L / min, hydrogen as a carrier gas with a flow rate of 1-3 L / min, adjusting the central temperature of the reactor at 1000°C-1200°C, and the growth time for 20-40 min; then stopping the introduction of hydrogen and methane, and cooling to room temperature by introducing 1-3 L / min of argon (Ar) to obtain single-walled carbon nanotube powder.

[0038] The present invention also provides a preparation device for a catalyst for preparing single-walled carbon nanotubes, which includes a liquid-phase coarse powder preparation device and a solid-phase microwave plasma synthesis device; the liquid-phase coarse powder preparation device includes a hydrothermal reaction kettle, a centrifuge, a drying device and a grinder; the catalyst precursor obtained by the liquid-phase coarse powder preparation device is supplied to the solid-phase microwave plasma synthesis device; the solid-phase microwave plasma synthesis device includes a microwave plasma generator, a reduction cavity, a cooling cavity and a collection cavity; the microwave plasma generator, the reduction cavity, the cooling cavity and the collection cavity are connected in sequence from top to bottom.

[0039] Furthermore, the hydrothermal reactor, centrifuge, grinder and drying equipment are all standard equipment that can be purchased.

[0040] Furthermore, the reaction temperature of the hydrothermal reactor is 150-200° C., and the volume of the raw materials in the reactor accounts for 60%-80% of the volume of the hydrothermal reactor.

[0041] Furthermore, the rotation speed of the centrifuge is 8000-15000 rpm.

[0042] Furthermore, the drying process of the drying equipment is drying at 150-200° C. in air for 8-12 hours.

[0043] Furthermore, the grinding machine can be a planetary ball mill, etc., and 0.5-3 mm zirconium beads are placed in the ball mill to make the grinding particle size of the powder reach 50-500 nm.

[0044] Furthermore, the microwave plasma generator includes a microwave power supply, a microwave plasma torch and a waveguide; the microwave power supply is connected to the waveguide to generate microwaves and transmit the microwaves through the waveguide; the microwave plasma torch is connected to the waveguide to receive microwaves.

[0045] Furthermore, the power of the microwave power supply is 4-75kw, and the frequency of the microwave is 915MHZ.

[0046] Furthermore, the waveguide is a metal conduit for transmitting microwaves, which then enters a microwave plasma torch (such as a quartz torch glass tube or an alumina ceramic tube, etc.) to excite the ignition gas under normal pressure to form microwave plasma.

[0047] Furthermore, the microwave is excited and ignited at normal pressure to generate a microwave plasma flame, and the plasma flame extends vertically from top to bottom in the microwave plasma torch; the microwave plasma torch is provided with an inlet pipeline for the input of gas and raw materials, the microwave plasma torch is sealed and connected to the reduction cavity, the diameter of the microwave plasma torch is 30 to 80 mm, and the ignition method is normal pressure excitation (normal pressure excitation requires ignition using an ignition needle, specifically: a metal needle can be inserted into the microwave plasma torch, and the needle can be removed after ignition); the microwave plasma torch can use quartz glass or alumina ceramic tube as a container for forming and containing microwave plasma, and the microwave can be transmitted through a waveguide and then penetrate the tube wall of the quartz glass or alumina ceramic tube to form microwave plasma.

[0048] Furthermore, the inlet pipeline is connected to a feeding device for exciting gas and catalyst precursor powder (the feeding device can be a loss-in-weight metering feeder, one end of the inlet pipeline is connected to the quartz glass or alumina ceramic tube, and the side wall of the main pipeline at the other end is connected to the outlet of the screw loss-in-weight metering feeder, which is used to load the catalyst precursor into the microwave plasma area, and the main pipeline is connected to the exciting gas; the loss-in-weight metering feeder can be a single screw or a twin-screw structure, which can be flexibly adjusted as needed. The screw loss-in-weight metering feeder can also be equipped with a weighing and metering system and PLC control to improve intelligent operation, and can adopt conventional industry configurations).

[0049] Furthermore, the powder feeding speed in the catalyst precursor powder feeding device is 10 g / h to 5 kg / h.

[0050] Furthermore, the reduction chamber is made of stainless steel, preferably 316L stainless steel; the inner diameter of the reduction chamber is Φ100-400mm, the length is 150-500mm, and the wall thickness is 8-15mm; the setting function of the reduction chamber is to provide a closed environment and reduction space for catalyst preparation.

[0051] Furthermore, the cooling cavity is made of stainless steel, preferably 316L stainless steel; the inner diameter of the cooling cavity is Φ100-400mm, the length is 150-500mm, and the wall thickness is 8-15mm; it can be integrally formed with the reduction cavity or can be separated and then connected. If a split structure is used, the connection is sealed with a seal; an annular wind knife is arranged in the cooling cavity, and the angle of the annular wind knife and the inner wall of the cooling cavity are 30-60°, and the air volume in the annular wind knife is 0.5-50m 3 / h; the gas blown in by the annular air knife is argon or nitrogen, and the blown-in airflow can make the reduced and spheroidized powders crystallize quickly and cool down to shape.

[0052] Furthermore, the collection cavity is made of stainless steel and is sealed to the cooling cavity; an exhaust device is provided on the collection cavity to discharge exhaust gas; the catalyst powder can be collected after gathering at the bottom of the collection cavity under the action of airflow and gravity.

[0053] Furthermore, both the collection chamber and the reduction chamber are provided with observation windows; this structure can be used to observe the product status.

[0054] Furthermore, the microwave plasma extends from the microwave plasma torch into the reduction chamber.

[0055] Compared with the prior art, this application has the following advantages and beneficial effects:

[0056] 1. The present application utilizes graphene as a carrier and loaded metal nanoparticles as a catalyst for the synthesis of single-walled carbon nanotubes, wherein one of the raw materials for preparing the catalyst is graphene oxide, which releases gas during the hydrothermal reduction process, thereby preventing the agglomeration of metal particles attached to the surface of the graphene oxide; at the same time, in the process of preparing single-walled carbon nanotubes, the carrier graphene in the catalyst has a high specific surface area, which can effectively prevent the metal catalyst nanoparticles from melting in a high temperature field, thereby maintaining a high catalytic activity.

[0057] 2. The present application utilizes tellurium as the active site of the catalyst. By adjusting the proportion of tellurium, a highly active catalyst powder can be prepared. Thus, the single-walled carbon nanotubes prepared using the catalyst have a higher aspect ratio and better crystallinity.

[0058] 3. The present application proposes to use microwave plasma to treat a catalyst precursor compound / graphene oxide composite, and by optimizing the treatment process, the precursor compound and graphene oxide can be efficiently reduced to form a graphene-loaded composite catalyst; at the same time, the catalyst powder reduced by microwave plasma is quickly cooled by cooling gas to prevent excessive size growth caused by violent collisions of the catalyst under high temperature conditions; the catalyst particles prepared by the device and method of the present application are highly spheroidized and uniform in size, and the method is simple and efficient, which is suitable for large-scale production.

