Preparation method of Ti3Al / (alpha + beta) Ti gradient performance disc and aviation engine compressor disc

By designing stratification and phase change points, using high-energy beam powder feeding additive manufacturing and multi-fire thermal deformation process to prepare Ti3Al/(α+β)Ti gradient performance discs, the material performance mismatch and structural defects in the existing technology are solved. problem, achieving the gradient performance requirements of the aero-engine compressor disk and improving the strength and toughness of the material.

CN118699402APending Publication Date: 2024-09-27AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410723230.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

It is difficult to prepare aero-engine compressor disks with gradient performance using existing technology. A single alloy material cannot meet the working conditions of different parts, and the structural defects and low mechanical properties in the additive manufacturing process cannot meet the needs of the engine.

Method used

Using the preparation method of Ti3Al/(α+β)Ti gradient performance disk, by designing the layering and phase transition points, using high-energy beam powder feeding additive manufacturing and multi-fire thermal deformation process, the composition gradient transition layer is prepared layer by layer, and Perform heat treatment to eliminate metallurgical defects and improve tissue density.

Benefits of technology

It achieves excellent performance in each area of ​​the alloy disk, improves strength, plasticity, toughness and fatigue properties, ensures the continuity of component stratification transition and the density of the structure, and meets the gradient performance requirements of the aeroengine compressor disk.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004877831590000012
    Figure HDA0004877831590000012
  • Figure HDA0004877831590000011
    Figure HDA0004877831590000011
Patent Text Reader

Abstract

The invention provides a preparation method of a Ti3Al / (alpha + beta) Ti gradient performance disc. The preparation method comprises the following steps: designing the size and components of the gradient performance disc; determining the phase transformation point of the transition component layer alloy; designing a thermal deformation heat storage tool; preparing a Ti3Al alloy base ring; forming a gradient performance disc; and heat treatment. In the preparation process of the Ti3Al / (alpha + beta) Ti gradient performance disc, a gradient performance disc blank with component and structure gradient transition is prepared by adopting a radial layer-by-layer high-energy beam powder feeding additive manufacturing and layer-by-layer thermal deformation cogging process, and finally, the Ti3Al / (alpha + beta) Ti gradient performance disc is obtained through a thermal treatment process. The Ti3Al / (alpha + beta) Ti gradient performance disc prepared by the preparation method disclosed by the invention is continuous in component transition and compact in structure, and the performance is optimized. The prepared gradient performance disc can be used for preparing an aviation engine compressor disc, and the gradient performance requirement and the weight reduction requirement are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal heat processing, and in particular to a preparation method of a Ti3Al / (α+β)Ti gradient performance disk and an aviation engine compressor disk. Background Art

[0002] The realization of high thrust-to-weight ratio of aircraft engines requires the improvement of service performance of components on the one hand, and the reduction of weight on the other hand. As a key rotor component in the engine, the compressor disc has gradient performance requirements for the disc body in its service conditions: on the one hand, the disc core to the disc edge is subjected to a temperature gradient from low to high, and the disc core needs to have a medium-low temperature bearing capacity of 300℃ to 400℃, while the disc edge needs to have a high temperature bearing capacity of about 600℃ or even higher; on the other hand, the load-bearing type from the disc core to the disc edge is gradiently transitioned, and the disc core is mainly centrifugal tensile stress, requiring the material to have high strength and plasticity, while the disc edge requires the material to have high creep resistance and fracture toughness. In view of the above performance requirements, the gradient performance requirements pose challenges to the disc manufacturing technology.

[0003] At present, a single alloy is widely used as the compressor disc material in China. The single performance is difficult to meet the operating conditions of different parts. In addition, the disc structure design is conservative and the structure weight is heavy. It has become increasingly difficult to adapt to the lightweight and efficient manufacturing needs of the engine. Therefore, the use of gradient materials to achieve gradient performance has become an urgent need for the preparation of advanced compressor discs.

