High-definition biaxially oriented polyester film and its coating process

By using PET raw materials with low crystallinity and organic additives, combined with airflow drying and infrared heating technology, the coating process is optimized, and the problem of fillers affecting optical performance and coating process complexity is solved, and high transparency and clarity are achieved The film production simplifies the equipment structure and installation process.

CN118698837BActive Publication Date: 2024-11-15CHANGZHOU ZHONGHENG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411198306.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

In the production of high-definition bidirectional stretch polyester films, the addition of fillers causes the optical performance to be affected, and the online coating process is complex, the area is occupied, and the installation is troublesome, making it difficult to improve the clarity and transparency of the film.

Method used

Using PET raw materials and organic additives with low crystallinity, optimized through airflow drying, airflow heating, infrared heating and other processes, a simplified coating process flow is designed, reflow treatment is eliminated, and improved coating liquid feeding device and coating are used. The concave roller structure reduces equipment components and footprint.

Benefits of technology

It improves the transparency and clarity of the film, reduces haze, simplifies the online coating process, reduces equipment complexity and installation difficulty, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118698837B_ABST
    Figure CN118698837B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-definition biaxially oriented polyester film and its coating process. The polyester film is composed of PET raw material and organic additives. The high-definition biaxially oriented polyester film PET raw material is obtained after drying, melting, casting, longitudinal stretching, cooling, transverse stretching, heat setting and cooling. The crystallinity of the PET raw material is less than 2%. The organic additive is cross-linked polystyrene, and the amount is 1-5% of the PET raw material. The coating process of the high-definition biaxially oriented polyester film includes the preparation of the coating liquid, the supply of the coating liquid, the film corona treatment, and the gravure roller coating. The present invention selects PET raw materials with low crystallinity, and the transparency of BOPET is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a general process for coating a surface with a fluid, and in particular to a high-definition biaxially stretched polyester film and a coating process thereof. Background Art

[0002] High-definition biaxially oriented polyester film is mainly used for electronic product protection, building environmental protection and energy-saving window film, automobile glass film and release protective film, and film for LCD backlight assembly. Patent with publication number CN1579742A: A highly transparent multi-layer co-extruded biaxially oriented polyester film and its production method, the biaxially oriented polyester film contains two surface layers A and C, and an intermediate layer B. The surface A and C layers contain anti-adhesion agents, and the intermediate B layer can use recycled slices. The present invention also discloses a production method of the biaxially oriented polyester film, including the steps of preparing polyester raw materials, extruding, casting, stretching, heat setting, relaxation, pulling, and winding. The clarity of the biaxially oriented polyester film is improved by selecting additives. Patent publication number CN103612405B: According to the mass percentage, 0.1-0.3% curing agent is added to 0.2-0.9% pure water or ionized water and stirred evenly, and then 2.4-12.5% ​​adhesive, 0.4-3.8% silica sol, 0.02-0.1% surfactant and 0.5-2.0% organic solvent are added, and the remaining amount of pure water or ionized water is added after stirring evenly to prepare a water-based coating liquid with a viscosity of less than 10cps and a solid content of 3-12% for standby use, and the core layer polyester chips and the surface layer mixture are added. The cast sheet with three-layer structure is sent to the main and auxiliary extruders for melting and extrusion, and is heated and longitudinally stretched to form a film. The aqueous coating liquid is evenly coated on the film, and the coated film is transversely stretched, heat-set, dried and solidified, and then pulled and rolled to obtain a polyester film... In the process of producing biaxially stretched polyester film, in order to prevent the film from contacting with the roller and scratching during the rolling process, and to prevent the film from sticking after rolling, inorganic or organic fillers are often added to the film to increase the smoothness between the films, so as to prevent the above phenomenon from occurring. This method has a certain impact on the optical properties of the film due to the difference in refractive index between the filler and the polyester material, and the product haze is generally high. The currently disclosed "a kind of optical polyester film and its preparation method" has fillers added to the entire thickness direction of the coating base film. Although it is helpful to avoid scratches that may be caused by contact between the substrate and the longitudinal pulling roller before coating, this method has a greater impact on the optical properties of the film than adding fillers only to the surface layer of the three-layer co-extruded substrate. In order to improve the optical performance of polyester film, some people choose not to use fillers, which will inevitably cause scratches at the longitudinal pulling before coating, affecting the appearance of the final product... The surface layer mixture is a mixture of 90-97% polyester chips and 3-10% polyester masterbatch by mass, and the polyester masterbatch contains 0.3% inorganic filler or organic filler. By adding a small amount of filler to the surface layer, it reduces the cost of film production while reducing the impact of fillers added to the substrate on the optical properties of the film. It has high light transmittance and low haze. However, they only improve clarity by changing additives, and there is no technical means in the prior art to improve clarity through other technical improvement paths.