[0059] 4. The hydrothermal reaction in step (2) of the catalyst preparation of the present application is carried out at 150-200°C. Under this condition, the iron-based metal salt and telluric acid or hypotelluric acid can form iron-based tellurium oxide nanoparticles under alkaline, high temperature and high pressure conditions. The catalyst prepared by this method has the advantages of complete grain development, small particle size, uniform distribution, and light particle agglomeration. At the same time, in a high temperature, high pressure and alkaline environment, some oxygen-containing groups of graphene oxide are deoxidized and reduced to release gas, which can further prevent the agglomeration of nanoparticles. In addition, its ultra-high specific surface area as a catalyst carrier can make the catalyst particles easier to adhere to the surface, avoiding excessive growth of grains and loss of activity.

[0060] 5. The catalyst of the present application has a specific composition and content range. The iron element and the tellurium element form an iron-tellurium alloy and adhere to the surface of the graphene sheet. The tellurium element can produce a synergistic effect with the iron element. The catalyst has high activity, uniform particle size, and uniform diameter of the obtained single-walled carbon nanotubes (the diameter distribution state can be seen from the Raman RBM peak); the catalyst has good high-temperature stability. In high-temperature and long-term catalytic reactions, graphene can prevent the catalyst particles from fusing and maintain a high catalytic activity; especially when the graphene content is 4-7%, the iron content is 88-95%, and the tellurium content is 2-4%, the catalyst activity is the highest.

[0061] 6. The content of catalyst particles on the graphene surface of the present application can be adjusted by the preparation method; and graphene with a specific size and a certain specific surface area range can promote the stability and activity of the catalyst. When the graphene sheet diameter is 100 to 300 nm and the specific surface area is greater than 750 m 2 / g, the activity of the catalyst particles is the highest; when the size of the graphene microsheets is too large, there are too many catalyst particles loaded on the surface, and the specific gravity is too large, resulting in a decrease in activity; graphene sheets with low specific surface area have lower adsorption properties, resulting in insufficient catalyst particle loading and affecting catalyst activity.

[0062] 7. The tellurium element in the catalyst powder of the present invention can greatly increase the activity of the catalyst, forming highly active defects for the iron-based catalyst nanoparticles (carbon nanotubes will grow at the defect sites). During the synthesis of single-walled carbon nanotubes, the carbon atoms melted in the catalyst particles under high temperature conditions are directionally precipitated at the defect sites of the tellurium element to form high-quality single-walled carbon nanotubes.

[0063] 8. In the present application, the argon and hydrogen are ionized under the action of microwaves to form a microwave plasma, which can melt the surface of the nanoparticles while reducing the catalyst precursor to form a sphere with a more regular size; the regular spherical structure concentrates the defect sites of the catalyst in the tellurium island area, which is conducive to the growth of ultra-long and high-quality single-walled carbon nanotubes.

[0064] 9. The single-walled carbon nanotube powder obtained by the specific catalyst combined with the preparation method of the present application has high crystallinity and high yield; the ratio of G peak to D peak (IG / ID) in Raman test is not less than 15, and the 30min production capacity is not less than 0.06g; the catalyst prepared by the preparation method of the present application can maintain high dispersion and stability in a high temperature environment, so the prepared single-walled carbon nanotubes have uniform diameters, the diameters are concentrated in the range of 1.6 to 2.0 nm, have a high aspect ratio, and good crystallinity. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 This is a schematic structural diagram of a catalyst preparation device for synthesizing single-walled carbon nanotubes in the present application.

[0066] Figure 2 This is a schematic structural diagram of an example of the solid-phase microwave plasma synthesis device described in this application.

[0067] Figure 3 This is a schematic structural diagram of another example of the solid-phase microwave plasma synthesis device described in the present application.

[0068] As shown in the attached figure: 1. hydrothermal reactor, 2. centrifuge, 3. drying equipment, 4. grinder, 5. microwave plasma generator, 51. microwave power supply, 52. microwave plasma torch, 53. waveguide, 54. microwave plasma flame (microwave plasma), 55. inlet pipe, 56. catalyst precursor powder feeding device, 6. reduction chamber, 7. cooling chamber, 71. annular air knife, 8. collection chamber, 81. exhaust device, 9. observation window.

[0069] Figure 4 A flow chart of catalyst preparation in a preferred embodiment of the present invention;

[0070] Figure 5 This is the Raman spectrum of the single-walled carbon nanotubes prepared in Example 1 of the present invention.

[0071] Figure 6 This is the Raman spectrum of the single-walled carbon nanotubes prepared in Comparative Example 2 of the present invention.

[0072] Figure 7 This is a picture of the catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0073] The following will combine the embodiments and drawings to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only preferred embodiments, not all embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application;

[0074] It should also be noted that when a component is referred to as being "fixed to" another component, it may be directly on the other component or there may be another intermediate component, fixed through the intermediate component. When a component is considered to be "connected" to another component, it may be directly connected to the other component or there may be another intermediate component at the same time. When a component is considered to be "set on" another component, it may be directly set on the other component or there may be another intermediate component at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by technicians in the technical field of this application. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0075] In addition, the present application limits the molar number of carbon in graphene oxide and graphene as the quantitative standard. Although graphene oxide loses some carbon atoms to form carbon dioxide during the deoxygenation process, the change to the overall carbon molar number is not significant, so the limited numerical range of the content of graphene oxide and graphene remains consistent.

[0076] The following is described by specific embodiments and the following devices:

[0077] As attached Figure 1-3 As shown, a preparation device for a catalyst for preparing single-walled carbon nanotubes of the present application comprises a liquid phase coarse powder preparation device and a solid phase microwave plasma synthesis device; the liquid phase coarse powder preparation device comprises a hydrothermal reaction kettle 1, a centrifuge 2, a drying device 3 and a grinder 4 (the above-mentioned hydrothermal reaction kettle 1, centrifuge 2, drying device 3 and grinder 4 can be existing commercially available equipment, and the above-mentioned equipment can be connected to each other or independently set up. After completing the operation in one device, the material can be transferred to the next device for corresponding processing; it can also be connected to each other through a conveying pipeline to improve automation, that is, as shown in the attached Figure 1 As shown); the liquid phase coarse powder preparation device is used to supply the prepared catalyst precursor to the solid phase microwave plasma synthesis device; the solid phase microwave plasma synthesis device includes a microwave plasma generator 5, a reduction cavity 6, a cooling cavity 7 and a collection cavity 8; the microwave plasma generator 5, the reduction cavity 6, the cooling cavity 7 and the collection cavity 8 are connected in sequence from top to bottom; the reduction cavity 6, the cooling cavity 7 and the collection cavity 8 of the present application are devices prepared by specific materials, and the cavity structures formed inside them are convenient for accommodating materials.

[0078] As an example, the hydrothermal reactor 1, centrifuge 2, grinder 3 and drying equipment 4 described in the present application are all standard equipment that can be purchased on the market. The corresponding equipment that can be used to prepare the catalyst precursor of the present application is applicable to the present application and will not be described in detail here.

[0079] As an example, the reaction temperature in the hydrothermal reactor 1 described in the present application is 150-200° C., and the volume of the raw materials in the reactor accounts for 60%-80% of the volume of the hydrothermal reactor.

[0080] As an example, the rotation speed of the centrifuge 2 described in the present application is set to 8000-15000 rpm.

[0081] As an example, the drying process of the drying equipment 4 described in the present application is drying at 150-200° C. in air for 8-12 hours.