[0004] The light intermetallic compound material Ti3Al has a maximum use temperature of over 600°C and is an aviation structural material with great application prospects. However, due to the low plasticity of the alloy, it does not meet the performance requirements of the disk core. If Ti3Al is used as the rim material, and the composition and properties (including mechanical properties and temperature resistance) are gradually transitioned from the disk rim to the disk core to the (α+β)Ti two-phase titanium alloy with excellent comprehensive performance and a use temperature of 300°C to 400°C, a gradient performance disk can be prepared, which can fully tap the disk structure and performance potential, and has subversive significance for the development of compressor disks.

[0005] For gradient performance disks, the continuous gradient transition of composition and organizational properties is the key to the development of disks. Domestic and foreign researchers have conducted a lot of research using additive manufacturing processes. By mixing two alloy powders in different proportions, laser cladding composition gradient materials are prepared using additive manufacturing processes to achieve gradient performance. However, the gradient material prepared by this process is an additive dendrite structure and contains microscopic structural defects such as pores and unfused materials, and has low mechanical properties. It cannot meet the use requirements of key rotating parts of engines. In order to achieve the performance requirements of gradient performance disks, the development of Ti3Al / (α+β)Ti gradient performance disks requires the search for new processes and methods. Summary of the invention

[0006] The technical problem solved by the present invention is to provide a method for preparing a Ti3Al / (α+β)Ti gradient performance disk. The preparation method provided by the present application can prepare an alloy disk with excellent comprehensive properties such as strength, plasticity, toughness and fatigue performance, and the alloy disk has the advantages of optimal performance in each region and continuous transition of composition in each region.

[0007] In view of this, the present application provides a method for preparing a Ti3Al / (α+β)Ti gradient performance disk, comprising the following steps:

[0008] S1) According to the structure of the gradient performance disk to be prepared, the gradient performance disk to be prepared is divided into n component layers from the outer edge to the core, and the content of Ti3Al and (α+β)Ti in the component layers is designed, and the component content of the xth layer from the outer edge to the core satisfies the following relationship:

[0009] (nx) / (n-1)×C Ti3Al +(x-1) / (n-1)×C Ti ,

[0010] Among them, C Ti3Al is the composition of Ti3Al alloy, C Ti is (α+β)Ti alloy composition, n≥3;

[0011] S2) respectively determining the phase transition points of each component layer except the outer edge component layer;

[0012] S3) designing a thermal deformation heat storage tool for thermal deformation according to the structure of the gradient performance disk to be prepared;

[0013] S4) preparing a Ti3Al alloy base ring, the size of which after machining is consistent with the size of the outer edge component layer of the gradient performance disk;

[0014] S5) on the basis of the Ti3Al alloy base ring, radially performing high-energy beam powder feeding additive preparation layer by layer according to the component content in step S1), and utilizing the thermal deformation heat storage tooling in step S2) for thermal deformation layer by layer to obtain a gradient performance disk blank;

[0015] S6) heat treating the gradient performance disk blank.

[0016] Preferably, step S2) is specifically:

[0017] The additive cladding process is used to prepare metallographic samples of each component layer in step S1), and then the phase transition point of each metallographic sample is detected.

[0018] Preferably, the thermal deformation heat storage tooling comprises a heat storage outer cylinder, an upper end surface heat storage sleeve ring and a lower end surface heat storage sleeve ring, the inner diameter of the heat storage outer cylinder matches the outer diameter of the gradient performance disk, and the thickness is not less than the radial width of the outer edge component layer; the heat storage sleeve ring is composed of n-1 layers from the secondary outer edge to the core, and the inner diameter / outer diameter of the x-th layer of the heat storage sleeve ring corresponds in sequence to the inner diameter / outer diameter of the x-th layer of the component layer of the gradient performance disk, and the thickness is not less than the thickness of the gradient performance disk.

[0019] Preferably, the Ti3Al alloy base ring is prepared by a plastic deformation process and has a fine forged structure.

[0020] Preferably, step S5) is specifically:

[0021] On the basis of the Ti3Al alloy base ring, from outside to inside, the steps include: the second layer of high-energy beam powder feeding additive preparation → the second layer of thermal deformation → the third layer of high-energy beam powder feeding additive preparation → the third layer of thermal deformation →... → the n-1 layer of high-energy beam powder feeding additive preparation → the n-1 layer of thermal deformation → the n layer of high-energy beam powder feeding additive preparation → the n layer of thermal deformation.