[0003] High-definition biaxially oriented polyester film can be coated with PVDC to improve its heat sealing, barrier and printing adhesion. The coating liquid prepared for coating is generally water-based, and the basic components are water, leveling agent (to make the coating liquid evenly dispersed), functional coating liquid (to provide the main function of the coating liquid), curing agent (also known as cross-linking agent, which reacts with the resin through the drying process to make the resin firmly bonded to the film surface) and catalyst. Coating is compared with other surface treatment methods as follows: no offline rewinding is required, coating is applied between longitudinal stretching and transverse stretching, and the transverse stretching section is used as an oven to dry the coating liquid, which has high production efficiency; and because the coating is uniform, the coating is thinner than offline coating, and the coating effect is better, which can significantly reduce the coating cost. The surface tension of the film treated with corona will gradually decay over time, and there is no corona decay problem on the surface of the film treated with coating. The coating process is generally as follows: after the polyester film is longitudinally stretched by the longitudinal stretching equipment, the corona equipment is required to perform corona treatment on the surface of the film to increase the surface tension of the film and enhance the wetting performance. At the same time, the intermediate pump pumps the coating liquid in the intermediate material tank into the closed scraper cavity, and the concave roller transfers the coating liquid in the cavity to the surface of the film through the contact angle with the film, forming a coating layer on the surface of the film. The film coated with the coating liquid then enters the transverse stretching equipment. In the transverse stretching preheating section, the coating liquid evaporates water through the drying process, and finally forms a uniform chemical treatment layer on the surface of the film. Existing technology such as Zhao Fu's paper "A Brief Discussion on Online Coating Technology of Polyester Film" published in "China Packaging Industry" in 2013 mentioned: The online coating equipment of polyester film usually consists of a coating liquid feeding device, a corona device, a kiss coating guide roller, a coating scraper cavity, a coating concave roller, a coating rubber pressure roller, an S-shaped lead-out roller, etc. ... 2.3 scraper cavity. The scraper cavity consists of a cavity and a coating scraper. The scraper cavity is in close contact with the coating concave roller in the working state, and the coating liquid is transferred to the coating concave roller. The coating scraper is used to remove excess coating liquid on the coating roller so that the coating liquid is evenly distributed on the coating roller. The replaceable coating scraper is usually made of stainless steel... The concave roller transfers the coating liquid in the cavity to the surface of the film through the contact angle with the film to form a coating layer on the surface of the film. Another example of the prior art is Wu Jianping's paper "Analysis of Factors Affecting the Stability of Online Coated Film Production in Polyester Film Production" published in "Plastic Packaging" Vol. 19, No. 4, 2009. It is mentioned that the coating head consists of a coating liquid feeding area, a coating knife, and a coating knife holder. The coating liquid feeding area is used to transfer the coating liquid to the coating wheel, and the coating knife is used to remove excess coating liquid on the coating roller so that the coating liquid is evenly distributed on the coating roller. The coating knife is usually made of steel or plastic and other materials, and the coating knife holder is used to fix the coating knife. Combined with the diagram, it can be seen that the coating liquid feeding area (that is, its Figure 2The component marked 4 in the figure) is the scraper chamber, and it is found through these two prior arts that the scraper chamber is in close contact with the coating roller (or coating concave roller), and the scraper chamber is either vertically or inclined, but both require reflux treatment of the coating liquid (that is, reflux equipment is required, please refer to the prior art: Li Mingyong’s paper "Overview and Prospect of the Development of Online Coating of Functional Polyester Film" published in "Polyester Industry" Vol. 36, No. 1, 2023-01 mentioned: The main equipment for online coating is composed of a coating liquid supply device, a corona device, a coating head, an S-shaped lead-out roller, etc. The coating liquid supply device transports the configured coating liquid to the coating head and is equipped with a reflux device. The entire liquid supply system is a circulation system), which makes the online coating process complicated, with more processing steps, and the online coating processing equipment is complicated, occupies a lot of space, and is troublesome to install. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects in the prior art and provide a coating process for a high-definition biaxially oriented polyester film. A PET raw material with a lower crystallinity is selected, and the haze of the BOPET film (i.e., biaxially oriented polyester film) is reduced, so the transparency of the BOPET is increased and the clarity is improved; an organic additive is selected in the formula instead of an inorganic additive. Since the refractive index of the organic additive is similar to that of the PET resin and the compatibility with the PET resin is good, the effect on the transparency of the product is relatively small.