[0082] As an example, the grinder 3 described in the present application can be a planetary ball mill, etc., and the powder grinding particle size is 50 to 500 nm; the catalyst precursor to be ball-milled and zirconium beads with a particle size of 0.5 to 3 mm (the zirconium bead filling rate is 30% to 50%) are loaded in a ball mill jar, which revolves around the turntable axis while performing a reverse planetary rotation around its own axis. The zirconium beads and precursors in the jar collide and rub against each other during high-speed motion, thereby achieving the purpose of uniform crushing.

[0083] As attached Figure 1-3 As shown, the microwave plasma generator 5 described in the present application includes a microwave power supply 51, a microwave plasma torch 52 and a waveguide 53; the microwave power supply 51 is connected to the waveguide 52 for generating microwaves and transmitting microwaves through the waveguide 53; the microwave plasma torch 52 is connected to the waveguide 53 for receiving microwaves.

[0084] As an example, the power of the microwave power supply 51 described in the present application is 4-75kw, and the frequency of the microwave is 915MHZ.

[0085] As an example, the waveguide 53 described in the present application is a metal conduit for transmitting microwaves, which then enters a microwave plasma torch (a specific microwave plasma torch may be a quartz torch glass tube or an alumina ceramic tube) to excite gas under normal pressure to form a microwave plasma flame 54 in the torch.

[0086] As an example, the microwave described in the present application is excited and ignited at normal pressure to generate a microwave plasma flame 54, and the plasma flame extends vertically from the top to the bottom in the microwave plasma torch 52 and extends into the reduction chamber 6; the microwave plasma torch 52 is provided with an inlet pipe 55, and the inlet pipe 55 is used for inputting the excitation gas, and is also connected to a feeding device 56 to input the catalyst precursor processed from the grinder into the microwave plasma torch 52; the microwave plasma torch 52 is sealed and connected to the reduction chamber 6, the diameter of the microwave plasma torch 52 is 30 to 80 mm, and the ignition method is normal pressure excitation (normal pressure excitation requires ignition using an ignition needle, specifically: a metal needle can be inserted into the microwave plasma torch, and the needle can be removed after ignition); the microwave plasma torch can use a quartz glass or alumina ceramic tube as a container for forming and containing microwave plasma, and the microwave can be transmitted through a waveguide and then penetrate the tube wall of the quartz glass or alumina ceramic tube to form microwave plasma.

[0087] As attached Figure 1-3As shown, the inlet pipeline 55 described in the present application connects the excitation gas and the catalyst precursor powder feeding device 56; the catalyst precursor powder feeding device 56 is used to receive the discharge of the ball mill 4; specifically, the powder feeding device 56 can be a loss-in-weight metering feeder, one end of the inlet pipeline is connected to the quartz glass or alumina ceramic tube, and the other end is connected to the outlet of the loss-in-weight metering feeder, which is used to load the catalyst precursor into the microwave plasma area; the loss-in-weight metering feeder can be a single screw or a twin-screw structure, which can be flexibly adjusted as needed; the screw loss-in-weight metering feeder is equipped with a weighing and metering system and PLC control to improve intelligent operation.

[0088] As an example, the powder feeding rate in the catalyst precursor powder feeding device 56 described in the present application is 100 g / h to 5 kg / h.

[0089] As an example, the reduction chamber 6 described in the present application is made of stainless steel, preferably 316L stainless steel; the inner diameter of the reduction chamber is Φ100~400mm, the length is 150~500mm, and the wall thickness is 8~15mm; the setting function of the reduction chamber is to provide a closed environment and reduction space for catalyst preparation.

[0090] As an example, the cooling cavity 7 described in the present application is made of stainless steel, preferably 316L stainless steel; the inner diameter of the cooling cavity is Φ100-400mm, the length is 150-500mm, and the wall thickness is 8-15mm; it can be integrally formed with the reduction cavity or can also be a split structure. If a split structure is used, the connection is sealed with a seal.

[0091] As an example, the attached Figure 3 As shown, the cooling cavity 7 described in the present application is provided with an annular air knife 71, the angle of the annular air knife 71 and the inner wall of the cooling cavity 7 is 30-60°, and the air volume is 0.5-50m 3 / h; the gas blown in by the annular air knife is argon or nitrogen, and the blown-in airflow can make the reduced and spheroidized powders crystallize quickly and cool down to shape.

[0092] As an example, the collection chamber 8 described in the present application is made of stainless steel and is sealed and connected to the cooling chamber 7; an exhaust device 81 is provided on the collection chamber 8 (specifically, an exhaust pipe and an exhaust pump can be connected to discharge the gas in the collection chamber) for discharging exhaust gas; the catalyst powder is collected after gathering at the bottom of the collection chamber 8 under the action of airflow and gravity.

[0093] As an example, the attached Figure 2As shown, the collection chamber 8 and the reduction chamber 6 described in the present application are both provided with an observation window 9 (i.e., a visual window made of transparent material, which is convenient for observing the internal reaction conditions so as to adjust the reaction state in time); this structure can be used to observe the product conditions.

[0094] As attached Figure 1-2 As shown, the microwave plasma described in the present application extends from the microwave plasma torch 52 to the reduction chamber 6 to ensure that the reduction reaction is carried out more fully and thoroughly.

[0095] The following is a device prepared by using the catalyst described above in this application, and in combination with the attached Figure 4 The specific process steps described in detail in this application:

[0096] Example 1

[0097] 1. Weigh 8 mol of ferric nitrate, 1 mol of cobalt acetate, and 0.3 mol of telluric acid and add them to 700 mL of a monolayer graphene oxide aqueous solution with a carbon molar concentration of 0.5 mol, the sheet diameter of the graphene oxide is 50-150 nm, and slowly add ammonia water to the above solution while stirring to adjust the pH to 9.5;

[0098] 2. Place the above solution in a 1L hydrothermal reactor 1, perform hydrothermal reaction at 180°C for 12 hours, and after the reaction is completed, cool the solution to room temperature, place it in a centrifuge 2 and centrifuge it at 15000 rpm to obtain a solid substance, and place it in a dryer 3 and dry it in an air atmosphere at 150°C for 10 hours;

[0099] 3. The dried powder was mixed with zirconium beads with a particle size of 1 mm and placed in a planetary ball mill (mill 4) for 2 h, and then sieved through a 200-mesh sieve to obtain a catalyst precursor powder;

[0100] 4. Place the screened catalyst precursor powder in a powder feeder (catalyst precursor powder feeder 56), and introduce 20 m3 of gas into the gas inlet (the input port of the inlet pipeline 55). 3 / h argon and 10m 3 / h hydrogen, turn on the microwave power supply 51 (power 20kW) to form microwave plasma in the microwave plasma torch 52 and the reduction chamber 6, add the catalyst precursor powder at a feeding rate of 500g / h, and pass 40m in the cooling chamber 7 through the annular air knife 71. 3 / h argon gas, set the wind knife angle to 45 degrees, and collect graphene-supported iron-cobalt-tellurium composite catalyst powder in the collection chamber 8; the specific state of the catalyst powder is shown in the attached Figure 7 Shown is a picture of the catalyst product prepared in this example.