[0022] Preferably, the thermal deformation is in the form of radial thinning deformation, and the thermal deformation temperature is 20 to 50° C. below the phase transition point of the component layer.

[0023] Preferably, the thermal deformation layer by layer using the thermal deformation heat storage tooling in step S2) is specifically as follows: before the thermal deformation of the xth layer, the thermal storage outer cylinder, the 1st to x-1th layers of upper end surface thermal storage rings, and the 1st to x-1th layers of lower end surface thermal storage rings are installed; after the heating is completed, the thermal storage outer cylinder, the 1st to x-1th layers of upper end surface thermal storage rings, and the 1st to x-1th layers of lower end surface thermal storage rings are removed, and then the xth layer is thermally deformed.

[0024] Preferably, the radial thickness of each initial component layer prepared by the high-energy beam powder feeding additive is such that the initial component layer undergoes radial plastic deformation with a thinning rate of 30-70% and the size obtained after machining meets the structural size of the gradient performance disk to be prepared in step S1), and the holding time of each initial component layer prepared by the high-energy beam powder feeding additive at the thermal deformation temperature is the cross-sectional thickness D of the initial layer. x ×(0.6~0.8)min / mm.

[0025] Preferably, the heat treatment temperature is 400-760° C., the time is 2-10 hours, and the heat treatment is air-cooled.

[0026] The present application also provides an aircraft engine compressor disk, which is prepared from a gradient performance disk, and the gradient performance disk is a Ti3Al / (α+β)Ti gradient performance disk prepared by the preparation method.

[0027] The present invention provides a method for preparing a Ti3Al / (α+β)Ti gradient performance disk, which first designs the size and composition of the transition zone of the gradient performance disk, and on this basis determines the phase transition point of each component layer alloy to determine the optimal hot working temperature of each layer, and then prepares the outermost Ti3Al alloy base ring and prepares the composition gradient transition layer layer by layer on the inner side by the method of additive cladding + thermal deformation to obtain a gradient performance disk blank, and finally heat treats the blank to prepare the gradient performance disk. The preparation method provided in the present application obtains a gradient performance disk with dense structure by thermally deforming the gradient transition layer layer by layer, eliminates metallurgical defects such as pores and unfused, and realizes the recrystallization reconstruction of the coarse additive dendrite structure, so that the strength, plasticity, toughness and fatigue performance of the obtained gradient performance disk are significantly improved.

[0028] Furthermore, considering the difference in the optimal hot working temperature caused by the composition change of each transition layer, the phase transition point of each component layer alloy was determined respectively, and the differentiated hot deformation and cogging temperature of each layer was determined accordingly, ensuring the optimal primary α / α2 phase content and grain size of each layer. By using hot deformation heat storage tooling in the multi-fire hot deformation and cogging process and finally only performing low-temperature annealing or aging treatment, the component layer that has obtained the optimal structure is avoided from being deteriorated due to repeated high-temperature thermal cycles, thereby ensuring the optimal performance of each area of ​​the gradient performance disk. At the same time, the hot deformation and cogging process provides a channel for element diffusion through lattice defects such as vacancies and dislocations caused by grain boundary sliding and deformation, further improving the continuity of the composition transition of each layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic diagram of the structure and dimensions of a gradient performance disk in an embodiment of the present invention;

[0030] Figure 2 It is a schematic diagram of the installation of the thermal deformation heat storage tooling during the thermal deformation process of the gradient performance disk in an embodiment of the present invention. DETAILED DESCRIPTION

[0031] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0032] In view of the technical problems of organizational defects and low mechanical properties in the preparation process of gradient materials in the prior art, the present application provides a method for preparing a Ti3Al / (α+β)Ti gradient performance disk, which uses high-energy beam powder feeding additive manufacturing and multi-fire thermal deformation to achieve organizational modification and elimination of metallurgical defects. The final prepared Ti3Al / (α+β)Ti gradient performance disk has continuous transitions between the component layers and excellent mechanical properties. Specifically, the present application provides a method for preparing a Ti3Al / (α+β)Ti gradient performance disk, comprising the following steps:

[0033] S1) According to the structure of the gradient performance disk to be prepared, the gradient performance disk to be prepared is divided into n component layers from the outer edge to the core, and the content of Ti3Al and (α+β)Ti in the component layers is designed, and the component content of the xth layer from the outer edge to the core satisfies the following relationship:

[0034] (nx) / (n-1)×C Ti3Al +(x-1) / (n-1)×C Ti ,

[0035] Among them, C Ti3Al is the composition of Ti3Al alloy, C Ti is (α+β)Ti alloy composition, n≥3;

[0036] S2) respectively determining the phase transition points of each component layer except the outer edge component layer;

[0037] S3) designing a thermal deformation heat storage tooling according to the structure of the gradient performance disk to be prepared;

[0038] S4) preparing a Ti3Al alloy base ring, the size of which after machining is consistent with the size of the outer edge component layer of the gradient performance disk;

[0039] S5) on the basis of the Ti3Al alloy base ring, radially performing high-energy beam powder feeding additive preparation layer by layer according to the component content in step S1), and utilizing the thermal deformation heat storage tooling in step S2) for thermal deformation layer by layer to obtain a gradient performance disk blank;

[0040] S6) heat treating the gradient performance disk blank.

[0041] The Ti3Al / (α+β)Ti gradient performance disk provided by the present application is a Ti3Al component and a (α+β)Ti component that realize a gradient transition of the composition in the alloy disk, rather than a direct compound of the Ti3Al component and the (α+β)Ti component. In the present application, the Ti3Al alloy includes a Ti3Al or Ti2AlNb-based intermetallic compound, and the (α+β)Ti is a two-phase titanium alloy with a use temperature of 300°C to 450°C, including but not limited to TC2, TC4 or TC6 alloys.

[0042] In the preparation process of the Ti3Al / (α+β)Ti gradient performance disk, the present application first designs the structural dimensions of the gradient performance disk, and divides the gradient performance disk into n component layers from the outer edge to the core. For example, from the outer edge to the inner core, there are the first layer, the second layer, the third layer... the n-1th layer, the nth layer in sequence. In the above n component layers, the contents of Ti3Al and (α+β)Ti in each component layer are distributed in a gradient. In the present application, the component contents of the xth layer from the outer edge to the core satisfy the following relationship:

[0043] (nx) / (n-1)×C Ti3Al +(x-1) / (n-1)×C Ti ,

[0044] Among them, C Ti3Al is the composition of Ti3Al alloy, C Ti is (α+β)Ti alloy composition, n≥3;

[0045] According to the above relationship, taking n=4 as an example, the composition of the first layer is Ti3Al, and the composition of the second layer is 2 / 3C Ti3Al +1 / 3C Ti , the composition of the third layer is 1 / 3C Ti3Al +2 / 3C Ti , the 4th layer is C Ti .

[0046] The present application then determines the phase transition points of each component layer except the outer edge component layer to prepare for the thermal deformation of the later transition layer. The determination of the phase transition point is carried out according to the metallographic method well known to those skilled in the art. In order to ensure the accuracy of the phase transition point under the same conditions, the present application adopts an additive cladding process to prepare metallographic samples of each component layer respectively. The raw materials are mixed powders of Ti3Al and (α+β)Ti in different proportions in the above steps; and then the metallographic samples are tested for phase transition points. The additive cladding process is prepared according to the process well known to those skilled in the art, and the present application has no special restrictions on this.

[0047] According to the present invention, a thermal deformation heat storage tooling for thermal deformation is then designed based on the structure of the gradient performance disk to be prepared, the thermal deformation heat storage tooling includes a heat storage outer cylinder, an upper end surface heat storage sleeve ring and a lower end surface heat storage sleeve ring, the inner diameter of the heat storage outer cylinder matches the outer diameter of the gradient performance disk, and the thickness is not less than the radial width of the outer edge component layer; the heat storage sleeve ring is composed of n-1 layers from the outer edge to the core, and the inner diameter / outer diameter of the x-th layer of the heat storage sleeve ring corresponds to the inner diameter / outer diameter of the x-th layer of the gradient performance disk in sequence, and the thickness is not less than the thickness of the gradient performance disk. The thermal deformation heat storage tooling is detachable.