[0005] To achieve the above purpose, the technical scheme of the present invention is to design a coating process for high-definition biaxially oriented polyester film, which is composed of PET raw materials and organic additives; the PET raw materials are selected from one or more of polyethylene terephthalate, polybutylene terephthalate, or copolyesters thereof; the high-definition biaxially oriented polyester film PET raw materials are obtained after drying, melting, casting, longitudinal stretching, cooling, transverse stretching, heat setting and cooling; the crystallinity of the PET raw materials is less than 2%; the organic additives are cross-linked polystyrene or polymethacrylate, and the amount is 1-5% of the PET raw materials. As the crystallinity of PET increases, the haze of BOPET film increases, that is, the transparency of BOPET decreases; therefore, under the premise of ensuring the quality of the film, this scheme selects PET raw materials with lower crystallinity; the commonly used additives for BOPET film include inorganic particles such as silicon dioxide, calcium carbonate, aluminum oxide, kaolin, and organic particles such as cross-linked polystyrene. Since the refractive index of the organic additive is similar to that of the PET resin and the compatibility with the PET resin is good, the effect on the transparency of the product is relatively small. Therefore, this solution uses organic additives in the formula instead of inorganic additives. As the additive content increases, the scattered light increases and the haze of the film increases accordingly; therefore, when producing BOPET film, a reasonable formula should be used to avoid adding excessive additives as much as possible; the additive content in this solution is relatively low.

[0006] A further technical solution is that the water content of the PET raw material before drying is 0.4%, and the water content after drying is less than 20 mg / kg; the PET raw material is dried by airflow drying, and the fluid uses heated air with a dew point temperature below -40°C; the drying time is 4 hours. The water content of PET resin decreases with the increase of drying temperature; it decreases with the increase of drying time, but when the drying time reaches a certain value, the water content no longer decreases, so the present application reasonably controls the drying time. During the airflow drying process, the moisture content of the heated air is an important factor affecting the evaporation rate of water in the slices. The lower the moisture content of the heated air, the greater the difference with the moisture content of the slices, and the easier it is for the moisture in the slices to evaporate and be carried away by the air. Therefore, this scheme uses heated air with a dew point temperature below -40°C, and the airflow drying effect is good.

[0007] A further technical solution is that in the preheating process in the longitudinal stretching process, the preheating temperature is about 80±2°C; the temperature of the stretching process is less than 90°C; the stretching ratio is less than 3.17; and after the longitudinal stretching, the film is quenched at a temperature less than 35°C;

[0008] In the transverse stretching process, there are four processes including preheating, stretching, heat treatment and cooling; the preheating temperature is 82-90°C; the stretching temperature is 95-110°C; the stretching ratio is less than 4; and the heat setting temperature is 220-230°C. The sheet needs to be preheated before stretching, until the temperature of the preheating roller in the longitudinal stretching preheating zone gradually increases before stretching. In order to make the sheet reach uniform internal and external temperature distribution in a short time, an infrared heater can be used for further heating to control the preheating temperature at about 82°C; the film after longitudinal stretching is quenched at a temperature of less than 35°C, which can reduce the crystallization rate and create good processing conditions for transverse stretching. The heat setting temperature of transverse stretching is 220-230°C, avoiding the crystallization temperature of 190°C at the maximum crystallization rate (and it is well known to those in the field: PET is a crystalline material, the light transmittance of the crystalline material is closely related to the crystallinity, the high crystallinity has poor light transmittance, and the influence of crystallinity in production is closely related to the cooling rate of the molten material).

[0009] The present invention also provides a technical solution, which is a coating process for a high-definition biaxially oriented polyester film, which is used for coating a high-definition biaxially oriented polyester film, and is composed of the following process steps performed in sequence:

[0010] Preparation of coating liquid, supply of coating liquid, film corona treatment, gravure roller coating; wherein the gravure roller coating process also includes overflow reflux treatment of the coating liquid.

[0011] The present invention also provides a technical solution, which is a coating process for a high-definition biaxially oriented polyester film, which is used for coating a high-definition biaxially oriented polyester film, and is composed of the following process steps performed in sequence:

[0012] Preparation of coating liquid, supply of coating liquid, film corona treatment, gravure roller coating;

[0013] In the gravure roller coating process, the gravure roller carries more coating liquid, and the excess coating liquid falls back to the gravure roller coating station instead of flowing back to the coating liquid preparation station. This solution eliminates the reflux treatment process, and by allowing the excess coating liquid to fall back to the gravure roller coating station, there is no need for a reflux device, eliminating the reflux treatment, streamlining the online coating process, reducing the treatment process, simplifying the online coating processing equipment, reducing the equipment footprint, and reducing the number of equipment components, making installation easier.