[0101] 5. 0.1 g of the catalyst prepared above was placed in the high temperature zone of a corundum tube with an inner diameter of 80 cm to prepare single-walled carbon nanotubes. The temperature of the high temperature zone of the corundum tube was set at 1200°C, methane was used as the carbon source, and its flow rate was controlled at 0.1 L / min, and hydrogen was used as the carrier gas, and its flow rate was controlled at 2 L / min. The growth was carried out for 30 minutes; then the introduction of hydrogen and methane was stopped, and argon was introduced at 2 L / min to cool to room temperature to obtain about 0.1 g of single-walled carbon nanotube powder.

[0102] As a preferred embodiment of the present invention, the product was characterized by Raman spectroscopy. Figure 5 It can be seen that there is a strong G peak near 1560cm-1, a weak D peak at 1330cm-1, and an I G / I D About 40; in the low wave number region of 100-250cm-1, a typical single-walled carbon nanotube breathing vibration peak RBM peak appears, with a peak position of 140cm-1. The peak frequency shift of the single-walled carbon nanotube is inversely proportional to the diameter. According to d = 248 / ω RBM It can be seen that the diameter of a single-walled carbon nanotube is about 1.77 nm.

[0103] Example 2

[0104] 1. Weigh 8 mol of ferric nitrate, 1 mol of cobalt acetate, and 0.1 mol of telluric acid and add them to 700 mL of a monolayer graphene oxide aqueous solution with a carbon molar concentration of 0.5 mol, and the flake diameter is 50-150 nm. Slowly add ammonia water to the above solution while stirring to adjust the pH to 9.5;

[0105] 2. Place the above solution in a 1L hydrothermal reactor and perform hydrothermal reaction at 180°C for 12 hours. After the reaction is completed, the solution is cooled to room temperature and centrifuged at 15000 rpm to obtain a solid substance, which is then dried in an air atmosphere at 150°C.

[0106] 3. The dried powder was mixed with 1 mm zirconium beads and placed in a planetary ball mill for 2 h. The catalyst precursor powder was obtained after sieving through a 200-mesh sieve.

[0107] 4. Place the screened catalyst precursor powder in the powder feeder and introduce 20m 3 / h argon and 10m 3 / h hydrogen, turn on the microwave power supply (power 20kW) to form microwave plasma in the reduction chamber, add catalyst precursor powder at a feeding rate of 500g / h, and pass 40m 3 / h argon gas, set the wind knife angle to 45 degrees, and collect graphene-loaded iron-cobalt-tellurium composite catalyst powder in the collection chamber.

[0108] 5. Single-walled carbon nanotubes were prepared using the above catalyst. The specific preparation method was as follows: a corundum tube with a diameter of 80 cm was used as a reactor, methane was used as a carbon source with a flow rate of 0.1 L / min, hydrogen was used as a carrier gas with a flow rate of 2 L / min, the center temperature of the reactor was adjusted to 1200°C, and the growth was carried out for 30 minutes; hydrogen and methane were stopped, 2 L / min of argon was introduced and cooled to room temperature to obtain 0.06 g of single-walled carbon nanotube powder.

[0109] The Raman test results of the single-walled carbon nanotube powder in this embodiment are as follows: G / I D It is about 50, and the diameter of a single-walled carbon nanotube is about 1.65nm.

[0110] Example 3

[0111] 1. Weigh 8 mol of ferric nitrate, 1 mol of cobalt acetate, and 0.5 mol of telluric acid and add them to 700 mL of a monolayer graphene oxide aqueous solution with a carbon molar concentration of 0.5 mol, and the flake diameter is 50-150 nm. Slowly add ammonia water to the above solution while stirring to adjust the pH to 9.5;

[0112] 2. Place the above solution in a 1L hydrothermal reactor and perform hydrothermal reaction at 180°C for 12 hours. After the reaction is completed, the solution is cooled to room temperature and centrifuged at 15000 rpm to obtain a solid substance, which is then dried in an air atmosphere at 150°C.

[0113] 3. The dried powder was mixed with 1 mm zirconium beads and placed in a planetary ball mill for 2 h. The catalyst precursor powder was obtained after sieving through a 200-mesh sieve.

[0114] 4. Place the screened catalyst precursor powder in the powder feeder and introduce 20m 3 / h argon and 10m 3 / h hydrogen, turn on the microwave power supply (power 20kW) to form microwave plasma in the reduction chamber, add catalyst precursor powder at a feeding rate of 500g / h, and pass 40m 3 / h argon gas, set the wind knife angle to 45 degrees, and collect graphene-loaded iron-cobalt-tellurium composite catalyst powder in the collection chamber.

[0115] 5. Single-walled carbon nanotubes were prepared using the above catalyst. The specific preparation method was as follows: a corundum tube with a diameter of 80 cm was used as a reactor, methane was used as a carbon source with a flow rate of 0.1 L / min, hydrogen was used as a carrier gas with a flow rate of 2 L / min, the center temperature of the reactor was adjusted to 1200°C, and the growth was carried out for 30 minutes; hydrogen and methane were stopped, 2 L / min of argon was introduced and cooled to room temperature to obtain 0.18 g of single-walled carbon nanotube powder.

[0116] The Raman test results of the single-walled carbon nanotube powder in this embodiment are as follows: G / I D It is about 20, and the diameter of a single-walled carbon nanotube is about 1.95nm.

[0117] Example 4

[0118] 1. Weigh 8 mol of ferric nitrate, 1 mol of cobalt acetate, and 0.3 mol of telluric acid and add them to 700 mL of a monolayer graphene oxide aqueous solution with a carbon molar concentration of 0.1 mol, and the flake diameter is 50-150 nm. Slowly add ammonia water to the above solution while stirring to adjust the pH to 9.5;

[0119] 2. Place the above solution in a 1L hydrothermal reactor and perform hydrothermal reaction at 180°C for 12 hours. After the reaction is completed, the solution is cooled to room temperature and centrifuged at 15000 rpm to obtain a solid substance, which is then dried in an air atmosphere at 150°C.

[0120] 3. The dried powder was mixed with 1 mm zirconium beads and placed in a planetary ball mill for 2 h. The catalyst precursor powder was obtained after sieving through a 200-mesh sieve.

[0121] 4. Place the screened catalyst precursor powder in the powder feeder and introduce 20m 3 / h argon and 10m 3 / h hydrogen, turn on the microwave power supply (power 20kW) to form microwave plasma in the reduction chamber, add catalyst precursor powder at a feeding rate of 500g / h, and pass 40m 3 / h argon gas, set the wind knife angle to 45 degrees, and collect graphene-loaded iron-cobalt-tellurium composite catalyst powder in the collection chamber.

[0122] 5. Single-walled carbon nanotubes were prepared using the above catalyst. The specific preparation method was as follows: a corundum tube with a diameter of 80 cm was used as a reactor, methane was used as a carbon source with a flow rate of 0.1 L / min, hydrogen was used as a carrier gas with a flow rate of 2 L / min, the center temperature of the reactor was adjusted to 1200°C, and the growth was carried out for 30 minutes; hydrogen and methane were stopped, 2 L / min of argon was introduced and cooled to room temperature to obtain 0.09 g of single-walled carbon nanotube powder.

[0123] The Raman test results of the single-walled carbon nanotube powder in this embodiment are as follows: G / I D It is about 35, and the diameter of a single-walled carbon nanotube is about 1.79nm.