[0048] After the above preparations are completed, the gradient performance disk is prepared. First, a Ti3Al alloy base ring is prepared, and its size after machining should meet the size of the outer edge component layer of the gradient performance disk. The Ti3Al alloy base ring is preferably prepared by a plastic deformation process, specifically, by a ring rolling process, and has a fine forged structure.

[0049] On the basis of the above-mentioned Ti3Al alloy base ring, high-energy beam powder feeding additive manufacturing and thermal deformation are performed radially layer by layer to prepare an alloy disk with a gradient transition of composition; except for the Ti3Al alloy base ring, i.e., the outer edge component layer, the preparation of other component layers includes the following steps from the outer to the inner radial direction: the second layer high-energy beam powder feeding additive manufacturing → the second layer thermal deformation → the third layer high-energy beam powder feeding additive manufacturing → the third layer thermal deformation →... → the n-1 layer high-energy beam powder feeding additive manufacturing → the n-1 layer thermal deformation → the n layer high-energy beam powder feeding additive manufacturing → the n layer thermal deformation. The raw materials in the above-mentioned layers of high-energy beam powder feeding additive manufacturing are the Ti3Al and (α+β)Ti alloy mixed powders of the corresponding proportions of the layer. In the high-energy beam powder feeding additive manufacturing, the stacking direction is from the outer to the inner radial direction of the gradient performance disk. The radial thickness of each initial component layer prepared by the high-energy beam powder feeding additive is such that the initial component layer undergoes radial plastic deformation with a thinning rate of 30 to 70% and the size obtained after machining meets the structural size of the gradient performance disk to be prepared; that is, the radial thickness of each initial component layer prepared by the high-energy beam powder feeding additive should be greater than the structural size of the designed gradient performance disk, so that the size of each initial component layer after thinning and polishing meets the structural size of the designed gradient performance disk; the thinning rate in the present application is 30 to 70% of the radial thickness of each initial component layer, and more specifically 40 to 60%.

[0050] After additive preparation, thermal deformation is performed. Before thermal deformation, the above-mentioned thermal deformation heat storage tooling needs to be installed. After heating, the thermal deformation heat storage tooling is removed and then thermal deformation is performed. Except for the outer edge component layer, i.e., the first layer, after additive preparation of the second layer, the thermal storage outer cylinder, the thermal storage sleeve ring on the upper end face of the first layer, and the thermal storage sleeve ring on the lower end face of the first layer are installed first, and the heating time is the cross-sectional thickness D1×(0.6~0.8)min / mm of the initial component layer of the first layer. After heating, the thermal storage outer cylinder, the thermal storage sleeve ring on the upper end face of the first layer, and the thermal storage sleeve ring on the lower end face of the first layer are removed, and then the thermal deformation of the second layer is performed; after additive preparation of the third layer, the thermal storage outer cylinder, the thermal storage sleeve ring on the upper end face of the first layer, the thermal storage sleeve ring on the lower end face of the first layer, the thermal storage sleeve ring on the upper end face of the second layer, and the thermal storage sleeve ring on the lower end face of the second layer are installed first, and the heating time is the cross-sectional thickness D2×(0.6~0.8)min / mm of the initial component layer of the second layer. After heating, the heat storage outer cylinder, the heat storage sleeve ring on the upper end face of the first layer, the heat storage sleeve ring on the lower end face of the first layer, the heat storage sleeve ring on the upper end face of the second layer and the heat storage sleeve ring on the lower end face of the second layer are removed, and then the third layer is thermally deformed; after the additive preparation of the fourth layer, the heat storage outer cylinder, the heat storage sleeve ring on the upper end face of the first layer, the heat storage sleeve ring on the lower end face of the first layer, the heat storage sleeve ring on the upper end face of the second layer, the heat storage sleeve ring on the lower end face of the second layer, the heat storage sleeve ring on the upper end face of the third layer and the heat storage sleeve ring on the lower end face of the third layer are installed first, and the heating time is the initial component layer section thickness D3×(0.6~0.8)min / mm. After heating, the heat storage outer cylinder, the first layer upper end heat storage sleeve ring, the first layer lower end heat storage sleeve ring, the second layer upper end heat storage sleeve ring, the second layer lower end heat storage sleeve ring, the third layer upper end heat storage sleeve ring and the third layer lower end heat storage sleeve ring are removed, and then the fourth layer is thermally deformed. The thermal deformation temperature should be the alloy phase transition point T of the component layer. βx Below 20℃~50℃, the deformation amount should meet the design requirements of the metal thinning rate of this layer. The specific forming method of the thermal deformation can be carried out in a manner familiar to those skilled in the art, including but not limited to ring rolling, radial forging, and rotary forging. After thermal deformation, the inner side of the metal layer is polished to the design size of the layer to meet the preparation and processing of the subsequent transition component layer, and the upper and lower end surfaces are polished and leveled for the subsequent installation of the heat storage ring to obtain a gradient performance disk blank. The purpose of designing a thermal deformation heat storage tooling is to heat only the deformed component layer to the deformation temperature to soften and thermally deform, so that the deformed component layer can absorb heat through the thermal deformation heat storage tooling, and its actual temperature is controlled to be lower than the deformation temperature and basically does not deform. Therefore, the above-mentioned heating time is limited. If the heating time is too long, the overall heat penetration will lose the purpose of designing the thermal deformation heat storage tooling. The phase transition point gradually decreases from the outer edge component layer to the core component layer. Therefore, during the processing of the second transition layer, the thermal deformation temperature is lower than the deformation temperature of the first layer, and repeated heating has little effect on the performance of the first layer. The purpose of the thermal deformation heat storage tooling is also to ensure that the upper and lower end surfaces of the first layer absorb heat quickly during the heating of the second layer to prevent the first layer from being repeatedly heated to high temperature.