[0014] The present invention also provides a technical solution, which is a coating processing device for high-definition biaxially oriented polyester film, which is used in the coating process of high-definition biaxially oriented polyester film, and is composed of a corona device, a scraper chamber, a coating concave roller and a coating liquid preparation device which are arranged in sequence; the coating liquid preparation device is composed of a liquid preparation tank, a liquid supply pump and an intermediate tank; the liquid preparation tank, the liquid supply pump and the intermediate tank are connected through a liquid supply pipe;

[0015] The rotation direction of the coating roller is opposite to the forward direction of the film; the groove on the surface of the coating concave roller is higher along the rotation direction away from the film so that the coating concave roller carries more coating liquid; a liquid level gauge is arranged in the scraper chamber, and the liquid level gauge is connected to the controller signal; the controller is outside the coating processing equipment, and the controller is connected to the liquid supply pump signal in the coating liquid feeding device. Through the improvements in the scraper chamber, the coating concave roller and the liquid supply control, the reflux process is eliminated. The liquid supply of the coating liquid feeding device can be controlled according to the signal of the liquid level gauge in the scraper chamber, avoiding the method of using excess liquid supply and then reflux in the prior art.

[0016] The advantages and beneficial effects of the present invention are: when the crystallinity of PET increases, the haze of BOPET film increases, that is, the transparency of BOPET decreases; therefore, under the premise of ensuring the quality of the film, this solution selects PET raw materials with lower crystallinity; the commonly used additives for BOPET film include inorganic particles such as silicon dioxide, calcium carbonate, aluminum oxide, kaolin, and organic particles such as cross-linked polystyrene. Since the refractive index of organic additives is similar to that of PET resin and the compatibility with PET resin is good, the effect on the transparency of the product is relatively small. Therefore, this solution selects organic additives in the formula instead of inorganic additives.

[0017] As the content of additives increases, the scattered light increases and the haze of the film increases accordingly; therefore, when producing BOPET film, a reasonable formulation should be adopted and additives should not be added excessively as much as possible; the amount of additives used in this solution is relatively small.

[0018] The water content of PET resin decreases with the increase of drying temperature; it decreases with the increase of drying time, but when the drying time reaches a certain value, the water content no longer decreases, so this application reasonably controls the drying time. During the airflow drying process, the moisture content of the heated air is an important factor affecting the evaporation rate of water in the slices. The lower the moisture content of the heated air, the greater the difference with the moisture content of the slices, and the easier it is for the moisture in the slices to evaporate and be carried away by the air. Therefore, this scheme uses heated air with a dew point temperature below -40°C, and the airflow drying effect is better.

[0019] The sheet needs to be preheated before stretching, and the temperature of the preheating roller in the longitudinal stretching preheating zone gradually increases before stretching. In order to make the sheet achieve uniform temperature distribution inside and outside in a short time, an infrared heater can be used for further heating to control the preheating temperature at around 82°C; the film after longitudinal stretching is quenched at a temperature below 35°C, which can reduce the crystallization rate and create good processing conditions for transverse stretching.

[0020] The heat setting temperature for transverse stretching is 220~230℃, avoiding the crystallization temperature of 190℃ at the maximum crystallization rate.

[0021] This solution eliminates the reflux treatment process and allows the surplus coating liquid to fall back to the gravure roller coating station, so there is no need for a reflux device, eliminating the reflux treatment, streamlining the online coating process, reducing the treatment process, simplifying the online coating processing equipment, reducing the equipment footprint, and reducing the number of equipment components, making installation easier.