[0124] Example 5

[0125] 1. Weigh 8 mol of ferric nitrate, 1 mol of cobalt acetate, and 0.3 mol of telluric acid and add them to 700 mL of a monolayer graphene oxide aqueous solution with a carbon molar concentration of 1.0 mol, and the flake diameter is 50-150 nm. Slowly add ammonia water to the above solution while stirring to adjust the pH to 9.5;

[0126] 2. Place the above solution in a 1L hydrothermal reactor and perform hydrothermal reaction at 180°C for 12 hours. After the reaction is completed, the solution is cooled to room temperature and centrifuged at 15000 rpm to obtain a solid substance, which is then dried in an air atmosphere at 150°C.

[0127] 3. The dried powder was mixed with 1 mm zirconium beads and placed in a planetary ball mill for 2 h. The catalyst precursor powder was obtained after sieving through a 200-mesh sieve.

[0128] 4. Place the screened catalyst precursor powder in the powder feeder and introduce 20m 3 / h argon and 10m 3 / h hydrogen, turn on the microwave power supply (power 20kW) to form microwave plasma in the reduction chamber, add catalyst precursor powder at a feeding rate of 500g / h, and pass 40m 3 / h argon gas, set the wind knife angle to 45 degrees, and collect graphene-loaded iron-cobalt-tellurium composite catalyst powder in the collection chamber.

[0129] 5. Single-walled carbon nanotubes were prepared using the above catalyst. The specific preparation method was as follows: a corundum tube with a diameter of 80 cm was used as a reactor, methane was used as a carbon source with a flow rate of 0.1 L / min, hydrogen was used as a carrier gas with a flow rate of 2 L / min, the center temperature of the reactor was adjusted to 1200°C, and the growth was carried out for 30 minutes; hydrogen and methane were stopped, 2 L / min of argon was introduced and cooled to room temperature to obtain 0.8 g of single-walled carbon nanotube powder.

[0130] The Raman test results of the single-walled carbon nanotube powder in this embodiment are as follows: G / I D It is about 30, and the diameter of a single-walled carbon nanotube is about 1.67nm.

[0131] Example 6

[0132] 1. Weigh 8 mol of ferric nitrate, 0.8 mol of cobalt acetate, and 0.3 mol of telluric acid and add them to 700 mL of a monolayer graphene oxide aqueous solution with a carbon molar concentration of 0.5 mol, and the flake diameter is 50-150 nm. Slowly add ammonia water to the above solution while stirring to adjust the pH to 9.5;

[0133] 2. Place the above solution in a 1L hydrothermal reactor and perform hydrothermal reaction at 180°C for 12 hours. After the reaction is completed, the solution is cooled to room temperature and centrifuged at 15000 rpm to obtain a solid substance, which is then dried in an air atmosphere at 150°C.

[0134] 3. The dried powder was mixed with 1 mm zirconium beads and placed in a planetary ball mill for 2 h. The catalyst precursor powder was obtained after sieving through a 200-mesh sieve.

[0135] 4. Place the screened catalyst precursor powder in the powder feeder and introduce 20m 3 / h argon and 10m 3 / h hydrogen, turn on the microwave power supply (power 20kW) to form microwave plasma in the reduction chamber, add catalyst precursor powder at a feeding rate of 500g / h, and pass 40m 3 / h argon gas, set the wind knife angle to 45 degrees, and collect graphene-loaded iron-cobalt-tellurium composite catalyst powder in the collection chamber.

[0136] 5. Use 0.1 g of the above catalyst to place in the high temperature zone of a corundum tube with an inner diameter of 80 cm to prepare single-walled carbon nanotubes. Set the temperature of the high temperature zone of the corundum tube at 1200°C, use methane as the carbon source with a flow rate of 0.1 L / min, and use hydrogen as the carrier gas with a flow rate of 2 L / min, and grow for 30 minutes; stop hydrogen and methane, pass 2 L / min of argon and cool to room temperature to obtain about 0.12 g of single-walled carbon nanotube powder.

[0137] The Raman test results of the single-walled carbon nanotube powder in this embodiment are as follows: G / I D It is about 35, and the diameter of a single-walled carbon nanotube is about 1.89nm.

[0138] Example 7

[0139] 1. Weigh 8 mol of ferric nitrate, 1.6 mol of cobalt acetate, and 0.3 mol of telluric acid and add them to 700 mL of a monolayer graphene oxide aqueous solution with a carbon molar concentration of 0.5 mol, and the flake diameter is 50-150 nm. Slowly add ammonia water to the above solution while stirring to adjust the pH to 9.5;

[0140] 2. Place the above solution in a 1L hydrothermal reactor and perform hydrothermal reaction at 180°C for 12 hours. After the reaction is completed, the solution is cooled to room temperature and centrifuged at 15000 rpm to obtain a solid substance, which is then dried in an air atmosphere at 150°C.

[0141] 3. The dried powder was mixed with 1 mm zirconium beads and placed in a planetary ball mill for 2 h. The catalyst precursor powder was obtained after sieving through a 200-mesh sieve.

[0142] 4. Place the screened catalyst precursor powder in the powder feeder and introduce 20m 3 / h argon and 10m 3 / h hydrogen, turn on the microwave power supply (power 20kW) to form microwave plasma in the reduction chamber, add catalyst precursor powder at a feeding rate of 500g / h, and pass 40m 3 / h argon gas, set the wind knife angle to 45 degrees, and collect graphene-loaded iron-cobalt-tellurium composite catalyst powder in the collection chamber.

[0143] 5. Use 0.1 g of the above catalyst to place in the high temperature zone of a corundum tube with an inner diameter of 80 cm to prepare single-walled carbon nanotubes. Set the temperature of the high temperature zone of the corundum tube at 1200°C, use methane as the carbon source with a flow rate of 0.1 L / min, and use hydrogen as the carrier gas with a flow rate of 2 L / min, and grow for 30 minutes; stop hydrogen and methane, pass 2 L / min of argon and cool to room temperature to obtain about 0.07 g of single-walled carbon nanotube powder.

[0144] The Raman test results of the single-walled carbon nanotube powder in this embodiment are as follows: G / I D It is about 45, and the diameter of a single-walled carbon nanotube is about 1.63nm.

[0145] Example 8

[0146] 1. Weigh 8 mol of ferric nitrate, 1 mol of cobalt acetate, and 0.3 mol of telluric acid and add them to 700 mL of a monolayer graphene oxide aqueous solution with a carbon molar concentration of 0.5 mol, and the flake diameter is 50-150 nm. Slowly add ammonia water to the above solution while stirring to adjust the pH to 8.5;

[0147] 2. Place the above solution in a 1L hydrothermal reactor and perform hydrothermal reaction at 180°C for 12 hours. After the reaction is completed, the solution is cooled to room temperature and centrifuged at 15000 rpm to obtain a solid substance, which is then dried in an air atmosphere at 150°C.

[0148] 3. The dried powder was mixed with 1 mm zirconium beads and placed in a planetary ball mill for 2 h. The catalyst precursor powder was obtained after sieving through a 200-mesh sieve.

[0149] 4. Place the screened catalyst precursor powder in the powder feeder and introduce 20m 3 / h argon and 10m 3 / h hydrogen, turn on the microwave power supply (power 20kW) to form microwave plasma in the reduction chamber, add catalyst precursor powder at a feeding rate of 500g / h, and pass 40m3 / h argon gas, set the wind knife angle to 45 degrees, and collect graphene-loaded iron-cobalt-tellurium composite catalyst powder in the collection chamber.