[0051] Finally, the present application performs heat treatment on the above-mentioned gradient performance disk blank, and the heat treatment is specifically low-temperature annealing or aging heat treatment; the heat treatment temperature is 400-760°C, the time is 2-10 hours, and air cooling.

[0052] In order to make the gradient performance disk after heat treatment meet the size requirements, it is preferred to perform finishing processing on the gradient performance disk after heat treatment to obtain the gradient performance disk. The finishing processing is performed in a manner well known to those skilled in the art, and there is no particular limitation in this application.

[0053] The present application also provides an aviation engine compressor disk, which is prepared from a gradient performance disk, and the gradient performance disk is a Ti3Al / (α+β)Ti gradient performance disk prepared by the above preparation method.

[0054] The present invention proposes a method for preparing a Ti3Al / (α+β)Ti gradient performance disk by laser / electron beam powder feeding additive manufacturing + multi-fire variable temperature hot deformation process. The preparation method provided by the present application solves the technical difficulties of poor organization and low performance level in preparing gradient performance disks by a simple additive manufacturing process. The Ti3AL / (α+β)Ti gradient performance disk prepared by the method has a continuous transition in composition and a fine and dense organization, and can achieve the gradient performance requirements of advanced engine compressor disks.

[0055] In order to further understand the present invention, the preparation method of the Ti3Al / (α+β)Ti gradient performance disk provided by the present invention is described in detail below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0056] Example 1

[0057] Φ400mm×60mm (transition layer layer position Φ160mm, Φ240mm, Φ320mm, such as Figure 1 The preparation method of the Ti3Al / TC4 dual alloy disk (shown) comprises the following steps:

[0058] (1) Design of the size and composition of the gradient transition layer of the Ti3Al / TC4 dual alloy disk: According to the structural size of the dual alloy disk, the disk is divided into four composition layers from the outer edge to the core, of which the outermost edge, i.e., the first layer, is a Ti3Al forged ring blank, the second layer from the outer edge to the core has a composition of 67% Ti3Al + 33% TC4, the third layer has a composition of 33% Ti3Al + 67% TC4, and the fourth layer has a composition of TC4 alloy;

[0059] (2) Determination of the phase transition point of the transition layer alloy: The phase transition point is determined by metallographic method. The sample used is a metallographic sample prepared by additive cladding process according to the composition of each transition layer in step (1). The raw materials are mixed powders of Ti3Al and TC4 alloys with different proportions calculated in step (1). The phase transition point of the second layer determined by metallographic method is 1028°C, the phase transition point of the third layer is 1011°C, and the phase transition point of the fourth layer is 995°C.