[0022] Through the improvement of the scraper chamber, coating concave roller and liquid supply control, the reflux process is eliminated. The liquid supply of the coating liquid feeding device can be controlled according to the signal of the liquid level meter in the scraper chamber, avoiding the existing technology of using excess liquid supply and then reflux. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of a second embodiment of a coating processing device for a high-definition biaxially oriented polyester film according to the present invention;

[0024] Figure 2 yes Figure 1 An enlarged schematic diagram of the middle scraper chamber, coating concave roller and coating pressure roller;

[0025] Figure 3 yes Figure 2 A magnified schematic diagram of part A;

[0026] Figure 4 It is an enlarged schematic diagram of the scraper chamber and the coating concave roller in the third embodiment of the present invention;

[0027] Figure 5 yes Figure 4 A magnified schematic diagram of part B;

[0028] Figure 6 yes Figure 4 Side view of part B;

[0029] Figure 7 yes Figure 6 A magnified schematic diagram of part C;

[0030] Figure 8 yes Figure 6 A three-dimensional perspective view of a groove and a groove plate;

[0031] Fig. 9 yes Figure 8 Schematic diagram of the decomposition of

[0032] Fig.10 is a schematic diagram of a fourth embodiment of the present invention;

[0033] Fig.11 yes Fig.10 An enlarged schematic diagram of the middle coating gap roller, the coating film lead-out roller and some of the nearby components.

[0034] In the figure: 1. corona device; 2. scraper chamber; 3. coating concave roller; 4. coating pressure roller; 5. liquid preparation tank; 6. liquid supply pump; 7. intermediate tank; 8. film; 9. groove; 10. liquid level gauge; 11. controller; 12. slot plate; 13. spring; 14. coating spacing roller; 15. coating film lead-out roller; 16. steering roller; 17. proportional valve; 18. infrared heater. DETAILED DESCRIPTION

[0035] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.

[0036] Embodiment 1: The present invention is a coating process for high-definition biaxially oriented polyester film, which is composed of PET raw materials and organic additives; the PET raw materials are selected from one or more of polyethylene terephthalate, polybutylene terephthalate, or their copolymerized polyesters; the high-definition biaxially oriented polyester film PET raw materials are obtained after drying, melting, casting, longitudinal stretching, cooling, transverse stretching, heat setting and cooling; the crystallinity of the PET raw materials is less than 2%; the organic additives are cross-linked polystyrene or polymethacrylate, and the amount is 1-5% of the PET raw materials. The water content of the PET raw materials before drying is 0.4%, and the water content after drying is less than 20mg / kg; the PET raw materials are dried by airflow drying method, and the fluid uses heated air with a dew point temperature below -40℃; the drying time is 4h. In the preheating process in the longitudinal stretching process, the preheating temperature is about 80±2°C; the temperature of the stretching process is less than 90°C; the stretching ratio is less than 3.17; after longitudinal stretching, it is quenched at a temperature less than 35°C; in the transverse stretching process, it includes four processes: preheating, stretching, heat treatment and cooling; the preheating temperature is 82-90°C; the stretching temperature is 95-110°C; the stretching ratio is less than 4; and the heat setting temperature is 220-230°C.

[0037] The coating process of high-definition biaxially oriented polyester film is used for coating high-definition biaxially oriented polyester film, and is composed of the following process steps in sequence:

[0038] Preparation of coating liquid, supply of coating liquid, film corona treatment, gravure roller coating; wherein the gravure roller coating process also includes overflow reflux treatment of the coating liquid.

[0039] Embodiment 2: The difference from Embodiment 1 is that Figures 1 to 3 As shown, the coating process of high-definition biaxially oriented polyester film is used for coating the high-definition biaxially oriented polyester film, and is composed of the following process steps performed in sequence:

[0040] Preparation of coating liquid, supply of coating liquid, film corona treatment, gravure roller coating;

[0041] In the gravure roller coating process, the gravure roller carries more coating liquid, and the excess coating liquid falls back to the gravure roller coating station instead of flowing back to the coating liquid preparation station.

[0042] The coating processing equipment for high-definition biaxially oriented polyester film is used in the coating process of high-definition biaxially oriented polyester film, and is composed of a corona device 1, a scraper chamber 2, a coating concave roller 3 and a coating liquid preparation device which are arranged in sequence (of course, a coating pressure roller 4 is arranged on the opposite side of the coating concave roller 3, that is, on the other side of the film 8); the coating liquid preparation device is composed of a liquid preparation tank 5, a liquid supply pump 6, and an intermediate tank 7; the liquid preparation tank 5, the liquid supply pump 6 and the intermediate tank 7 are connected through a liquid supply pipe; the liquid supply pump 6 inputs the coating liquid in the liquid preparation tank 5 into the intermediate tank 7 through the liquid supply pipe The intermediate tank 7 then inputs the coating liquid into the scraper chamber 2 through a pipeline (a liquid feed pump can be provided on the pipeline); the rotation direction of the coating concave roller 3 is opposite to the forward direction of the film 8; the side of the groove 9 on the surface of the coating concave roller 3 away from the film 8 along the rotation direction is higher so that the coating concave roller 3 carries more coating liquid; a liquid level meter 10 is provided in the scraper chamber 2, and the liquid level meter 10 is connected to the controller 11 by signal; the controller 11 is outside the coating processing equipment, and the controller 11 is connected to the liquid feed pump 6 in the coating liquid feeding device by signal. The bottom wall of the scraper chamber is inclined to the horizontal plane; the size of the scraper chamber is larger than that of the conventional scraper chamber; the scraper chamber is inclined to the horizontal plane (or vertical plane) and the direction from the lower end to the upper end of the scraper chamber is along the direction of the film (or conveying) (this can ensure that the groove on the coating roller carries more coating liquid without leakage).