[0150] 5. Use 0.1 g of the above catalyst to place in the high temperature zone of a corundum tube with an inner diameter of 80 cm to prepare single-walled carbon nanotubes. Set the temperature of the high temperature zone of the corundum tube at 1200°C, use methane as the carbon source with a flow rate of 0.1 L / min, and use hydrogen as the carrier gas with a flow rate of 2 L / min, and grow for 30 minutes; stop hydrogen and methane, pass 2 L / min of argon and cool to room temperature to obtain about 0.1 g of single-walled carbon nanotube powder.

[0151] The Raman test results of the single-walled carbon nanotube powder in this embodiment are as follows: G / I D It is about 35, and the diameter of a single-walled carbon nanotube is about 1.94nm.

[0152] Example 9

[0153] 1. Weigh 8 mol of ferric nitrate, 1 mol of cobalt acetate, and 0.3 mol of telluric acid and add them to 700 mL of a monolayer graphene oxide aqueous solution with a carbon molar concentration of 0.5 mol, and the flake diameter is 50-150 nm. Slowly add ammonia water to the above solution while stirring to adjust the pH to 9.5;

[0154] 2. Place the above solution in a 1L hydrothermal reactor and perform hydrothermal reaction at 180°C for 12 hours. After the reaction is completed, the solution is cooled to room temperature and centrifuged at 15000 rpm to obtain a solid substance, which is then dried in an air atmosphere at 150°C.

[0155] 3. The dried powder was mixed with 1 mm zirconium beads and placed in a planetary ball mill for 2 h. The catalyst precursor powder was obtained after sieving through a 200-mesh sieve.

[0156] 4. Place the screened catalyst precursor powder in the powder feeder and introduce 20m 3 / h argon and 10m 3 / h hydrogen, turn on the microwave power supply (power 20kW) to form microwave plasma in the reduction chamber, add catalyst precursor powder at a feeding rate of 500g / h, and pass 40m 3 / h argon gas, set the wind knife angle to 45 degrees, and collect graphene-loaded iron-cobalt-tellurium composite catalyst powder in the collection chamber.

[0157] 5. Use 0.1 g of the above catalyst to place in the high temperature zone of a corundum tube with an inner diameter of 80 cm to prepare single-walled carbon nanotubes. Set the temperature of the high temperature zone of the corundum tube at 1200°C, use methane as the carbon source with a flow rate of 0.1 L / min, and use hydrogen as the carrier gas with a flow rate of 2 L / min, and grow for 30 minutes; stop hydrogen and methane, pass 2 L / min of argon and cool to room temperature to obtain about 0.1 g of single-walled carbon nanotube powder.

[0158] The Raman test results of the single-walled carbon nanotube powder in this embodiment are as follows: G / I D It is about 38, and the diameter of a single-walled carbon nanotube is about 1.79nm.

[0159] Example 10

[0160] 1. Weigh 8 mol of ferric nitrate, 1 mol of nickel sulfate, and 0.3 mol of telluric acid and add them to 700 mL of a monolayer graphene oxide aqueous solution with a carbon molar concentration of 0.5 mol, and the flake diameter is 50-150 nm. Slowly add ammonia water to the above solution while stirring to adjust the pH to 9.5;

[0161] 2. Place the above solution in a 1L hydrothermal reactor and perform hydrothermal reaction at 180°C for 12 hours. After the reaction is completed, the solution is cooled to room temperature and centrifuged at 15000 rpm to obtain a solid substance, which is then dried in an air atmosphere at 150°C.

[0162] 3. The dried powder was mixed with 1 mm zirconium beads and placed in a planetary ball mill for 2 h. The catalyst precursor powder was obtained after sieving through a 200-mesh sieve.

[0163] 4. Place the screened catalyst precursor powder in the powder feeder and introduce 20m 3 / h argon and 10m 3 / h hydrogen, turn on the microwave power supply (power 20kW) to form microwave plasma in the reduction chamber, add catalyst precursor powder at a feeding rate of 500g / h, and pass 40m 3 / h argon gas, set the wind knife angle to 45 degrees, and collect graphene-loaded iron-cobalt-tellurium composite catalyst powder in the collection chamber.

[0164] 5. Use 0.1 g of the above catalyst to place in the high temperature zone of a corundum tube with an inner diameter of 80 cm to prepare single-walled carbon nanotubes. Set the temperature of the high temperature zone of the corundum tube at 1200°C, use methane as the carbon source with a flow rate of 0.1 L / min, and use hydrogen as the carrier gas with a flow rate of 2 L / min, and grow for 30 minutes; stop hydrogen and methane, pass 2 L / min of argon and cool to room temperature to obtain about 0.08 g of single-walled carbon nanotube powder.

[0165] The Raman test results of the single-walled carbon nanotube powder in this embodiment are as follows: G / I D It is about 42, and the diameter of a single-walled carbon nanotube is about 1.57nm.

[0166] Comparative Example 1

[0167] The same as Example 1, except that methyl mercaptan is used instead of telluric acid.

[0168] Results: The yield of single-walled carbon nanotubes was 0.05 g, and Raman test I G / I D is 12.

[0169] Comparative Example 2

[0170] The same as Example 1, except that deionized water is used instead of the graphene oxide aqueous solution.

[0171] Result: Participated Figure 4 , single-walled carbon nanotube yield is 0.02g, Raman test I G / I D is 3.

[0172] Comparative Example 3

[0173] The same as Example 1, except that the diameter of the graphene oxide sheet is 1 to 10 um.

[0174] Results: The yield of single-walled carbon nanotubes was 0.04 g, and Raman test I G / I D is 30.

[0175] Comparative Example 4

[0176] Same as Example 1, except that cobalt acetate was not used.

[0177] Results: The yield of single-walled carbon nanotubes was 0.15 g, and Raman test I G / I D is 14.

[0178] Comparative Example 5

[0179] Same as Example 1, except that telluric acid is not used.

[0180] Results: The yield of single-walled carbon nanotubes was 0.01 g, and Raman test I G / I D It is 41.

[0181] Comparative Example 6

[0182] The same as Example 1, except that the molar mass of telluric acid added is 2 mol.

[0183] Results: Single-walled carbon nanotube yield 0.2g, Raman test I G / I D is 2.8.

[0184] Comparative Example 7

[0185] Same as Example 1, except that the pH was not adjusted.

[0186] Results: Single-walled carbon nanotube yield 0.02g, Raman test I G / I D is 15.

[0187] Comparative Example 8

[0188] The same as Example 1, except that step 4 is replaced by reduction using a tubular furnace, that is, the screened catalyst precursor powder is placed in a 150 mm diameter tubular furnace corundum tube, 20 m3 / h argon and 10 m3 / h hydrogen are introduced at the gas inlet, the high temperature zone temperature is set to 1000°C, and the reduction time is 2 h.

[0189] Results: Single-walled carbon nanotube yield 0.03g, Raman test I G / I D is 10.

[0190] Comparative Example 9

[0191] The same as Example 1, except that air flow cooling is not used in step 4.

[0192] Results: Single-walled carbon nanotube production 0.09 g / h, Raman test I G / I D is 3.5.