[0060] (3) Design of forging hot deformation heat storage tooling: According to the structural dimensions of the gradient transition layer in step (1), a detachable hot deformation heat storage tooling for forging heating is designed, as shown in the attached Figure 2 As shown;

[0061] (4) Preparation of Ti3Al alloy base ring: The Ti3Al alloy base ring is prepared by ring rolling process, and the surface is polished to meet the design size of the Ti3Al component layer at the outermost edge of the disk in step (1);

[0062] (5) Gradient performance disk forming: According to the composition design of step (1), the second composition transition layer is prepared on the inner side of the first Ti3Al alloy base ring by using the additive cladding process. The raw material for the second layer of additive cladding is a mixed powder of 67% Ti3Al + 33% TC4. The stacking direction of the mixed powder is radially from outside to inside. The radial thickness of the cladding layer is twice the radial design thickness of the second layer. The radial thinning rate of the metal layer is designed to be 50%. The second transition layer metal is subjected to radial rotary forging thinning deformation. The deformation temperature is 993°C (phase transition point T β2 -35℃), before forging and heating, the outer heat storage outer cylinder and the first layer of heat storage sleeves on the upper and lower end surfaces designed and processed in step (3) should be installed, and the heat preservation time at 993℃ is 40min (D2=50mm, 50mm×0.8min / mm), the radial deformation is 50%, and the heat deformation is performed after the heat deformation tooling is removed, and the inner side of the metal layer is polished to the designed size of the layer and the upper and lower end surfaces are polished and leveled;

[0063] The third component transition layer is prepared on the inner side of the second transition layer by using the additive cladding process. The raw material for the third layer of additive cladding is a mixed powder of 33% Ti3Al+67% TC4. The stacking direction of the mixed powder is radially from outside to inside. The radial thickness of the cladding layer is twice the radial design thickness of the third layer in step (1). The radial thinning rate of the metal layer is designed to be 50%. The metal of the second transition layer is subjected to radial rotary forging thinning deformation. The deformation temperature is 976°C (phase transition point T β3 -35℃), before forging heating, the outer heat storage outer cylinder and the first and second heat storage sleeves on the upper and lower end surfaces designed and processed in step (3) should be installed, the heat preservation time at 976℃ is 40min (D3=50mm, 50mm×0.8min / mm), the radial deformation is 50%, and the heat deformation is performed after the heat deformation tooling is removed, the inner side of the metal layer is polished to the designed size of the layer, and the upper and lower end surfaces are polished and leveled;

[0064] The fourth component layer is prepared on the inner side of the third component layer by using an additive cladding process. The raw material for the fourth layer of additive cladding is TC4 alloy powder. The stacking direction of the alloy powder is radially from the outside to the inside. The radial thickness of the cladding layer is twice the radial design thickness of the fourth layer in step (1). The radial thinning rate of the metal layer is designed to be 50%. The metal of the fourth component layer is subjected to radial rotary forging thinning deformation. The deformation temperature is 960°C (phase transition point T β4 -35℃), before forging heating, the outer heat storage outer cylinder and the first, second and third heat storage sleeve rings on the upper and lower end surfaces designed and processed in step (3) should be installed, and the insulation time at 960℃ is 40min (D4=50mm, 50mm×0.8min / mm), and the radial deformation is 50%; after removing the heat deformation tooling, the inner side of the metal layer is polished to the designed size of the layer and the upper and lower end surfaces are polished and leveled;

[0065] (6) Heat treatment of the disk: anneal the gradient disk blank prepared in step (5) at 700°C for 2h, AC;

[0066] (7) Disk finishing: The gradient disk blank is finished according to the disk design dimensions in step (1) to obtain a gradient performance disk.