[0043] The liquid supply of the coating liquid feeding device can be controlled according to the signal of the liquid level meter in the scraper chamber, avoiding the method of using surplus liquid supply and then reflux in the prior art. According to the method of ensuring the coating amount in the prior art (such as the adhesive consumption in the glue storage barrel, in the field of online coating of biaxially stretched polyester film, that is, the consumption of coating liquid in the scraper chamber), when the coating liquid in the scraper chamber exceeds the set value (indicating that either the surplus coating liquid from the coating concave roller flows into the scraper chamber, or the liquid supply pump pumps too much coating liquid), the liquid level meter receives a signal at this time, and the controller controls the liquid supply pump to reduce the liquid supply until the liquid level of the coating liquid in the scraper chamber returns to the preset set value. With the scraper chamber with an enlarged size and an inclined setting, there is no need to worry about the problem of coating liquid overflowing, and it also solves the problem of the prior art requiring reflux treatment and a reflux device.

[0044] The doctor blade chamber is still inclined, but with a larger size. Based on the basic principle that "the running direction of the coating roll needs to be set opposite to the advancing direction of the film to achieve the purpose of transferring the coating liquid", the groove on the surface of the concave coating roll (it is known from the prior art that the coating roll is a metal roll with fine grooves on the surface) is set higher on one side to carry more coating liquid; and a liquid level gauge is provided on the doctor blade chamber with an enlarged size, and the liquid level gauge is connected to the controller by signal; the controller is located outside the on-line coating processing equipment, and the controller is connected to the coating liquid feeding device by signal; in this way, no reflux treatment is required, and the excess coating liquid on the coating roll is brought back into the doctor blade chamber with an enlarged size. The liquid supply amount of the coating liquid feeding device can be controlled only according to the signal of the liquid level gauge in the doctor blade chamber, avoiding the way of using an excessive liquid supply amount and then refluxing in the prior art, streamlining the on-line coating process flow, reducing the processing procedures, simplifying the on-line coating processing equipment, reducing the equipment footprint, and the reduction of equipment components makes the installation easier. After such a setting, through the improvements in aspects such as the doctor blade chamber, the coating roll, and the control of the liquid supply amount, the reflux treatment is removed.

[0045] Since the prior art uses the way of overflow or excess coating liquid to ensure the integrity of the on-line coating of the film (or to avoid the lack of coating liquid on some surfaces of the film during coating), and then the excess coating liquid is refluxed. Now, by increasing the height of the groove on the surface of the concave coating roll, it still provides excess coating liquid (because the increase in the height of one side of the groove makes the carried coating liquid more), so it still ensures the integrity of the on-line coating of the film (or to avoid the lack of coating liquid on some surfaces of the film during coating), and through the improvements in aspects such as the doctor blade chamber, the coating roll, and the control of the liquid supply amount, the reflux treatment is removed.

[0046] Embodiment 3: The difference from Embodiment 2 is that, as Figures 4 to 9 shown, the side of the groove 9 on the surface of the concave coating roll 3 that is farther away from the film along the rotation direction is higher by adding a movable groove side wall on the basis of the original groove with equal groove depth, that is, a blind hole-shaped slot is provided on the top wall of the groove 9, and a groove plate 12 with a shape similar to half of the groove is slidably arranged in the slot (generally, the groove is in a rectangular ring shape; so the groove plate 12 is in a semi-rectangular ring shape, that is, in a "U" shape), the thickness of the groove plate 12 is less than the wall thickness of the groove 9, the bottom wall of the groove plate is fixedly connected with a spring 13 (when the groove plate is not stressed, that is, when the spring is only affected by the gravity of the groove plate, the upper end surface of the groove plate exceeds the top wall of the groove), and a sliding seal is provided at the slot, so as to ensure the sealing performance (because only in this way can it be ensured that more coating liquid is really carried, and to avoid the excess coating liquid carried from flowing out between the groove plate and the slot during the up and down sliding of the groove plate).