[0193] From the results of Examples 1 to 10, it can be seen that when graphene with a sheet diameter of 50 to 500 nm has a carbon molar content of 1 to 10%, an iron-based metal element molar content of 85 to 98% (wherein the atomic ratio of iron to cobalt or nickel is 5 to 10 / 1), and a tellurium element molar content of 1 to 5%, a composite catalyst with high catalytic activity can be obtained by combining hydrothermal reaction, microwave plasma reduction, airflow cooling and other methods.

[0194] As can be seen from Example 1 and Comparative Example 1, conventional growth promoters such as mercaptan cannot obtain catalysts with high catalytic activity when added during the catalyst preparation process. This may be because the iron-sulfur phase formed by sulfur and iron-based catalysts during the high-temperature catalyst preparation process cannot exist stably at low temperatures, while tellurium, as a Group VI element, has similar chemical properties to sulfur and can form a stable composite structure with iron metal. As can be seen from Examples 1 to 3 and Comparative Examples 5 and 6, a certain proportion of tellurium has a significant enhancing effect on the activity of the catalyst, but when its content is too low, the yield of single-walled carbon nanotubes drops sharply, and when its content is too high, the yield increases, but the cleanliness of the product is significantly reduced.

[0195] It can be seen from Examples 1, 4, 5 and Comparative Examples 2 and 3 that in the present invention, graphene is used as a catalyst carrier, and its catalytic activity of the product has a significant effect. Within a certain ratio range (carbon molar fraction 1-10%), high-yield and high-quality single-walled carbon nanotubes can be prepared. As shown in Comparative Example 2, if the graphene carrier is not suitable in the raw material, its catalytic activity is reduced, the G / D of the product is also reduced, and the crystallinity is deteriorated. This is because the gas released by graphene oxide during the hydrothermal reduction process can prevent the metal particles attached to the surface of graphene oxide from agglomerating; at the same time, in the process of preparing single-walled carbon nanotubes, the high specific surface area of ​​graphene can effectively prevent the metal catalyst nanoparticles from melting in a high temperature field, and maintain a high catalytic activity. As shown in Comparative Example 3, the sheet diameter of graphene also has a certain effect on the catalytic activity. When the diameter of the graphene sheet is too large, although the catalyst can still be evenly loaded on the graphene surface, in the process of preparing single-walled carbon nanotubes, excessive steric hindrance will hinder the melting of carbon atoms and catalyst particles, resulting in a decrease in yield.

[0196] It can be seen from Comparative Examples 4 and 7 that the type of iron-based metal in the raw material and the pH during the preparation process also have a certain influence on the activity of the catalyst. Binary catalysts such as iron-cobalt or iron-nickel have higher catalytic activity than pure iron catalysts. The pH value in the hydrothermal reaction process accelerates the formation of metal oxides to a certain extent, and can form a higher bridging effect between the metal and graphene, making it easier for metal ions to evenly adhere to the graphene surface.

[0197] The microwave plasma reduction and rapid cooling method of the present invention is the key to preparing the catalyst of the present invention. The catalyst precursor supported by graphene oxide absorbs the heat of microwave plasma, and the graphene oxide is reduced to graphene, releasing a large amount of gas to inhibit the melting of catalyst particles under high temperature. In addition, the catalyst particles are reduced to nanoparticles with high catalytic activity under the action of hydrogen. At the same time, the catalyst powder reduced by microwave plasma is rapidly cooled by cooling gas to prevent excessive size growth caused by violent collision of the catalyst under high temperature conditions. It can be seen from Comparative Example 8 of the present invention that traditional high-temperature annealing reduction cannot obtain a catalyst with high catalytic activity, and changing the process parameters of the microwave plasma of the present invention, such as not applying rapid cooling (such as Comparative Example 9), will cause the catalyst particles to continue to be high temperature and then deactivated. Therefore, rapid cooling by airflow plays an obvious role in the present invention.

[0198] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the principles and spirit of the present invention are included in the protection scope of the present invention.

Claims

1. A catalyst for synthesizing single-walled carbon nanotubes, characterized in that: The catalyst comprises iron-based metal elements, tellurium elements and graphene, wherein the molar content of the iron-based metal elements is 85-98%, the molar content of the tellurium elements is 1-5%, the molar content of the graphene carbon is 1-10%, and the size of the catalyst particles is 10-40nm.

2. The catalyst for synthesizing single-walled carbon nanotubes according to claim 1, characterized in that: The molar content of the iron-based metal element is 88-95%, the molar content of the tellurium element is 2-4%, and the molar content of carbon in the graphene is 4-7%.

3. The catalyst for synthesizing single-walled carbon nanotubes according to claim 1, characterized in that: The graphene is a single-layer or multi-layer structure with a specific surface area of ​​300 to 1000 m 2 / g, and the flake diameter is 50-500nm.

4. The catalyst for synthesizing single-walled carbon nanotubes according to claim 3, characterized in that: The specific surface area of ​​the graphene is 750 m 2 / g~1000m 2 / g, and the flake diameter is 100~300nm.

5. The catalyst for synthesizing single-walled carbon nanotubes according to claim 1, characterized in that: The iron-based metal element is one or more of iron, cobalt and nickel; the source material of the tellurium element is one of telluric acid or hypotelluric acid.

6. The catalyst for synthesizing single-walled carbon nanotubes according to claim 5, characterized in that: The iron-based metal elements are two or more of iron, cobalt and nickel.

7. The catalyst for synthesizing single-walled carbon nanotubes according to claim 6, characterized in that: The iron-based metal elements are iron and nickel or iron and cobalt, and the molar ratio of iron to cobalt or iron to nickel is 5-10:

1.

8. The catalyst for synthesizing single-walled carbon nanotubes according to claim 6, characterized in that: The sources of the iron, cobalt and nickel are water-soluble compounds.

9. A method for preparing a catalyst for synthesizing single-walled carbon nanotubes according to any one of claims 1 to 8, characterized in that: include: (1) weighing a precursor containing an iron-based metal element and a tellurium element and dissolving it in an aqueous solution of graphene oxide, then dropping ammonia water into the solution and adjusting the pH to 8 to 10 to obtain a solution A; (2) placing solution A in a reaction kettle, wherein the volume of solution A accounts for 60-80% of the volume of the reaction kettle; then hydrothermally reacting at 150° C.-200° C. for 10-12 hours; then cooling, centrifuging and drying to obtain a crude catalyst precursor B; (3) ball-milling the crude catalyst precursor B, and then sieving it with a sieve to obtain a catalyst precursor C; (4) placing the catalyst precursor C in a powder feeder, introducing argon and hydrogen at the gas inlet, turning on the microwave power supply to form microwave plasma in the reduction chamber, and then adding the catalyst precursor C into the reduction chamber through the powder feeder for a reduction reaction. After the reduction reaction, the catalyst precursor C is cooled. During the cooling process, the particles are shaped to form catalyst powders of uniform size.

10. The method for preparing a catalyst for synthesizing single-walled carbon nanotubes according to claim 9, characterized in that: The graphene oxide described in step (1) is a single-layer or multi-layer structure, with a sheet diameter of 50 to 500 nm and a specific surface area of ​​300 to 1000 m 2 / g; the iron-based metal element described in step (1) is one or more of iron, cobalt, and nickel; the carbon molar content of the graphene oxide described in step (1) is 1-10%, the molar content of the iron-based metal element is 85-98%, and the molar content of the tellurium element is 1-5%; the pH described in step (1) is 9-10.