[0067] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0068] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a Ti3Al / (α+β)Ti gradient performance disk, comprising the following steps: S1) According to the structure of the gradient performance disk to be prepared, the gradient performance disk to be prepared is divided into n component layers from the outer edge to the core, and the content of Ti3Al and (α+β)Ti in the component layers is designed, and the component content of the xth layer from the outer edge to the core satisfies the following relationship: (n-x) / (n-1)×C Ti3Al +(x-1) / (n-1)×C Ti , Among them, C Ti3Al is the composition of Ti3Al alloy, C Ti is (α+β)Ti alloy composition, n≥3; S2) respectively determining the phase transition points of each component layer except the outer edge component layer; S3) designing a thermal deformation heat storage tool for thermal deformation according to the structure of the gradient performance disk to be prepared; S4) preparing a Ti3Al alloy base ring, the size of which after machining is consistent with the size of the outer edge component layer of the gradient performance disk; S5) on the basis of the Ti3Al alloy base ring, radially performing high-energy beam powder feeding additive preparation layer by layer according to the component content in step S1), and utilizing the thermal deformation heat storage tooling in step S2) for thermal deformation layer by layer to obtain a gradient performance disk blank; S6) heat treating the gradient performance disk blank.

2. The preparation method according to claim 1, characterized in that: Step S2) is specifically: The additive cladding process is used to prepare metallographic samples of each component layer in step S1), and then the phase transition point of each metallographic sample is detected.

3. The preparation method according to claim 1, characterized in that: The thermal deformation heat storage tooling comprises a heat storage outer cylinder, an upper end surface heat storage sleeve ring and a lower end surface heat storage sleeve ring. The inner diameter of the heat storage outer cylinder matches the outer diameter of the gradient performance disk, and the thickness is not less than the radial width of the outer edge component layer; the heat storage sleeve ring is composed of n-1 layers from the secondary outer edge to the core, and the inner diameter / outer diameter of the x-th layer of the heat storage sleeve ring corresponds in sequence to the inner diameter / outer diameter of the x-th layer of the gradient performance disk, and the thickness is not less than the thickness of the gradient performance disk.

4. The preparation method according to claim 1, characterized in that: The Ti3Al alloy base ring is prepared by a plastic deformation process and has a fine forged structure.

5. The preparation method according to claim 1, characterized in that: Step S5) is specifically: On the basis of the Ti3Al alloy base ring, from outside to inside, the steps include: the second layer of high-energy beam powder feeding additive preparation → the second layer of thermal deformation → the third layer of high-energy beam powder feeding additive preparation → the third layer of thermal deformation →... → the n-1 layer of high-energy beam powder feeding additive preparation → the n-1 layer of thermal deformation → the n layer of high-energy beam powder feeding additive preparation → the n layer of thermal deformation.

6. The preparation method according to claim 1 or 5, characterized in that: The thermal deformation is in the form of radial thinning deformation, and the thermal deformation temperature is 20 to 50° C. below the phase transition point of the component layer.

7. The preparation method according to claim 3, characterized in that: The specific method of thermal deformation layer by layer using the thermal deformation heat storage tooling in step S2) is as follows: before thermal deformation of the xth layer, the thermal storage outer cylinder, the 1st to x-1th layers of upper end surface thermal storage sleeves, and the 1st to x-1th layers of lower end surface thermal storage sleeves are installed; after heating, the thermal storage outer cylinder, the 1st to x-1th layers of upper end surface thermal storage sleeves, and the 1st to x-1th layers of lower end surface thermal storage sleeves are removed, and then thermal deformation of the xth layer is performed.

8. The preparation method according to claim 1, characterized in that: The radial thickness of each initial component layer prepared by the high-energy beam powder feeding additive is such that the initial component layer undergoes radial plastic deformation with a thinning rate of 30-70% and the size obtained after machining meets the structural size of the gradient performance disk to be prepared in step S1), and the holding time of each initial component layer prepared by the high-energy beam powder feeding additive at the thermal deformation temperature is the cross-sectional thickness D of the initial layer. x ×(0.6~0.8)min / mm.

9. The preparation method according to claim 1, characterized in that: The heat treatment temperature is 400-760° C., the time is 2-10 hours, and the heat treatment is air-cooled.

10. An aircraft engine compressor disk, prepared from a gradient performance disk, wherein the gradient performance disk is a Ti3Al / (α+β)Ti gradient performance disk prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Application of double-channel powder feeding process in preparation of blank of turbine disc of aero-engine

    CN120606088A