[0047] After such arrangement, when the coating concave roller 3 rotates (its running direction is opposite to the forward direction of the film), the groove 9 on the coating concave roller first carries the coating liquid in the scraper chamber 2, and because the groove on the coating concave roller contacts the scraper chamber 2 first, the groove 9 that contacts the scraper chamber first is not subjected to force (not subjected to the pressure of the film), so the groove plate 12 exceeds the top wall of the groove, and cooperates with the sliding seal, so compared with the groove in the prior art, it can carry more coating liquid (so the overflow of the prior art is still adopted, that is, the surplus liquid supply to ensure sufficient coating on the film surface), and when the groove 9 on the coating concave roller 3 rotates and After the polyester film is in contact, the groove plate 12 on the groove retracts due to pressure (not only the pressure of the film, but also the pressure of the coating roller) (that is, the groove plate retracts into the groove, and the spring 13 is compressed), and a part of the extra coating liquid flows to the surface of the film, and the other part flows back to the scraper cavity due to the expansion of the size of the scraper cavity 2; in order to ensure that no reflux device is required and the reflux treatment is omitted, the scraper cavity 2 can be set to a semi-annular shape (in this way, the entire coating concave roller can be "enclosed", effectively preventing the coating liquid from flowing out from the other side of the coating concave roller and leaving the coating concave roller and dripping onto the workshop floor where the coating equipment is located).

[0048] Embodiment 4: The difference from Embodiment 2 is that Fig.10 , Fig.11 As shown, the coating processing equipment for high-definition biaxially oriented polyester film is used in the coating process of high-definition biaxially oriented polyester film, and is composed of a corona device 1, a coating liquid preparation device, two coating spacing rollers 14 and a coating film lead-out roller 15 which are arranged in sequence (the film 8 is located below the coating spacing roller 14 and the coating film lead-out roller 15); the distance between the two coating spacing rollers 14 and the film 8 gradually decreases along the film forward direction; the coating liquid preparation device is composed of a liquid preparation tank 5, a liquid supply pump 6, and an intermediate tank 7; the liquid preparation tank 5, the liquid supply pump 6 and the intermediate tank 7 are connected through a liquid supply pipe; the liquid supply pump 6 passes the liquid supply pipe to The coating liquid in the liquid preparation tank 5 is input into the intermediate tank 7, and the intermediate tank 7 then inputs the coating liquid onto the film 8 located between the steering roller 16 and the coating film lead-out roller 15 through a pipeline (a liquid feed pump may be provided on the pipeline); a proportional valve 17 is provided on the liquid supply pipe, and the proportional valve 17 is connected to the controller 11 signal of the coating processing equipment located in the high-definition biaxially oriented polyester film, and the controller 11 is also connected to the liquid supply pump 6 signal; an infrared heater 18 is provided between two coating spacing rollers 14 arranged in sequence; an infrared heater 18 is also provided between the coating film lead-out roller 15 and the coating spacing roller 14 located below (i.e., lower).

[0049] After such arrangement, the required output amount of the coating liquid can be calculated according to the inclination angle of the film 8 between the steering roller 16 and the coating film lead-out roller 15 and the conveying speed of the film. The controller controls the liquid supply pump 6 to open and controls the opening of the proportional valve 17, so as to avoid the problem of too much coating liquid supply. The coating spacing roller 14 gradually approaches the film 8 to ensure the thickness of the coating liquid coated on the surface of the film 8. An infrared heater 18 is arranged between the two coating spacing rollers 14 arranged in sequence; an infrared heater 18 is also arranged between the coating film lead-out roller 15 and the coating spacing roller 14 located below (that is, lower), so that the pre-heating process in the horizontal stretching process can be eliminated; and the simultaneous use of infrared heating during coating can ensure the stability of the coating liquid thickness. This setting changes the original preparation process. Compared with the method of applying the coating liquid from the lower surface of the film 8, it can better keep the workshop floor clean and avoid waste of coating liquid. With the inclined setting of the film, the coating liquid is first input at the upper end of the inclined film, so a slightly larger amount of coating liquid than the calculated supply can be output. The subsequent coating spacing roller 14 and the infrared heater 18 can ensure the thickness of the coating liquid. There is no need to worry about the lack of coating liquid on part of the film surface, and overflow caused by too much supply can be avoided.