11. The method for preparing a catalyst for synthesizing single-walled carbon nanotubes according to claim 10, characterized in that: The iron-based metal element described in step (1) is two or more of iron, cobalt and nickel, specifically iron and nickel or iron and cobalt, and the molar ratio of iron to cobalt or iron to nickel is 5 to 10:1; the carbon molar content of the graphene oxide described in step (1) is 4 to 7%, the molar content of the iron-based metal element is 88 to 95%, and the molar content of the tellurium element is 2-4%.

12. The method for preparing a catalyst for synthesizing single-walled carbon nanotubes according to claim 9, characterized in that: The drying described in step (2) is baking under air atmosphere at 150-200° C. for 8-12 hours.

13. The method for preparing a catalyst for synthesizing single-walled carbon nanotubes according to claim 9, characterized in that: The ball milling described in step (3) is dry milling using a planetary ball mill, wherein the precursor and zirconium beads with a particle size of 0.5 to 3 mm are placed in a ball mill jar of the ball mill for ball milling, and the filling rate of the zirconium beads in the ball mill is 30% to 50%; the ground powder described in step (3) is sieved through a 200-mesh filter to obtain a composite catalyst precursor powder with uniform particle size.

14. The method for preparing a catalyst for synthesizing single-walled carbon nanotubes according to claim 9, characterized in that: The power of the microwave plasma in step (4) is 4 to 75 kW, and the temperature of the microwave plasma is 4000 to 6000 K; the powder supply amount of the powder feeder in step (4) is 10 to 500 g / h; the gas supply amount of the gas inlet in step (4) is 0.1 to 50 m 3 / h, wherein the volume ratio of argon to hydrogen is 1 / 1 to 3 / 1; the cooling described in step (4) is performed by setting a cooling cavity in the cavity, wherein an annular air knife is provided in the cooling cavity, and the angle between the annular air knife and the inner wall of the cooling cavity is 30 to 60°, the cooling gas type is nitrogen or argon, and the air volume in the cooling air knife is 0.5 to 50m 3 / h.

15. A method for preparing single-walled carbon nanotubes by combining the catalyst for synthesizing single-walled carbon nanotubes according to any one of claims 1 to 8 with a chemical vapor deposition method, characterized in that: Specifically: a corundum tube with a diameter of 60-100 cm is used as a reactor, methane is used as a carbon source with a flow rate of 0.05-0.2 L / min, hydrogen is used as a carrier gas with a flow rate of 1-3 L / min, the central temperature of the reactor is adjusted to 1000° C.-1200° C., and the growth time is 20-40 min; after the growth time is up, the introduction of hydrogen and methane is stopped, and argon is introduced at 1-3 L / min to cool to room temperature to obtain single-walled carbon nanotube powder.

16. A device for preparing a catalyst for preparing single-walled carbon nanotubes according to any one of claims 1 to 8, characterized in that: The device comprises a liquid phase coarse powder preparation device and a solid phase microwave plasma synthesis device; the liquid phase coarse powder preparation device comprises a hydrothermal reaction kettle, a centrifuge, a drying device and a grinder; the catalyst precursor obtained by the liquid phase coarse powder preparation device is supplied to the solid phase microwave plasma synthesis device; the solid phase microwave plasma synthesis device comprises a microwave plasma generator, a reduction cavity, a cooling cavity and a collection cavity; the microwave plasma generator, the reduction cavity, the cooling cavity and the collection cavity are connected in sequence from top to bottom.

17. The device for preparing a catalyst for preparing single-walled carbon nanotubes according to claim 16, characterized in that: The reaction temperature of the hydrothermal reactor is 150-200°C, and the volume of the raw materials in the reactor accounts for 60%-80% of the volume of the hydrothermal reactor; the rotation speed of the centrifuge is 8000-15000rpm; the drying process of the drying equipment is drying at 150-200°C in an air atmosphere for 8-12 hours; the grinder is a planetary ball mill, etc., and 0.5-3mm zirconium beads are placed in the ball mill to make the grinding particle size of the powder reach 50-500nm.

18. The device for preparing a catalyst for preparing single-walled carbon nanotubes according to claim 16, characterized in that: The microwave plasma generator comprises a microwave power supply, a microwave plasma torch and a waveguide; the microwave power supply is connected to the waveguide for generating microwaves and transmitting the microwaves through the waveguide; the microwave plasma torch is connected to the waveguide for receiving microwaves.

19. The device for preparing a catalyst for preparing single-walled carbon nanotubes according to claim 18, characterized in that: The power of the microwave power supply is 4-75kw, and the frequency of the microwave is 915MHZ; the waveguide is a metal conduit for transmitting microwaves, which then enter the microwave plasma torch and excite the ignition gas under normal pressure to form microwave plasma.

20. The device for preparing a catalyst for preparing single-walled carbon nanotubes according to claim 18, characterized in that: The microwave is excited and ignited at normal pressure to generate a microwave plasma flame, and the plasma flame extends vertically from top to bottom in the microwave plasma torch; the microwave plasma torch is provided with an inlet pipeline for inputting gas and raw materials, the microwave plasma torch is sealed and connected to the reduction cavity, the diameter of the microwave plasma torch is 30 to 80 mm, and the ignition method is normal pressure excitation.

21. The device for preparing a catalyst for preparing single-walled carbon nanotubes according to claim 20, characterized in that: The inlet pipeline is connected to the exciting gas and the catalyst precursor powder feeding device; the powder feeding speed in the catalyst precursor powder feeding device is 10g / h to 5kg / h.

22. The device for preparing a catalyst for preparing single-walled carbon nanotubes according to claim 18, characterized in that: The reduction cavity is made of stainless steel, with an inner diameter of Φ100-400mm, a length of 150-500mm, and a wall thickness of 8-15mm; the cooling cavity is made of stainless steel, with an inner diameter of Φ100-400mm, a length of 150-500mm, and a wall thickness of 8-15mm; an annular wind knife is arranged in the cooling cavity, and the angle of the annular wind knife and the inner wall of the cooling cavity are 30-60°, and the air volume in the annular wind knife is 0.5-50m 3 / h, the gas blown in by the annular wind knife is argon or nitrogen; the collecting cavity is made of stainless steel and is sealed and connected to the cooling cavity; an exhaust device is provided on the collecting cavity to discharge the exhaust gas; the catalyst powder can be collected after gathering at the bottom of the collecting cavity under the action of airflow and gravity.

23. The device for preparing a catalyst for preparing single-walled carbon nanotubes according to claim 22, characterized in that: The collecting cavity and the reducing cavity are both provided with observation windows; the microwave plasma extends from the microwave plasma torch to the reducing cavity.

Citation Information

Patent Citations

  • Catalyst taking graphene as carrier and carbon nano-material prepared by catalyst

    CN103691446A

  • Porous graphene / nickel tellurium composite catalyst as well as preparation method and application thereof

    CN108539216A

  • CoTe nanowire-graphene composite material and preparation method thereof

    CN109742378A

  • Method for modifying cerium-based catalyst with chlorine resistance enhanced by plasma

    CN116809053A

  • Method for macroscopically preparing single-walled carbon nanotubes with concentrated chirality and application of macroscopically preparing single-walled carbon nanotubes

    CN117023566A