[0050] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. Coating process for high-definition biaxially oriented polyester film, used for coating treatment of high-definition biaxially oriented polyester film, Characterized in that, It consists of the following technological steps carried out in sequence: Preparation of coating liquid, supply of coating liquid, corona treatment of film, gravure coating; In the gravure coating process, more coating liquid is carried on the gravure roll; The surplus coating liquid falls back to the gravure coating station instead of flowing back to the coating liquid preparation station; Coating processing equipment for high-definition biaxially oriented polyester film, used in the coating process of high-definition biaxially oriented polyester film, is composed of a corona device, a doctor blade chamber, a coating gravure roll and a coating liquid preparation device arranged in sequence. A coating pressure roll is provided on the opposite side of the coating gravure roll, that is, on the other side of the film. The coating liquid preparation device is composed of a liquid mixing tank, a supply pump and an intermediate tank. The liquid mixing tank, the supply pump and the intermediate tank are connected by a supply pipe. The supply pump inputs the coating liquid in the liquid mixing tank into the intermediate tank through the supply pipe, and the intermediate tank then inputs the coating liquid into the doctor blade chamber through a pipeline, and a liquid feeding pump is arranged on the pipeline. The rotation direction of the coating gravure roll is opposite to the advancing direction of the film. The groove on the surface of the coating gravure roll is higher on the side away from the film along the rotation direction so that the coating gravure roll can carry more coating liquid. A liquid level gauge is arranged in the doctor blade chamber, and the liquid level gauge is connected to the controller by signal. The controller is outside the on-line coating processing equipment, and the controller is connected to the supply pump in the coating liquid feeding device by signal. The bottom wall of the doctor blade chamber is inclined with respect to the horizontal plane. The size of the doctor blade chamber is larger than that of the conventional doctor blade chamber. The doctor blade chamber is inclined with respect to the horizontal plane or the vertical plane, and the direction from the lower end to the upper end of the doctor blade chamber is along the advancing or conveying direction of the film, so as to ensure that the groove on the coating roll can carry more coating liquid without leakage. The supply amount of the coating liquid feeding device can be controlled according to the signal of the liquid level gauge in the doctor blade chamber; The doctor blade chamber is inclined. Based on the operating direction of the coating roll, it needs to be set opposite to the advancing direction of the film to achieve the purpose of transferring the coating liquid. The groove surface of the coating gravure roll is set higher to carry more coating liquid; A liquid level gauge is arranged on the doctor blade chamber with an enlarged size, and the liquid level gauge is connected to the controller by signal. The controller is outside the on-line coating processing equipment, and the controller is connected to the coating liquid feeding device by signal. In this way, no reflux treatment is required, and the excess coating liquid on the coating gravure roll is brought back into the doctor blade chamber with an enlarged size. The supply amount of the coating liquid feeding device can be controlled only according to the signal of the liquid level gauge in the doctor blade chamber. The groove on the surface of the coating gravure roll is higher on the side away from the film along the rotation direction by adding a movable groove side wall on the basis of the original groove with equal depth, that is, a blind hole-shaped slot is arranged on the top wall of the groove, and a slot plate similar to half of the shape of the groove is slidably arranged in the slot. The groove is a rectangular ring. So the slot plate is a semi-rectangular ring, that is, a "U" shape. The thickness of the slot plate is less than the wall thickness of the groove. The bottom wall of the slot plate is fixedly connected with a spring. When the slot plate is not stressed, that is, when the spring is only affected by the gravity of the slot plate, the upper end surface of the slot plate exceeds the top wall of the groove. A sliding seal is arranged at the slot to prevent the excess coating liquid from flowing out from the slot plate and the slot during the up and down sliding of the slot plate; When the coating concave roller rotates, its running direction is opposite to the forward direction of the film. The grooves on the coating concave roller first carry the coating liquid in the scraper cavity. Since the grooves on the coating concave roller first contact the scraper cavity, the grooves that first contact the scraper cavity are not subjected to force, that is, they are not subjected to the pressure of the film. Therefore, the groove plate exceeds the top wall of the groove and cooperates with the sliding seal to carry more coating liquid. When the grooves on the coating concave roller contact the polyester film due to rotation, the groove plates on the grooves are under pressure, that is, not only the pressure of the film, but also the pressure of the coating roller, and retract, that is, the groove plates retract into the slots, the springs are compressed, and part of the extra coating liquid flows to the surface of the film, and the other part flows back to the scraper cavity due to the expansion of the scraper cavity size. The scraper cavity is set to a semi-annular shape to "cover" the entire coating gravure roller to prevent the coating liquid from flowing out from the other side of the coating gravure roller and dripping onto the workshop floor where the coating equipment is located after leaving the coating gravure roller.